Method for improving electrode continuity of multilayer chip ceramic capacitor

By optimizing gas flow in the tunnel furnace, the problems of electrode continuity and carbon residue in the multi-layer chip ceramic capacitor are solved, and the reliability and electrical performance of the capacitor are improved.

CN119092315APending Publication Date: 2024-12-06GUANGDONG FENGHUA ADVANCED TECHNOLOGY (HOLDING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411263081.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing multi-layer sheet ceramic capacitors have poor gas flow effect during high-temperature sintering, resulting in poor continuity of the internal electrode and a lot of carbon residue, which affects electrical performance and reliability.

Method used

Reducing gas is alternately or simultaneously introduced from the opposite sides of the furnace head in the tunnel furnace, and gas is introduced from the opposite sides of the furnace body and the furnace tail at the same time, optimizing gas flow, reducing carbon residue, and improving sintering quality.

Benefits of technology

The continuity and flatness of the inner electrode are improved, the sintering shrinkage stress is reduced, and the reliability and electrical performance of the multi-layer sheet ceramic capacitor are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092315A_ABST
    Figure CN119092315A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving electrode continuity of a multilayer chip ceramic capacitor, and belongs to the technical field of electronic elements. In the sintering treatment process, the reducing gas is alternately or simultaneously introduced from the two opposite sides of the furnace head, and the reducing gas is simultaneously introduced from the two opposite sides of the furnace body and the two opposite sides of the furnace tail, so that the gas inlet mode can better promote the flowing of the gas in the tunnel furnace, the mass exchange capacity is increased, and the sintering efficiency is improved. Organic matters such as an adhesive and a plasticizer in a green body are fully discharged, the residual quantity of carbon is reduced, the sintering quality is improved, the continuity of an inner electrode is improved, the stress generated in the sintering shrinkage process of the inner electrode is reduced, the risk of welding cracking during plate loading is reduced, and the reliability of the multilayer chip ceramic capacitor is improved; the inner electrode in the multilayer chip ceramic capacitor prepared by the method has the characteristics of few breakpoints and good electrode continuity and flatness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic components, and in particular to a method for improving the continuity of electrodes of a multilayer chip ceramic capacitor. Background Art

[0002] Multilayer ceramic capacitors (MLCC) have many advantages such as large capacitance, good voltage resistance, and high reliability, and have been widely used in various electronic devices. In the manufacturing process of multilayer ceramic capacitors, high-temperature sintering in a reducing atmosphere is a very important process. The effect of high-temperature sintering directly affects the mechanical properties, electrical properties and reliability of multilayer ceramic capacitors, and the continuity of the internal electrode is an important indicator to measure the sintering effect. Good internal electrode continuity is the basic guarantee for the electrical performance of multilayer ceramic capacitors. At the same time, good internal electrode continuity can reduce the internal stress generated by the internal electrode during sintering shrinkage, reduce the risk of solder cracking when mounting, and improve the reliability of the capacitor.

[0003] The existing technology uses a traditional tunnel furnace to perform high-temperature sintering into porcelain. During the sintering process, air is taken in from the air inlet located at the tail of the tunnel furnace, and exhaust is exhausted from the air outlet located at the head of the tunnel furnace. This air inlet and outlet method makes the gas flow effect in the furnace poor. After sintering into porcelain, there is a lot of residual carbon in the porcelain body, which cannot effectively improve the continuity of the internal electrode.

[0004] Based on this, there is an urgent need in the art to develop a method for improving the continuity of electrodes of multilayer ceramic capacitors. Summary of the invention

[0005] Based on the defects of the prior art, the object of the present invention is to provide a method for improving the continuity of electrodes of multilayer ceramic capacitors.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for improving the continuity of electrodes of a multilayer ceramic capacitor comprises the following steps:

[0008] S1. preparing a green body of a multilayer ceramic capacitor;

[0009] S2, conveying the green body obtained in step S1 into a tunnel furnace for sintering to obtain a ceramic body;

[0010] The tunnel furnace comprises a furnace head, a furnace body and a furnace tail which are connected in sequence, the green body is transported from the entrance of the furnace head to the exit of the furnace tail by a transport device, the furnace head has a first air inlet, a second air inlet and a first air outlet, the furnace body has a third air inlet and a fourth air inlet, the furnace tail has a fifth air inlet and a sixth air inlet, the first air inlet is opposite to the second air inlet, the third air inlet is opposite to the fourth air inlet, and the fifth air inlet is opposite to the sixth air inlet;

[0011] During the sintering process, the reducing gas is alternately or simultaneously introduced into the furnace head through the first gas inlet and the second gas inlet, the reducing gas is simultaneously and continuously introduced into the furnace body through the third gas inlet and the fourth gas inlet, and the reducing gas is simultaneously introduced into the furnace tail through the fifth gas inlet and the sixth gas inlet;

[0012] S3, post-processing the ceramic blank obtained in step S2 to obtain a multi-layer ceramic capacitor.

[0013] During the sintering process, the present invention introduces reducing gas alternately or simultaneously from opposite sides of the furnace head, and simultaneously introduces reducing gas from opposite sides of the furnace body and opposite sides of the furnace tail, which can better promote the flow of gas in the tunnel furnace, increase mass exchange, fully eliminate residual organic matter in the green body, reduce carbon residue, improve sintering quality, improve the continuity of the internal electrode, reduce the stress generated by the internal electrode during the sintering shrinkage process, reduce the risk of welding resistance cracking when putting on the board, and improve the reliability of multilayer ceramic capacitors.

[0014] As a preferred embodiment of the method for improving the continuity of multilayer ceramic capacitor electrodes according to the present invention, the reducing gas includes an inert gas and hydrogen, the inert gas includes at least one of nitrogen and argon, and the volume percentage of the hydrogen in the reducing gas is 0.2 to 1.0%.

[0015] The present invention can prevent the internal electrode from being oxidized and ensure that the ceramic body is not reduced and thus becomes a semiconductor by controlling the hydrogen content in the reducing gas within the above range.

[0016] As a preferred embodiment of the method for improving the continuity of multilayer ceramic capacitor electrodes described in the present invention, the furnace head also has a first gas outlet, and the furnace body also has a second gas outlet. During the sintering process, exhaust is simultaneously exhausted to the outside of the tunnel furnace through the first gas outlet and the second gas outlet, and the exhaust flow rate through the first gas outlet is the same as the exhaust flow rate through the second gas outlet.

[0017] Further preferably, the first air outlet and the second air outlet are on the same side, and the first air outlet and the second air outlet are both located above the first air inlet, the second air inlet, the third air inlet, the fourth air inlet, the fifth air inlet and the sixth air inlet.

[0018] As a preferred embodiment of the method for improving the continuity of multilayer ceramic capacitor electrodes described in the present invention, the gas flow rate entering the furnace body is 150-300 L / min, and the gas flow rate of the third air inlet is the same as the gas flow rate of the fourth air inlet; the gas flow rate entering the furnace tail is 30-80 L / min, and the gas flow rate of the fifth air inlet is the same as the gas flow rate of the sixth air inlet.

[0019] More preferably, the gas flow rate into the furnace body is 200-250 L / min, and the gas flow rate into the furnace tail is 40-60 L / min.

[0020] As a preferred embodiment of the method for improving the continuity of the multilayer ceramic capacitor electrodes of the present invention, the sintering process includes:

[0021] The first heating stage: heating from 30-50°C to 300-550°C at a heating rate of 2-5°C / min, and heating from 300-550°C to 750-950°C at a heating rate of 1-3°C / min;

[0022] The second heating stage: heating from 750-950°C to 950-1150°C at a heating rate of 2.5-5°C / min, and heating from 950-1150°C to 1200-1280°C at a heating rate of 1-2°C / min;

[0023] Heat preservation and tempering stage: cool down from 1200-1280℃ to 800-1100℃ at a cooling rate of 2-4℃ / min, and keep at 800-1100℃ for 120-180min;

[0024] Cooling stage: cooling from 800-1100°C to 40-200°C at a cooling rate of 2-5°C / min.

[0025] Further preferably, in the first heating stage, the reducing gas is periodically and alternately introduced into the furnace head through the first air inlet and the second air inlet, the gas flow rate into the furnace head is 30-70 L / min, and the alternating period is 10-30 min.

[0026] More preferably, the gas flow rate introduced into the furnace head is 40-60 L / min, and the alternating cycle is 15-20 min.

[0027] The inventor has discovered through research that, in the first heating stage, reducing gas is periodically and alternately introduced into the furnace head through the first air inlet and the second air inlet, and exhaust is discharged from the openings on the same side of the furnace head and the furnace body. This can effectively reduce the air flow vortex resistance formed by gas convection in the tunnel furnace, promote the flow of gas in the tunnel furnace, increase the mass exchange rate, achieve full removal of organic matter in the green body, reduce the carbon residue of the multilayer ceramic capacitor, improve the sintering quality, and improve the electrode continuity of the multilayer ceramic capacitor.

[0028] Further preferably, in the second heating stage, the insulation and tempering stage, and the cooling stage, the reducing gas is continuously introduced into the furnace head through the first air inlet and the second air inlet at the same time, and the gas flow rate into the furnace head is 30 to 70 L / min, and the gas flow rate of the first air inlet is the same as the gas flow rate of the second air inlet.

[0029] More preferably, in the second heating stage, the heat preservation and tempering stage, and the cooling stage, the gas flow rate introduced into the furnace head is 40-60 L / min.

[0030] Further preferably, the sintering process includes:

[0031] The first heating stage: heating from 30-50°C to 400-500°C at a heating rate of 3-4°C / min, and heating from 400-500°C to 800-900°C at a heating rate of 2-2.5°C / min;

[0032] The second heating stage: heating from 800-900°C to 1000-1100°C at a heating rate of 3-4°C / min, and heating from 1000-1100°C to 1200-1280°C at a heating rate of 1-1.5°C / min;

[0033] Heat preservation and tempering stage: cool down from 1200-1280℃ to 900-1000℃ at a cooling rate of 2-3℃ / min, and keep at 900-1000℃ for 120-180min;

[0034] Cooling stage: Cooling from 900-1000°C to 40-200°C at a cooling rate of 3-4°C / min.

[0035] The inventors have found that by optimizing the sintering process to increase the temperature in stages and controlling the process parameters of each stage within the above range, it is possible to efficiently remove binder and reduce the amount of residual carbon, while also improving the continuity and flatness of the internal electrodes in the prepared multilayer ceramic capacitors.

[0036] It is understandable that the first air inlet can be one or more; the second air inlet can be one or more; the third air inlet can be one or more; the fourth air inlet can be one or more; the fifth air inlet can be one or more; the sixth air inlet can be one or more; the first air outlet can be one or more; the second air outlet can be one or more. In the present invention, the number means that the number is not less than two.

[0037] As a preferred embodiment of the method for improving the continuity of electrodes of a multilayer ceramic capacitor according to the present invention, step S1 comprises:

[0038] S11, casting the ceramic slurry into a ceramic diaphragm;

[0039] S12, printing an inner electrode slurry on the surface of the ceramic diaphragm to obtain an inner electrode layer;

[0040] S13, alternately stacking a plurality of ceramic diaphragms and a plurality of internal electrode layers, laminating and cutting them to obtain a ceramic green body;

[0041] S14, subjecting the ceramic green body to a debinding treatment in a nitrogen or air atmosphere; during the debinding treatment, the temperature is increased to 280-450° C. at a heating rate of 0.03-2° C. / min, and the temperature is kept at this temperature for 120-240 minutes.

[0042] Furthermore, the ceramic slurry includes barium titanate, and the mass percentage of the barium titanate in the ceramic slurry is 60-95%.

[0043] Furthermore, the internal electrode paste includes at least one of nickel electrode paste, copper electrode paste and silver electrode paste.

[0044] As a preferred embodiment of the method for improving the continuity of electrodes of a multilayer ceramic capacitor of the present invention, the post-processing includes chamfering, end sealing, end firing, and deposition.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] In the present invention, during the sintering process, reducing gas is introduced alternately or simultaneously from opposite sides of the furnace head, and reducing gas is introduced simultaneously from opposite sides of the furnace body and opposite sides of the furnace tail. This air intake method can better promote the flow of gas in the tunnel furnace, increase the mass exchange amount, fully discharge organic matter such as adhesives and plasticizers in the green billet, reduce the residual carbon, improve the sintering quality, improve the continuity of the inner electrode, reduce the stress generated by the inner electrode during the sintering shrinkage process, reduce the risk of welding cracking when the board is placed, and improve the reliability of the multilayer chip ceramic capacitor;

[0047] The internal electrodes in the multilayer ceramic capacitor prepared by the method of the present invention have the characteristics of few breakpoints, good electrode continuity and flatness. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 A cross-sectional view of a tunnel furnace provided by an embodiment of the present invention;

[0049] Figure 2 Another cross-sectional view of the tunnel furnace provided by the present invention. DETAILED DESCRIPTION

[0050] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0051] Unless otherwise specified, the raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the component raw materials used in each parallel experiment are all of the same kind.

[0052] Examples 1 to 9

[0053] An embodiment of the method for improving the continuity of electrodes of a multilayer ceramic capacitor according to the present invention comprises the following steps:

[0054] S1. preparing a green body of a multilayer ceramic capacitor;

[0055] S11, preparing the components of ceramic slurry, wherein the ceramic slurry comprises the following components in parts by weight: BaTiO 3 72 parts, 7.5 parts of ethanol, 7.5 parts of toluene, 0.3 parts of dispersant, 10.7 parts of binder PVB, 2 parts of plasticizer DOP; adding the raw materials into a sand mill, mixing and sand grinding to obtain a ceramic slurry; casting the ceramic slurry into a ceramic diaphragm;

[0056] S12, preparing raw materials for the internal electrode slurry, wherein the internal electrode slurry comprises the following components in parts by weight: 55 parts of nickel powder, 7.5 parts of barium titanate powder, 2.5 parts of ethyl cellulose, 23 parts of terpineol, and 12 parts of hydrogenated terpineol; adding the components of the internal electrode slurry into a sand mill, mixing and sand-grinding to obtain the internal electrode slurry; printing the internal electrode slurry on the surface of the ceramic diaphragm to obtain the internal electrode layer;

[0057] S13, alternately stacking a plurality of ceramic diaphragms and a plurality of internal electrode layers, laminating and cutting them to obtain a ceramic green body;

[0058] S14, heating the ceramic green body to 400° C. at a rate of 1° C. / min in a nitrogen atmosphere, and performing a binder removal treatment at 400° C. for 3 hours to obtain a green body of a multilayer chip ceramic capacitor;

[0059] S2, conveying the green body obtained in step S1 into a tunnel furnace for sintering to obtain a ceramic body;

[0060] S3, chamfering, sealing, sintering and depositing the ceramic blank obtained in step S2 to obtain a multi-layer ceramic capacitor;

[0061] The reducing gas is a mixed gas of nitrogen and hydrogen, and the volume percentage of hydrogen in the reducing gas is 0.5%;

[0062] See also Figures 1-2 The tunnel furnace comprises a furnace head, a furnace body and a furnace tail which are connected in sequence. The green billet is transported from the entrance of the furnace head to the exit of the furnace tail by a conveying device. Two first air inlets 11 are arranged on one side wall of the furnace head, and two second air inlets 12 are arranged on the other side wall of the furnace head. The first air inlets 11 are opposite to the second air inlets 12 one by one. Three third air inlets 13 are arranged on one side wall of the furnace body, and three fourth air inlets 14 are arranged on the other side wall of the furnace body. The third air inlet 13 and the fourth air inlet 14 are opposite to each other. 14 are opposite to each other, two fifth air inlets 15 are arranged on one side wall of the furnace tail, and two sixth air inlets 16 are arranged on the other side wall of the furnace tail, and the fifth air inlets 15 are opposite to each other one by one; the spacing between any two adjacent air inlets among the two first air inlets 11, the three third air inlets 13 and the two fifth air inlets 15 located on the same side is the same, and the spacing between any two adjacent air inlets among the two second air inlets 12, the three fourth air inlets 14 and the two sixth air inlets 16 located on the same side is the same.

[0063] A first air outlet 17 is provided on one side wall of the furnace head, and a second air outlet 18 is provided on one side of the furnace body. The first air outlet 17 and the second air outlet 18 are on the same side and are both located above each air inlet. When working, the tunnel furnace is heated by silicon-molybdenum heating rods 19 arranged at the top and bottom thereof.

[0064] The sintering process includes the following stages:

[0065] The first heating stage: heating from 40°C to 400°C at a heating rate of 3°C / min, and heating from 400°C to 800°C at a heating rate of 2°C / min;

[0066] The second heating stage: heating from 800°C to 1000°C at a heating rate of 3°C / min, and heating from 1000°C to 1200°C at a heating rate of 1°C / min;

[0067] Heat preservation and tempering stage: cool down from 1200℃ to 1000℃ at a cooling rate of 2℃ / min, and keep at 1000℃ for 180min;

[0068] Cooling stage: cooling from 1000°C to 40°C at a cooling rate of 3°C / min.

[0069] In the first heating stage, the first air inlet 11 and the second air inlet 12 are periodically opened alternately, and the reducing gas is periodically passed into the furnace head alternately through the first air inlet 11 and the second air inlet 12, and the gas flow rate into the furnace head is Q 1 , the alternating period is T.

[0070] In the second heating stage, the heat preservation and tempering stage, and the cooling stage, the first air inlet 11 and the second air inlet 12 are kept open, and the reducing gas is introduced into the furnace head through the first air inlet 11 and the second air inlet 12. The air flow rate of the first air inlet 11 is the same as the air flow rate of the second air inlet 12, and the gas flow rate introduced into the furnace head is Q 2 .

[0071] In the first heating stage, the second heating stage, the heat preservation and tempering stage and the cooling stage, the third air inlet 13, the fourth air inlet 14, the fifth air inlet 15 and the sixth air inlet 16 are kept open, the reducing gas is introduced into the furnace body through the third air inlet 13 and the fourth air inlet 14, and the reducing gas is introduced into the furnace tail through the fifth air inlet 15 and the sixth air inlet 16. The air flow rate of the third air inlet 13 is the same as the air flow rate of the fourth air inlet 14, and the gas flow rate introduced into the furnace body is Q 3 The air flow rate of the fifth air inlet 15 is the same as the air flow rate of the sixth air inlet 16, and the gas flow rate entering the furnace head is Q 4 The first air outlet 17 and the second air outlet 18 remain open to exhaust air outside the tunnel furnace. The exhaust flow rate of the first air outlet 17 is the same as the exhaust flow rate of the second air outlet 18. The total air intake flow rate of the tunnel furnace is equal to the total exhaust flow rate of the tunnel furnace.

[0072] The reducing gas is a mixed gas of nitrogen and hydrogen, and the volume percentage of hydrogen in the reducing gas is 0.5%.

[0073] Q 1 , Q 2 , Q 3 , Q 4 , T are shown in Table 1.

[0074] Table 1

[0075] parameter T(min) <![CDATA[Q 1 (L / min)]]> <![CDATA[Q 2 (L / min)]]> <![CDATA[Q 3 (L / min)]]> <![CDATA[Q 4 (L / min)]]> Example 1 20 50 50 200 50 Example 2 15 50 50 200 50 Example 3 5 50 50 200 50 Example 4 30 50 50 200 50 Example 5 20 60 60 200 40 Example 6 20 40 40 200 60 Example 7 20 50 50 250 50 Example 8 20 30 30 300 30 Example 9 20 70 70 150 70

[0076] Example 10

[0077] The difference between this embodiment and embodiment 1 is that, in this embodiment, the first heating stage: heating from 40°C to 500°C at a heating rate of 4°C / min, and heating from 500°C to 900°C at a heating rate of 2.5°C / min; the second heating stage: heating from 900°C to 1100°C at a heating rate of 4°C / min, and heating from 1100°C to 1280°C at a heating rate of 1.5°C / min; heat preservation and tempering stage: cooling from 1280°C to 900°C at a cooling rate of 2°C / min, and keeping at 900°C for 150 minutes; cooling stage: cooling from 900°C to 40°C at a cooling rate of 4°C / min; the volume percentage of hydrogen in the reducing gas is 0.6%.

[0078] Embodiment 11

[0079] The difference between this embodiment and embodiment 1 is that, in this embodiment, the first heating stage: heating from 40°C to 300°C at a heating rate of 2°C / min, and heating from 300°C to 750°C at a heating rate of 1°C / min; the second heating stage: heating from 750°C to 950°C at a heating rate of 2.5°C / min, and heating from 950°C to 1200°C at a heating rate of 1°C / min; heat preservation and tempering stage: cooling from 1200°C to 800°C at a cooling rate of 3°C / min, and keeping at 800°C for 120 minutes; cooling stage: cooling from 800°C to 40°C at a cooling rate of 2°C / min; the volume percentage of hydrogen in the reducing gas is 0.6%.

[0080] Example 12

[0081] The difference between this embodiment and embodiment 1 is that, in this embodiment, the first heating stage: heating from 50°C to 550°C at a heating rate of 5°C / min, and heating from 550°C to 950°C at a heating rate of 3°C / min; the second heating stage: heating from 950°C to 1150°C at a heating rate of 5°C / min, and heating from 1150°C to 1280°C at a heating rate of 2°C / min; heat preservation and tempering stage: cooling from 1280°C to 1100°C at a cooling rate of 3°C / min, and keeping at 1100°C for 180 minutes; cooling stage: cooling from 1100°C to 40°C at a cooling rate of 5°C / min; the volume percentage of hydrogen in the reducing gas is 0.6%.

[0082] Comparative Example 1

[0083] The difference between this comparative example and Example 1 is that in this comparative example, in the first heating stage, the second heating stage, the insulation and tempering stage and the cooling stage, the first air inlet 11, the third air inlet 13 and the fifth air inlet 15 remain in an open state, the reducing gas is introduced into the furnace head through the first air inlet 11, the reducing gas is introduced into the furnace body through the third air inlet 13, and the reducing gas is introduced into the furnace tail through the fifth air inlet 15. The gas flow rate into the furnace head is 50 L / min, the gas flow rate into the furnace tail is 50 L / min, and the gas flow rate into the furnace body is 200 L / min.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 1 is that in the first heating stage, the second heating stage, the insulation and tempering stage and the cooling stage of this comparative example, the second air outlet 18 remains open to exhaust air outside the tunnel furnace, and the first air outlet 17 remains closed.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 1 is that the second heating stage of this comparative example is: heating to 1200°C at a heating rate of 10°C / min; the heat preservation and tempering stage of this comparative example is: keeping warm at 1200°C for 1h.

[0088] Effect Example 1

[0089] The products prepared in each embodiment and comparative example were subjected to the following performance tests, and the specific steps are as follows:

[0090] (1) Continuity of the inner electrode: preparation of grinding disc - ion polishing - scanning electron microscopy (SEM) - characterization of morphology - calculation of the continuity of the inner electrode by Avizo software; the continuity is calculated by the following formula to obtain a specific value: continuity (%) = (L2-L1) / L2*100%, where L2 is the total length of the inner electrode and L1 is the discontinuous length of the inner electrode.

[0091] (2) Flatness of the inner electrode: Make the grinding disc - ion polishing - Avizo software calculates the flatness of the inner electrode.

[0092] The test results are shown in Table 2.

[0093] Table 2

[0094]

[0095]

[0096] It can be seen from the test results in Table 2 that the embodiment of the present invention optimizes the sintering process to perform staged heating and control the process parameters of each stage within an appropriate range. During the sintering process, reducing gas is introduced alternately or simultaneously from opposite sides of the furnace head, and reducing gas is introduced from opposite sides of the furnace body and opposite sides of the furnace tail at the same time. Exhaust gas is discharged from the openings on the same side of the furnace head and the furnace body, which can better promote the flow of gas in the tunnel furnace, increase the mass exchange rate, fully discharge organic matter such as adhesives and plasticizers in the green body, reduce the residual carbon, improve the sintering quality, improve the continuity of the inner electrode, reduce the stress generated by the inner electrode during the sintering shrinkage process, reduce the risk of solder cracking when the plate is placed, and improve the reliability of the multilayer chip ceramic capacitor, so that the continuity of the inner electrode in the multilayer chip ceramic capacitor is not less than 85%, and the flatness is not less than 82%.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for improving the continuity of electrodes of a multilayer ceramic capacitor, characterized in that: The steps include: S1. preparing a green body of a multilayer ceramic capacitor; S2, conveying the green body obtained in step S1 into a tunnel furnace for sintering to obtain a ceramic body; The tunnel furnace comprises a furnace head, a furnace body and a furnace tail which are connected in sequence, the green body is transported from the entrance of the furnace head to the exit of the furnace tail by a transport device, the furnace head has a first air inlet, a second air inlet and a first air outlet, the furnace body has a third air inlet and a fourth air inlet, the furnace tail has a fifth air inlet and a sixth air inlet, the first air inlet is opposite to the second air inlet, the third air inlet is opposite to the fourth air inlet, and the fifth air inlet is opposite to the sixth air inlet; During the sintering process, the reducing gas is alternately or simultaneously introduced into the furnace head through the first gas inlet and the second gas inlet, the reducing gas is simultaneously and continuously introduced into the furnace body through the third gas inlet and the fourth gas inlet, and the reducing gas is simultaneously introduced into the furnace tail through the fifth gas inlet and the sixth gas inlet; S3, post-processing the ceramic blank obtained in step S2 to obtain a multi-layer ceramic capacitor.

2. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 1, characterized in that: The reducing gas includes an inert gas and hydrogen, the inert gas includes at least one of nitrogen and argon, and the volume percentage of the hydrogen in the reducing gas is 0.2-1.0%.

3. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 1, characterized in that: The furnace head also has a first gas outlet, and the furnace body also has a second gas outlet. During the sintering process, exhaust is simultaneously exhausted to the outside of the tunnel furnace through the first gas outlet and the second gas outlet, and the exhaust flow through the first gas outlet is the same as the exhaust flow through the second gas outlet.

4. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 1, characterized in that: The gas flow rate into the furnace body is 150~300L / min, and the gas flow rate of the third air inlet is the same as the gas flow rate of the fourth air inlet; the gas flow rate into the furnace tail is 30~80L / min, and the gas flow rate of the fifth air inlet is the same as the gas flow rate of the sixth air inlet.

5. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 1, characterized in that: The sintering process includes: The first heating stage: heating from 30-50°C to 300-550°C at a heating rate of 2-5°C / min, and heating from 300-550°C to 750-950°C at a heating rate of 1-3°C / min; The second heating stage: heating from 750-950°C to 950-1150°C at a heating rate of 2.5-5°C / min, and heating from 950-1150°C to 1200-1280°C at a heating rate of 1-2°C / min; Insulation stage: cool down from 1200-1280℃ to 800-1100℃ at a cooling rate of 2-4℃ / min, and keep at 800-1100℃ for 120-180min; Cooling stage: cooling from 800-1100°C to 40-200°C at a cooling rate of 2-5°C / min.

6. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 5, characterized in that: In the first heating stage, reducing gas is periodically and alternately introduced into the furnace head through the first air inlet and the second air inlet, the gas flow rate into the furnace head is 30-70 L / min, and the alternating period is 10-30 minutes.

7. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 5, characterized in that: In the second heating stage, the insulation and tempering stage and the cooling stage, the reducing gas is continuously introduced into the furnace head through the first air inlet and the second air inlet at the same time, and the gas flow rate into the furnace head is 30-70L / min. The gas flow rate of the first air inlet is the same as the gas flow rate of the second air inlet.

8. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 1, characterized in that: Step S1 includes: S11, casting the ceramic slurry into a ceramic diaphragm; S12, printing an inner electrode slurry on the surface of the ceramic diaphragm to obtain an inner electrode layer; S13, alternately stacking a plurality of ceramic diaphragms and a plurality of internal electrode layers, laminating and cutting them to obtain a ceramic green body; S14, subjecting the ceramic green body to a debinding treatment in a nitrogen or air atmosphere; during the debinding treatment, the temperature is increased to 280-450° C. at a heating rate of 0.03-2° C. / min, and the temperature is kept at this temperature for 120-240 minutes.

9. The method for improving the continuity of electrodes of a multilayer ceramic capacitor according to claim 8, characterized in that: The internal electrode paste includes at least one of a nickel electrode paste, a copper electrode paste, and a silver electrode paste.