NdFeB magnet without heavy rare earth and production process thereof
A heavy rare earth-free NdFeB magnet using PrAlCuCo alloy nanoparticles and NdFeB composite nanomaterials addresses coercivity and cost issues by enhancing coercive force and corrosion resistance, bypassing the need for scarce and costly heavy rare earths.
Patent Information
- Application Number
- CN202411447649.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-06
AI Technical Summary
Existing sintered NdFeB magnets suffer from poor coercivity and high production costs due to the addition of heavy rare earth elements like Dy and Tb, which also reduce remanence and magnetic energy product, and are limited by scarce resource reserves and high prices.
A heavy rare earth-free NdFeB magnet composed of PrAlCuCo alloy nanoparticles and NdFeB composite nanomaterials, prepared through vacuum melting, DC arc plasma, and cold isostatic pressing, with specific atomic and mass ratios, to enhance coercivity and corrosion resistance.
The magnet exhibits improved coercive force, high-temperature stability, and enhanced corrosion resistance through grain boundary diffusion and synergistic effects of Pr, Al, and Co, reducing reliance on scarce and expensive heavy rare earths.
Smart Images

Figure CN119092240A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth permanent magnet materials, and in particular relates to a heavy rare earth-free neodymium iron boron magnet and a production process thereof. Background Art
[0002] As the third generation of rare earth permanent magnet materials, sintered NdFeB has excellent magnetic properties (high remanence, high coercivity, high magnetic energy product) and high cost performance, and is widely used in many fields such as power machinery, medical equipment, automobile industry, wind power generation, electronics, hardware and household appliances, and aerospace. As downstream products develop towards miniaturization, micro-miniaturization and lightweight, higher requirements are also placed on the performance of sintered NdFeB magnets. In order to improve the magnetic properties of NdFeB magnets, especially to improve the coercivity of the magnets, heavy rare earth elements Dy and Tb are usually added during the preparation of magnets to form Dy2Fe with a higher magnetocrystalline anisotropy field. 14 B. Tb2Fe 14 B phase, and can also improve the temperature stability of the magnet. Since heavy rare earths Dy, Tb and Fe are antiferromagnetic coupling, the addition of Dy and Tb will inevitably reduce the remanence and magnetic energy product of the magnet. In addition, the resource reserves of heavy rare earths Dy and Tb are very small and the price is high, which increases the production cost of the magnet. Therefore, it is of great significance to develop heavy rare earth-free sintered NdFeB magnets. Summary of the invention
[0003] One of the purposes of the present invention is to provide a heavy rare earth-free NdFeB magnet to solve the problem of poor performance of existing sintered NdFeB magnets;
[0004] A second object of the present invention is to provide a production process for heavy rare earth-free NdFeB magnets.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] In the first aspect, a heavy rare earth-free NdFeB magnet is composed of PrAlCuCo alloy nanoparticles and NdFeB composite nanomaterials, wherein the atomic percentage composition of the PrAlCuCo alloy nanoparticles is: Pr 35 A l 50 Cu x Co 15-x , (0<x<15); the atomic percentage composition of the NdFeB composite nanomaterial is: Nd 10 Fe 84 B6; the mass ratio of the PrA l CuCo alloy nanoparticles to the NdFeB composite nanomaterial is 0.5-1.5:6;
[0007] As a further embodiment of the present invention, the method for preparing the PrAl CuCo alloy nanoparticles comprises the following steps:
[0008] S1. According to the atomic ratio of Pr:Al:Cu:Co=35:50:x:15-x, vacuum melting is performed to obtain a quaternary alloy ingot;
[0009] S2. The quaternary alloy ingot is placed under vacuum conditions, treated at 850-950°C for 18-24h, and then cooled to room temperature (25-30°C) under argon gas;
[0010] S3. The quaternary alloy ingot obtained by heat treatment in S2 is prepared by DC arc plasma method to obtain Pr 35 A l 50 Cu x Co 15-x Alloy nanoparticles.
[0011] As a further solution of the present invention, the DC arc voltage in S3 is 18-25V, and the current is 100-120A.
[0012] As a further solution of the present invention, the gas atmosphere in the DC arc plasma method in S3 is composed of argon and hydrogen in a volume ratio of 3:1-2.
[0013] As a further scheme of the present invention, the preparation method of the NdFeB composite nanomaterial comprises the following steps: according to the atomic ratio of Nd:Fe:B=10:84:6, vacuum arc melting is performed under argon conditions, followed by melt spinning and cooling; after spinning, annealing at 650-750°C for 1-2h to crystallize to obtain the NdFeB composite nanomaterial.
[0014] As a further solution of the present invention, the melt spinning cooling process uses a rotating wheel with a rotation speed of 200-300 rpm.
[0015] The NdFeB is melt-spun by a rotating wheel, so that it is cooled to form an amorphous band. The nano-composite material formed by crystallization after annealing has a large coercive force.
[0016] In a second aspect, a production process of a heavy rare earth-free NdFeB magnet comprises the following steps:
[0017] Step 1: Under vacuum and argon conditions, NdFeB composite nanomaterials and PrAl CuCo alloy nanoparticles are mixed in proportion, and the mixed material is pressed into a shape under a magnetic field and subjected to cold isostatic pressing;
[0018] Step 2: heat-treat the pressed sample at 800-1000°C for 2-6 hours, cool it to room temperature with argon, and then temper it at 400-600°C for 1-2 hours to obtain a heavy rare earth-free NdFeB magnet.
[0019] As a further solution of the present invention, in step 1, the magnetic field is 2-3T, and the cold isostatic pressing pressure is 250-350MPa.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention provides a heavy rare earth-free NdFeB magnet. PrAlCuCo alloy nanoparticles are prepared by doping Al, Cu and Co with light rare earth Pr. The coercive force of the NdFeB magnet is improved by the grain boundary diffusion of the PrAlCuCo alloy nanoparticles in the NdFeB composite nanomaterial.
[0022] 2. In the process of preparing heavy rare earth-free NdFeB magnets, the present invention adopts 800-1000°C as the infiltration temperature of alloy nanoparticles into NdFeB nanocomposite materials, which can effectively promote the infiltration process of eutectic and avoid excessive growth of grains.
[0023] 3. In the present invention, through the action of Pr and Al, the magnet obtained after the alloy particles diffuse forms a large number of continuous grain boundary phases. The preferred element Pr is parallel to the diffusion of Nd in the intergranular phase during grain diffusion, and due to penetration, a non-magnetic PrNdFe phase is produced, thereby wrapping NdFeB; most of Al is evenly distributed at the grain boundary, reacting with Nd or Fe to form NdAl or NdFeAl phase, thereby improving the smoothness of the grain boundary and improving wettability; since the standard potential of Cu is higher than that of Nd, it is beneficial to improve the corrosion resistance of the magnet; the Co element can form a Co-rich shell layer to improve the high-temperature performance of the magnet, thereby satisfying its penetration diffusion at 800-1000°C; on the other hand, Co and Al can further synergistically improve the coercive force of the magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described below in conjunction with the accompanying drawings.
[0025] Figure 1 The present invention is a production process flow chart of the heavy rare earth-free NdFeB magnet. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The preparation method of PrAl CuCo alloy nanoparticles comprises the following steps:
[0028] S1. According to the atomic ratio of Pr:Al:Cu:Co=35:50:x:15-x, vacuum melting is performed to obtain a quaternary alloy ingot;
[0029] S2. The quaternary alloy ingot is placed under vacuum conditions, treated at 850-950°C for 18-24h, and then cooled to room temperature with argon gas;
[0030] S3. The quaternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1-2, and Pr 35 A l 50 Cu x Co 15-x Alloy nanoparticles, DC arc voltage is 18-25V, current is 100-120A.
[0031] The preparation method of NdFeB composite nanomaterial comprises the following steps:
[0032] According to the atomic ratio of Nd:Fe:B=10:84:6, vacuum arc melting was carried out under argon conditions, and melt spinning cooling was carried out using a rotor with a rotation speed of 200-300rpm; after spinning, annealing was carried out at 650-750℃ for 1-2h to crystallize to obtain NdFeB composite nanomaterials.
[0033] A heavy rare earth-free NdFeB magnet, composed of PrAlCuCo alloy nanoparticles and NdFeB composite nanomaterials, wherein the atomic percentage composition of the PrAlCuCo alloy nanoparticles is: 35 A l 50 Cu x Co 15-x , (0<x<15); the atomic percentage composition of the NdFeB composite nanomaterial is: Nd 10 Fe 84 B6; the mass ratio of the PrA l CuCo alloy nanoparticles to the NdFeB composite nanomaterial is 0.5-1.5:6;
[0034] Please refer to Figure 1The production process of the heavy rare earth-free NdFeB magnet comprises the following steps:
[0035] Step 1, under vacuum and argon conditions, NdFeB composite nanomaterials and PrAl CuCo alloy nanoparticles are mixed in proportion, and the mixed material is pressed into shape at a pressure of 250-350MPa under a magnetic field of 2-3T and subjected to cold isostatic pressing;
[0036] Step 2: heat-treat the pressed sample at 800-1000°C for 2-6 hours, cool it to room temperature with argon, and then temper it at 400-600°C for 1-2 hours to obtain a heavy rare earth-free NdFeB magnet.
[0037] Example 1
[0038] The preparation method of PrAl CuCo alloy nanoparticles comprises the following steps:
[0039] S1. According to the atomic ratio of Pr:Al:Cu:Co=35:50:5:10, vacuum melting is performed to obtain a quaternary alloy ingot;
[0040] S2. The quaternary alloy ingot was placed under vacuum conditions, treated at 900°C for 20 h, and then cooled to room temperature in argon gas;
[0041] S3. The quaternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 A l 50 Cu5Co 10 Alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0042] Example 2
[0043] The preparation method of PrAl CuCo alloy nanoparticles comprises the following steps:
[0044] S1. According to the atomic ratio of Pr:Al:Cu:Co=35:50:10:5, vacuum melting is performed to obtain a quaternary alloy ingot;
[0045] S2. The quaternary alloy ingot was placed under vacuum conditions, treated at 900°C for 20 h, and then cooled to room temperature in argon gas;
[0046] S3. The quaternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 A l 50 Cu 10 Co5 alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0047] Example 3
[0048] The preparation method of NdFeB composite nanomaterial comprises the following steps:
[0049] According to the atomic ratio of Nd:Fe:B=10:84:6, vacuum arc melting was carried out under argon conditions, and melt spinning was cooled using a wheel with a rotation speed of 250rpm; after the spinning, annealing was carried out at 700℃ for 1.5h to crystallize and obtain NdFeB composite nanomaterials.
[0050] Example 4
[0051] A production process for a heavy rare earth-free NdFeB magnet comprises the following steps:
[0052] Step 1: Under vacuum and argon conditions, Nd prepared in Example 3 10 Fe 84 B6 composite nanomaterial and Pr prepared in Example 1 35 A l 50 Cu5Co 10 The alloy nanoparticles were mixed in a mass ratio of 6:1, and the mixed material was pressed into shape at a pressure of 300 MPa under a magnetic field of 2.5 T and subjected to cold isostatic pressing;
[0053] Step 2: heat-treat the pressed sample at 900°C for 4 hours, cool it to room temperature with argon, and then temper it at 500°C for 1.5 hours to obtain a heavy rare earth-free NdFeB magnet.
[0054] Example 5
[0055] A production process for a heavy rare earth-free NdFeB magnet comprises the following steps:
[0056] Step 1: Under vacuum and argon conditions, Nd prepared in Example 3 10 Fe 84 B6 composite nanomaterial and Pr prepared in Example 2 35 A l 50 Cu 10 Co5 alloy nanoparticles were mixed in a mass ratio of 6:1, and the mixed material was pressed into shape at a pressure of 300 MPa under a magnetic field of 2.5 T and subjected to cold isostatic pressing;
[0057] Step 2: heat-treat the pressed sample at 900°C for 24 hours, cool it to room temperature with argon, and then temper it at 500°C for 1.5 hours to obtain a heavy rare earth-free NdFeB magnet.
[0058] Example 6
[0059] A production process for a heavy rare earth-free neodymium iron boron magnet, which differs from Example 4 in that the Nd prepared in Example 3 in step 1 10 Fe 84 B6 composite nanomaterial and Pr prepared in Example 1 35 A l 50 Cu5Co 10 The alloy nanoparticles were mixed in a mass ratio of 6:0.5, and the other steps and parameters remained the same.
[0060] Example 7
[0061] A production process for a heavy rare earth-free neodymium iron boron magnet, which differs from Example 4 in that the Nd prepared in Example 3 in step 1 10 Fe 84 B6 composite nanomaterial and Pr prepared in Example 1 35 A l 50 Cu5Co 10 The alloy nanoparticles were mixed in a mass ratio of 6:1.5, and the other steps and parameters remained the same.
[0062] Comparative Example 1
[0063] The preparation method of PrAlCu alloy nanoparticles comprises the following steps:
[0064] S1. According to the atomic ratio of Pr:Al:Cu=35:50:15, vacuum melting is performed to obtain a ternary alloy ingot;
[0065] S2. The ternary alloy ingot is placed under vacuum conditions, treated at 900°C for 20 hours, and then cooled to room temperature in argon gas;
[0066] S3. The ternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 A l 50 Cu 15 Alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0067] Comparative Example 2
[0068] The preparation method of PrAlCo alloy nanoparticles comprises the following steps:
[0069] S1. According to the atomic ratio of Pr:Al:Co=35:50:15, vacuum melting is performed to obtain a ternary alloy ingot;
[0070] S2. The ternary alloy ingot is placed under vacuum conditions, treated at 900°C for 20 hours, and then cooled to room temperature in argon gas;
[0071] S3. The ternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 A l 50 Co 15 Alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0072] Comparative Example 3
[0073] The preparation method of PrCoCu alloy nanoparticles comprises the following steps:
[0074] S1. According to the atomic ratio of Pr:Co:Cu=35:50:15, vacuum melting is performed to obtain a ternary alloy ingot;
[0075] S2. The ternary alloy ingot is placed under vacuum conditions, treated at 900°C for 20 hours, and then cooled to room temperature in argon gas;
[0076] S3. The ternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 Co 50 Cu 15 Alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0077] Comparative Example 4
[0078] The preparation method of PrCoCu alloy nanoparticles comprises the following steps:
[0079] S1. According to the atomic ratio of Pr:Co:Cu=35:15:50, vacuum melting is performed to obtain a ternary alloy ingot;
[0080] S2. The ternary alloy ingot is placed under vacuum conditions, treated at 900°C for 20 hours, and then cooled to room temperature in argon gas;
[0081] S3. The ternary alloy ingot obtained by heat treatment in S2 is placed in a gas atmosphere composed of argon and hydrogen in a volume ratio of 3:1.5, and Pr 35 Co 15 Cu 50 Alloy nanoparticles, DC arc voltage is 20V, current is 110A.
[0082] Comparative Example 5
[0083] A production process for a heavy rare earth-free NdFeB magnet, which differs from Example 4 in that the Pr prepared in Comparative Example 1 is used. 35 A l 50 Cu 15Alloy nanoparticles, the rest of the steps and parameters remain the same.
[0084] Comparative Example 6
[0085] A production process of a heavy rare earth-free NdFeB magnet, which is different from Example 4 in that the Pr prepared in Comparative Example 2 is used. 35 A l 50 Co 15 Alloy nanoparticles, the rest of the steps and parameters remain the same.
[0086] Comparative Example 7
[0087] A production process for a heavy rare earth-free NdFeB magnet, which differs from Example 4 in that the Pr prepared in Comparative Example 3 is used. 35 Co 50 Cu 15 Alloy nanoparticles, the rest of the steps and parameters remain the same.
[0088] Comparative Example 8
[0089] A production process of a heavy rare earth-free NdFeB magnet, which is different from Example 4 in that the Pr prepared in Comparative Example 4 is used. 35 Co 15 Cu 50 Alloy nanoparticles, the rest of the steps and parameters remain the same.
[0090] Comparative Example 9
[0091] A production process for a heavy rare earth-free NdFeB magnet, which differs from Example 4 in that the Pr prepared in Example 1 is not added in step 1. 35 A l 50 Cu5Co 10 Alloy nanoparticles, the rest of the steps and parameters remain the same.
[0092] The performance tests were conducted on the heavy rare earth-free NdFeB magnets prepared in Examples 4-7 and Comparative Examples 5-9:
[0093] (1) The low temperature (20°C) and high temperature (160°C) magnetic properties (remanence Br, coercivity Hcj, maximum magnetic energy product (BH) max) were tested using the NI M-15000H hysteresis loop measuring instrument. The low temperature magnetic properties test results are shown in Table 1:
[0094] Table 1
[0095] Br(kGs) Hcj(kOe) (BH)max(MGOe) Example 4 13.71 17.35 44.51 Example 5 13.33 17.27 44.28 Example 6 13.29 17.21 43.87 Example 7 13.52 17.36 44.43 Comparative Example 5 12.73 13.32 42.17 Comparative Example 6 12.94 14.27 42.76 Comparative Example 7 12.38 12.87 41.65 Comparative Example 8 12.27 13.11 41.44 Comparative Example 9 12.16 11.87 39.41
[0096] The low temperature magnetic properties test results are shown in Table 2:
[0097] Table 2
[0098]
[0099]
[0100] It can be seen from Table 1 and Table 2 that the present invention optimizes the components in the heavy rare earth-free NdFeB magnet, and forms a wider continuous grain boundary phase by doping Co and Al in the quaternary alloy nanoparticles through synergistic diffusion, thereby improving the coercive force of the magnet and improving its high temperature stability.
[0101] (2) The corrosion resistance of the magnet was tested using a CHI 604D electrochemical workstation. The corrosion potential and corrosion current density in a 0.1 mol / L sodium chloride solution are shown in Table 3:
[0102] Table 3
[0103] Corrosion potential (V) <![CDATA[Corrosion current density (μA / cm 2 )]]> Example 4 -0.6847 37.7812 Example 5 -0.6816 36.2981 Example 6 -0.7014 38.7362 Example 7 -0.6927 38.4718 Comparative Example 5 -0.8674 65.4916 Comparative Example 6 -0.8016 59.4638 Comparative Example 7 -0.9436 79.8194 Comparative Example 8 -0.9271 81.2960 Comparative Example 9 -1.2575 96.0705
[0104] By doping Al, Cu and Co into Pr, the standard electrode potentials of Al, Cu and Co (-2.353V, -1.663V, 0.342V and -0.227V, respectively) are higher than -2.323V of Nd, so as to increase the electrode potential of the grain boundary phase in the NdFeB magnet, thereby enhancing the corrosion resistance of the magnet. As can be seen from Table 3, the higher corrosion potential and lower corrosion current density of the present invention indicate that the electrochemical stability of the magnet is improved through the penetration of PrAlCuCo nanoparticles.
[0105] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0106] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A heavy rare earth-free neodymium iron boron magnet, It is characterized in that The nanometer material is composed of PrAlCuCo alloy nanoparticles and NdFeB composite nanomaterials, wherein the atomic percentage composition of the nanometer material is: Pr 35 Al 50 Cu x Co 15-x , 0<x<15; the atomic percentage composition of the NdFeB composite nanomaterial is: Nd 10 Fe 84 B 6 ; The mass ratio of the PrAlCuCo alloy nanoparticles to the NdFeB composite nanomaterial is 0.5-1.5:
6.
2. A heavy rare earth-free neodymium iron boron magnet according to claim 1, It is characterized in that The method for preparing the PrAlCuCo alloy nanoparticles comprises the following steps: S1. According to the atomic ratio of Pr:Al:Cu:Co=35:50:x:15-x, vacuum melting is performed to obtain a quaternary alloy ingot; S2. The quaternary alloy ingot is placed under vacuum conditions, treated at 850-950°C for 18-24h, and then cooled to room temperature with argon gas; S3. The quaternary alloy ingot obtained by heat treatment in S2 is prepared by DC arc plasma method to obtain Pr 35 Al 50 Cu x Co 15-x Alloy nanoparticles.
3. A heavy rare earth-free NdFeB magnet according to claim 2, It is characterized in that The DC arc voltage in S3 is 18-25V, and the current is 100-120A.
4. A heavy rare earth-free NdFeB magnet according to claim 2, It is characterized in that The gas atmosphere in the DC arc plasma method in S3 is composed of argon and hydrogen in a volume ratio of 3:1-2.
5. A heavy rare earth-free NdFeB magnet according to claim 1, It is characterized in that The preparation method of the NdFeB composite nanomaterial comprises the following steps: According to the atomic ratio of Nd:Fe:B=10:84:6, vacuum arc melting was carried out under argon conditions, followed by melt spinning and cooling; after spinning, annealing was carried out at 650-750°C for 1-2h to crystallize to obtain NdFeB composite nanomaterials.
6. A heavy rare earth-free NdFeB magnet according to claim 5, It is characterized in that The melt spinning cooling process uses a rotating wheel with a rotation speed of 200-300 rpm.
7. A process for producing a heavy rare earth-free NdFeB magnet as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Under vacuum and argon conditions, NdFeB composite nanomaterials and PrAl CuCo alloy nanoparticles are mixed in proportion, and the mixed materials are pressed into shape under a magnetic field and subjected to cold isostatic pressing treatment; Step 2: heat-treat the pressed sample at 800-1000°C for 2-6 hours, cool it to room temperature with argon, and then temper it at 400-600°C for 1-2 hours to obtain a heavy rare earth-free NdFeB magnet.
8. The production process of a heavy rare earth-free NdFeB magnet according to claim 7, It is characterized in that In step 1, the magnetic field size is 2-3T, and the cold isostatic pressing pressure is 250-350MPa.