Composite substrate and manufacturing method thereof
By depositing and heat-treating a thin film containing carbon on a SiC single crystal substrate to form a laminate or graphene layer, the problem of large differences in number of graphene layers is solved, and the improvement of layer uniformity and crystallinity is achieved. It is suitable for Epitaxial film growth of semiconductor materials.
Patent Information
- Application Number
- CN202410591400.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-06
AI Technical Summary
When the SiC single crystal substrate is thermally decomposed, the number of layers of the graphene layer varies greatly, resulting in uneven growth and affecting the crystallinity of the epitaxial layer.
A thin film containing carbon is deposited on a SiC single crystal substrate using a deposition method that can be controlled by molecular layer level, and a carbon-containing layer is formed by heat treatment to ensure that the number of layers of the laminated body or graphene layer is less than one layer, and carbon is supplied externally. To suppress the locality of thermal decomposition.
The difference in the number of carbon-containing layers on the SiC single crystal substrate is effectively reduced, the crystallinity of the epitaxial layer is improved, and the growth quality of epitaxial films in semiconductor devices is improved.
Smart Images

Figure CN119092396A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a composite substrate and a method for manufacturing the same. Background Art
[0002] Among the methods for manufacturing graphene, the following method is known, which removes the oxide film covering the surface of a silicon carbide (SiC) single crystal substrate formed by natural oxidation, exposes the Si surface of the SiC single crystal substrate, and heats (thermally decomposes) the exposed SiC single crystal substrate in a vacuum or in an inert gas such as argon (Ar). By heating in a vacuum or in an inert gas such as argon (Ar), silicon (Si) sublimates and the remaining carbon (C) self-organizes, and graphene is formed on the SiC single crystal substrate in a stacked manner.
[0003] [Prior art literature]
[0004] [Patent Document]
[0005] [Patent Document 1] International Publication No. 2010 / 023934 Summary of the invention
[0006] [Problems to be solved by the invention]
[0007] However, when the SiC single crystal substrate is thermally decomposed, a carbon-containing layer such as a graphene layer grows starting from the step, but before the first layer completely covers it, the second layer grows partially on the surface of the SiC single crystal. In other words, the thermal decomposition of the SiC single crystal substrate occurs locally, and the difference in the number of carbon-containing layers may become large.
[0008] The present disclosure is proposed in view of the above-mentioned actual situation, and one of its purposes is to provide a composite substrate in which the difference in the number of carbon-containing layers formed on a SiC single crystal substrate is reduced to less than 1 layer. In addition, one of its purposes is to provide a method for manufacturing the composite substrate.
[0009] [Technical means to solve the problem]
[0010] A composite substrate in one form disclosed herein comprises: a SiC single crystal substrate having an off-angle; and a carbon-containing layer, which is arranged in contact with the surface of the SiC single crystal substrate and includes a stacked body or a graphene layer formed by stacking a reconstructed surface layer and a graphene layer; and when the outermost surface of the SiC single crystal substrate is a Si termination surface, a stacked body is arranged above the SiC single crystal substrate, and the graphene layer of the stacked body is 1 layer or 2 layers, and when the outermost surface of the SiC single crystal substrate is a C termination surface, 1 layer or 2 layers of graphene layers are arranged above the SiC single crystal substrate.
[0011] A method for manufacturing a composite substrate in one form disclosed herein includes the following steps: depositing a thin film containing carbon on a SiC single crystal substrate using a deposition method that can be controlled at the molecular layer level; and performing heat treatment to form a carbon-containing layer on the SiC single crystal substrate using the carbon supplied by the thin film, wherein the carbon-containing layer includes any one of a stack formed by stacking a reconstructed surface layer and a graphene layer or a graphene layer; and the difference in the number of layers of the carbon-containing layer on the SiC single crystal substrate is less than 1 layer.
[0012] [Effects of the invention]
[0013] According to the present disclosure, a composite substrate in which the difference in the number of carbon-containing layers formed on a SiC single crystal substrate is reduced to less than 1 layer and a method for manufacturing the composite substrate can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 A cross-sectional view showing a composite substrate according to an embodiment.
[0015] Figure 2 A cross-sectional view showing a composite substrate according to Modification 1.
[0016] Figure 3 A cross-sectional view showing a composite substrate according to Modification 2.
[0017] Figure 4A This is a cross-sectional view showing one step of the manufacturing steps of the composite substrate according to Modification 2 (Part 1).
[0018] Figure 4B This is a cross-sectional view showing one step of the manufacturing steps of the composite substrate according to Modification 2 (part 2).
[0019] Figure 4C This is a cross-sectional view showing one step of the manufacturing steps of the composite substrate according to Modification 2 (part 3).
[0020] Figure 4D This is a cross-sectional view showing one step of the manufacturing steps of the composite substrate according to Modification 2 (Part 4). DETAILED DESCRIPTION
[0021] Next, the embodiments are described with reference to the accompanying drawings. In the description of the drawings described below, the same or similar parts are marked with the same or similar symbols. The drawings are schematic. In addition, the embodiments shown below illustrate the device or method used to concretize the technical ideas, and do not specify the material, shape, structure, configuration, etc. of the parts. Various changes can be added to the embodiments.
[0022] The composite substrate according to this embodiment will be described with reference to the drawings.
[0023] Figure 1A cross-sectional view of composite substrate 100 according to this embodiment is shown.
[0024] The composite substrate 100 comprises: a SiC single crystal substrate 1 having an off angle; and a carbon-containing layer arranged in contact with the surface of the SiC single crystal substrate 1. In the present embodiment, the outermost surface of the SiC single crystal substrate 1 is a carbon (C) termination surface 1c, and the carbon-containing layer in contact with the C termination surface 1c is arranged with one or two graphene layers 10.
[0025] The "off angle" in this disclosure refers to the rotation angle θ when the grown crystal is rotated at a certain angle along the plane from the C-axis direction (the direction perpendicular to the substrate plane, the film thickness direction) and cut. The off angle of the SiC single crystal substrate 1 is preferably 0.5° to 10°, and more preferably 4° to 8°.
[0026] The SiC single crystal substrate 1 may also have any crystal structure of hexagonal (4H, 6H) crystals or cubic (3C) crystals. For example, the SiC single crystal substrate 1 including hexagonal (4H) crystals is obtained by sublimating SiC powder as a raw material in a graphite crucible filled with an inert gas such as nitrogen (N2) gas, and recrystallizing it into SiC seed crystals whose temperature is controlled to be lower than that of the raw material powder (modified Lely method (seed crystal sublimation recrystallization method)). At this time, impurities that determine the conductivity type of the SiC single crystal substrate 1 may also be added.
[0027] The graphene layer 10 has a single-layer structure of 1 layer or a stacked structure of 2 layers. The number of layers of the graphene layer 10 as a carbon-containing layer is 1 layer or 2 layers, so the result is that the difference in the number of layers of the carbon-containing layer is 1 layer or less. In addition, the number of layers of the carbon-containing layer can be observed, for example, by Raman spectroscopy, TEM (Transmission Electron Microscope), etc., and Raman imaging is preferably used for observing a large range. From the viewpoint of the difference in the number of layers of the carbon-containing layer, the number of layers of the graphene layer 10 is preferably 1 layer. If the difference in the number of layers of the carbon-containing layer is 1 layer or less, the crystal growth of the epitaxial layer that can be formed later becomes good.
[0028] Generally speaking, when a carbon-containing layer such as a graphene layer is formed on a SiC single crystal substrate, the SiC single crystal substrate is thermally decomposed, Si atoms in the SiC single crystal substrate are sublimated, and the remaining carbon (C) is self-organized, so that the graphene layer is formed in a stacked manner on the SiC single crystal substrate.
[0029] In this embodiment, in order to reduce the difference in the number of carbon-containing layers, in addition to supplying carbon from the SiC single crystal substrate 1 as described below, a deposition method that can be controlled at the molecular layer level is used to deposit a thin film containing carbon on the SiC single crystal substrate 1 as a new carbon supply source. Then, the thin film is carbonized by heat treatment to form a carbon-containing layer such as the graphene layer 10. Through this step, the growth of the carbon-containing layer can be promoted before the step aggregation of the SiC single crystal substrate occurs.
[0030] Here, when forming a carbon-containing layer, if carbon is supplied only by the SiC single crystal substrate, the in-plane difference of the carbon-containing layer becomes large due to the difference in the local thermal decomposition rate. Therefore, by supplying carbon from the outside when forming the carbon-containing layer as in the present embodiment, the difference of the carbon-containing layer is improved by relatively suppressing the effect of thermal decomposition of the SiC single crystal substrate when the same layer is obtained. In addition, since a carbon-containing layer with high crystallinity can be formed, the difference in epitaxial film growth in a semiconductor device can be reduced when a composite substrate including the carbon-containing layer is used as a material for a semiconductor device or the like.
[0031] According to the present embodiment, composite substrate 100 can be obtained in which the variation in the number of carbon-containing layers formed on the SiC single crystal substrate is reduced.
[0032] In the composite substrate 100 , the outermost surface of the SiC single crystal substrate 1 is a C-terminated surface 1 c , but the present invention is not limited thereto. For example, various variations as shown below are also possible.
[0033] <Variation 1>
[0034] The configuration of the composite substrate 100A according to the first variation is described. Figure 1 The above description is used for the common aspects of the composite substrate 100 shown, and the different aspects will be described below.
[0035] Figure 2 is a cross-sectional view of a composite substrate 100A according to a first variation. Figure 1 The composite substrate 100 shown is different in the following aspects: the outermost surface of the SiC single crystal substrate 1 is a silicon (Si) termination surface 1 si , and the carbon-containing layer in contact with the Si termination surface 1 si is a stacked body formed by stacking a reconstructed surface layer 10 a and a graphene layer 10 .
[0036] In the composite substrate 100A, the outermost surface of the SiC single crystal substrate 1 is the Si termination surface 1si, so when the graphene layer 10 is formed on the surface of the SiC single crystal substrate 1, a reconstructed surface layer 10a is formed on the surface of the SiC single crystal substrate 1, and the graphene layer 10 is formed on the reconstructed surface layer 10a. The reconstructed surface layer 10a plays a role in alleviating the lattice mismatch with the graphene layer 10, and is also called a buffer layer or the 0th layer of the graphene layer.
[0037] In Modification 1, when forming the carbon-containing layer, carbon is supplied from outside in addition to the SiC single crystal substrate. Thus, when obtaining the same single layer, the difference in the carbon-containing layer is improved by relatively suppressing the effect of thermal decomposition of the SiC single crystal substrate.
[0038] <Variation 2>
[0039] The configuration of a composite substrate 100B according to a second variation is described below. Figure 2 The above description is used for common aspects of the composite substrate 100A shown, and different aspects will be described below.
[0040] Figure 3 is a cross-sectional view of a composite substrate 100B according to a second variation. Figure 2 The composite substrate 100A shown is different in that it includes an epitaxial layer 3 disposed on the graphene layer 10 .
[0041] In the composite substrate 100B, by using the SiC single crystal substrate 1 having an off angle, the crystal type of the SiC single crystal substrate 1 is reflected in the crystal growth of the epitaxial layer 3 via the graphene layer 10. Therefore, it is possible to form an epitaxial layer 3 of a single crystal, that is, SiC, which is the same type of crystal type as that of the SiC single crystal substrate 1. From the viewpoint of the crystal growth of the epitaxial layer 3, the off angle is preferably 0.5° to 10°, and more preferably 4° to 8°.
[0042] In the second variation, when forming the carbon-containing layer, carbon is supplied from the outside in addition to the SiC single crystal substrate, thereby improving the difference in the carbon-containing layer by relatively suppressing the effect of thermal decomposition of the SiC single crystal substrate when the same 1 layer is obtained. Compared with the composite substrate 100, the composite substrate 100B is a structure that also has a reconstructed surface layer 10a, so it is easy to control the number of graphene layers, and the number of graphene layers is less different, so the crystallinity of the epitaxial layer 3 can be improved. That is, the same type of crystal as the SiC single crystal substrate can be grown on the graphene layer.
[0043] (Method for manufacturing composite substrate)
[0044] Next, an example of a method for manufacturing a composite substrate will be described. Here, a method for manufacturing the composite substrate 100B will be described.
[0045] First, if Figure 4A As shown, on the Si termination surface 1si of the SiC single crystal substrate 1, hydrofluoric acid is used to remove the natural oxide film from the SiC single crystal substrate 1. The SiC single crystal substrate 1 can be, for example, a 4H-SiC substrate having an off angle of 4°. The size of the SiC single crystal substrate 1 is not particularly limited, for example, a 10 mm 2 size.
[0046] Then, if Figure 4B As shown, a thin film 30 containing carbon is deposited on a SiC single crystal substrate 1 from which a natural oxide film has been removed. The thin film 30 is deposited using a deposition method that can be controlled at a molecular layer level. For example, the thin film 30 can be deposited using a physical vapor growth method, a chemical vapor growth method, a wet deposition method, etc. More specifically, a Langmuir-Blodgett method or an evaporation polymerization method can be used.
[0047] The film 30 may also be a Langmuir-Blodgett film or a self-organized monomolecular film using the Langmuir-Blodgett method. In addition, the film 30 may also include a molecular film having a weight average molecular weight of 100 to 1000. Examples of the molecular film having a weight average molecular weight of 100 to 1000 include stearic acid (C 2+) which is a saturated fatty acid. 17 H 35 COOH), palmitic acid (C 15 H 31 COOH) etc.
[0048] The film 30 functions as a carbon supply source for forming a carbon-containing layer such as a graphene layer. The thickness of the film 30 can be any thickness as long as it can function as a carbon supply source. The thickness of the film 30 is, for example, 0.3 nm to 100 nm, 1 nm to 90 nm, or 10 nm to 80 nm.
[0049] Here, stearic acid (C 17 H 35 COOH) is dissolved in hexane at a concentration of 1 mM, and the SiC single crystal substrate 1 from which the natural oxide film has been removed is immersed in a solution obtained by dropping the dissolving solution in pure water, and vertically pulled up and dried, thereby coating the SiC single crystal substrate 1 with a monomolecular film as a thin film 30. The drying time is, for example, 60 minutes. Furthermore, the SiC single crystal substrate 1 coated with the monomolecular film is placed in a high-frequency induction heating furnace and evacuated. The evacuation can be performed, for example, until the temperature reaches 1×10 - 3 N / m2 the following.
[0050] Then, if Figure 4C As shown, the SiC single crystal substrate 1 is subjected to a first heat treatment to carbonize the thin film 30 to form a thin film 30A. The first heat treatment is performed at a temperature of 1×10 -4 N / m 2 In a vacuum environment below 1×10 4 N / m 2 Above 1×10 6 N / m 2 The following inert gas environment is used for the experiment. As the inert gas, for example, argon gas can be mentioned.
[0051] Here, after coating the monomolecular film as the thin film 30 on the SiC single crystal substrate 1, the SiC single crystal substrate 1 is flushed with an inert gas such as argon, and after reaching atmospheric pressure, the SiC single crystal substrate 1 is heat-treated in an inert gas environment to carbonize the monomolecular film, thereby forming the thin film 30A. The heat treatment temperature is, for example, 400°C.
[0052] In addition, the thin film 30 may be further subjected to heat treatment before the first heat treatment. For example, the heating rate of the heat treatment may be 100°C / min to 18000°C / min, and resistance heating, lamp annealing, and high-frequency induction heating may be used. By subjecting the thin film 30 to the heat treatment, the thin film 30 can be efficiently carbonized in the first heat treatment.
[0053] Then, if Figure 4D As shown, the SiC single crystal substrate 1 stacked with the thin film 30A is subjected to a second heat treatment, and the carbon-containing layer is formed on the SiC single crystal substrate 1 using the carbon supplied by the thin film 30A. The carbon-containing layer includes a stacked body including a reconstructed surface layer 10a in contact with the Si termination surface 1Si of the SiC single crystal substrate 1 and a graphene layer 10 in contact with the reconstructed surface layer 10a.
[0054] The second heat treatment is performed at a temperature of, for example, 1000° C. to 2000° C. Here, as the heat treatment, the -4 N / m 2 In a vacuum environment, the SiC single crystal substrate 1 stacked with the thin film 30A is heated at 1600°C for 5 minutes to form a carbon-containing layer on the surface of the SiC single crystal substrate 1. The heating rate at this time is, for example, 400°C / second. The formed carbon-containing layer has an area ratio of, for example, only the reconstructed surface layer 10a and the stacked body including the reconstructed surface layer 10a and the graphene layer 10 of 80:20.
[0055] Then, if Figure 3As shown, an epitaxial layer 3 is formed on the graphene layer 10 included in the carbon-containing layer. Through the above operations, the composite substrate 100B is completed. The formation (deposition) method of the epitaxial layer 3 is not particularly limited, for example, physical vapor growth method and chemical vapor growth method can be used. In addition, the epitaxial layer 3 can be formed at a substrate temperature of 1000°C or more and 2000°C or less.
[0056] The raw material gas used to form the epitaxial layer 3 is not particularly limited, and for example, propane (C3H8) and silane (SiH4) may be used at a volume ratio of 1:3. In addition, silane (SiH4) may be used as a precursor of Si, and propane (C3H8) may be used as a precursor of C. In addition, argon gas that suppresses etching of the graphene layer 10 may be used as a carrier gas for transporting the raw material gas.
[0057] The thickness of the epitaxial layer 3 is not particularly limited, and is, for example, 500 nm.
[0058] (Other embodiments)
[0059] As described above, several embodiments are described, but the discussion and drawings that constitute part of the disclosure are illustrative and should not be understood as limiting. Based on this disclosure, the industry should be clear about various alternative embodiments, examples, and application technologies. As such, the embodiments include various embodiments not described here, etc.
[0060] <Example of Implementation>
[0061] Examples of this embodiment are given below. This embodiment is not limited to the following examples.
[0062] [Note 1]
[0063] A method for manufacturing a composite substrate 100, 100A, 100B includes the following steps: depositing a thin film 30 containing carbon on a SiC single crystal substrate 1 using a deposition method that can be controlled at a molecular layer level; and
[0064] Performing heat treatment to form a carbon-containing layer on the SiC single crystal substrate 1 using carbon supplied from the thin film 30, the carbon-containing layer including either a stacked body in which the reconstructed surface layer 10a and the graphene layer 10 are stacked or the graphene layer 10; and
[0065] The difference in the number of carbon-containing layers on the SiC single crystal substrate 1 is one layer or less.
[0066] [Note 2]
[0067] The method for manufacturing composite substrate 100 , 100A, 100B according to [Supplementary Note 1], wherein thin film 30 includes a molecular film having a weight average molecular weight of 100 or more and 1000 or less.
[0068] [Note 3]
[0069] According to the method for manufacturing the composite substrate 100, 100A, 100B described in [Supplementary Note 1] or [Supplementary Note 2], the thin film 30 is a Langmuir-Blodgett film or a self-organized monomolecular film.
[0070] [Note 4]
[0071] According to the method for manufacturing the composite substrate 100, 100A, 100B described in any one of [Appendix 1] to [Appendix 3], the deposition of the thin film 30 is performed by any method selected from the group consisting of physical vapor growth, chemical vapor growth and wet deposition.
[0072] [Note 5]
[0073] According to the method for manufacturing the composite substrate 100, 100A, 100B described in [Supplementary Note 4], the deposition of the thin film 30 is performed using a Langmuir-Blodgett method or an evaporation polymerization method.
[0074] [Note 6]
[0075] The method for manufacturing composite substrate 100 , 100A, 100B according to any one of [Supplementary Note 1] to [Supplementary Note 5], wherein the thickness of thin film 30 is not less than 0.3 nm and not more than 100 nm.
[0076] According to [Supplementary Note 1] to [Supplementary Note 6], when forming the carbon-containing layer, carbon is supplied from the outside in addition to the SiC single crystal substrate, thereby improving the difference in the carbon-containing layer. In addition, when the composite substrate 100, 100A, 100B including the carbon-containing layer is used as a material for a semiconductor device or the like, the difference in epitaxial film growth in the semiconductor device can be reduced.
[0077] [Note 7]
[0078] The method for manufacturing a composite substrate 100, 100A, or 100B according to any one of [Supplement 1] to [Supplement 6], wherein the heat treatment includes a first heat treatment, and the first heat treatment is performed in a vacuum environment or an inert gas environment at a temperature of 300° C. to 1000° C.,
[0079] In the first heat treatment, the thin film 30 is carbonized.
[0080] [Note 8]
[0081] According to the manufacturing method of the composite substrate 100, 100A, 100B described in [Note 7], before the first heat treatment, the thin film is subjected to heat treatment by any one of the group consisting of resistance heating, lamp annealing and high-frequency induction heating at a heating rate of not less than 100°C / minute and not more than 18000°C / minute.
[0082] [Note 9]
[0083] The method for manufacturing the composite substrate 100, 100A, 100B according to [Supplementary Note 7] or [Supplementary Note 8], wherein the first heat treatment is performed at 1×10 -4 N / m 2 In a vacuum environment below 1×10 4 N / m 2 Above 1×10 6 N / m 2 The following inert gas atmosphere was used for the experiment.
[0084] [Note 10]
[0085] The method for manufacturing a composite substrate 100, 100A, or 100B according to any one of [Supplement 7] to [Supplement 9], wherein the heat treatment includes a second heat treatment, the second heat treatment being performed at a temperature of 1000° C. to 2000° C. after the first heat treatment,
[0086] In the second heat treatment, the thin film 30A is formed as a carbon-containing layer.
[0087] According to [Supplementary Note 7] to [Supplementary Note 10], by controlling the heat treatment conditions, the thin film 30 can be efficiently carbonized, and a carbon-containing layer can be formed on the SiC single crystal substrate 1 using carbon supplied from the thin film 30 .
[0088] [Note 11]
[0089] The method for manufacturing composite substrate 100B according to any one of [Supplement 1] to [Supplement 10] further includes the step of forming epitaxial layer 3 grown via the carbon-containing layer on SiC single crystal substrate 1 after forming thin film 30 as the carbon-containing layer.
[0090] [Note 12]
[0091] According to the method for manufacturing the composite substrate 100B described in [Supplementary Note 11], the deposition of the epitaxial layer 3 is performed by any method selected from the group consisting of a physical vapor growth method and a chemical vapor growth method.
[0092] [Note 13]
[0093] The method for manufacturing composite substrate 100B according to [Supplementary Note 11] or [Supplementary Note 12], wherein epitaxial layer 3 is formed at a substrate temperature of 1000° C. to 2000° C.
[0094] According to [Supplementary Note 11] to [Supplementary Note 13], the difference in the number of graphene layers is small, and the crystallinity of the epitaxial layer 3 can be improved.
[0095] [Note 14]
[0096] A composite substrate 100, 100A, 100B comprises: a SiC single crystal substrate 1 having an off angle; and
[0097] The carbon-containing layer is disposed in contact with the surface of the SiC single crystal substrate 1 and includes either a stacked body in which the reconstructed surface layer 10a and the graphene layer 10 are stacked or the graphene layer 10; and
[0098] When the outermost surface of the SiC single crystal substrate 1 is the Si termination surface 1si, a stacked body is arranged on the SiC single crystal substrate 1, and the stacked body has one or two graphene layers 10.
[0099] When the outermost surface of the SiC single crystal substrate 1 is a C-terminated surface 1 c , one or two graphene layers 10 are arranged on the SiC single crystal substrate 1 .
[0100] [Note 15]
[0101] The composite substrate 100 , 100A, 100B according to [Supplementary Note 14], wherein the off angle is not less than 0.5° and not more than 10°.
[0102] [Note 16]
[0103] In the composite substrate 100 , 100A, or 100B according to [Supplementary Note 14] or [Supplementary Note 15], the SiC single crystal substrate 1 has a crystal structure of either a hexagonal crystal or a cubic crystal.
[0104] [Note 17]
[0105] The composite substrate 100 , 100A, or 100B according to any one of [Supplementary Note 14] to [Supplementary Note 16], wherein the number of graphene layers 10 included in the carbon-containing layer is one.
[0106] According to [Supplementary Note 14] to [Supplementary Note 17], when forming the carbon-containing layer, carbon is supplied from the outside in addition to the SiC single crystal substrate, thereby improving the difference in the carbon-containing layer. In addition, when the composite substrate 100, 100A, 100B including the carbon-containing layer is used as a material for a semiconductor device or the like, the difference in epitaxial film growth in the semiconductor device can be reduced.
[0107] [Note 18]
[0108] The composite substrate 100B according to any one of [Supplementary Note 14] to [Supplementary Note 17], further comprising an epitaxial layer 3, wherein the epitaxial layer 3 is arranged above the graphene layer 10 included in the carbon-containing layer,
[0109] Epitaxial layer 3 has the same crystal system as that of SiC single crystal substrate 1 .
[0110] According to [Supplementary Note 18], the graphene layer 10 can improve the crystallinity of the epitaxial layer 3 .
[0111] [Explanation of Symbols]
[0112] 1: SiC single crystal substrate
[0113] 1c: C termination surface
[0114] 1si: Si termination surface
[0115] 3: Epitaxial layer
[0116] 10: Graphene layer
[0117] 10a: Reconstructing the surface layer
[0118] 30, 30A: Thin film
[0119] 100, 100A, 100B: composite substrate.
Claims
1. A method for manufacturing a composite substrate, comprising the steps of: depositing a thin film containing carbon on a SiC single crystal substrate using a deposition method that can be controlled at a molecular layer level; and Performing heat treatment to form a carbon-containing layer on the SiC single crystal substrate using carbon supplied by the thin film, the carbon-containing layer including any one of a stacked body in which a reconstructed surface layer and a graphene layer are stacked or a graphene layer; and The difference in the number of layers of the carbon-containing layers on the SiC single crystal substrate is one layer or less. 2 . The method for manufacturing a composite substrate according to claim 1 , wherein the thin film comprises a molecular film having a weight average molecular weight of 100 or more and 1000 or less. 3 . The method for manufacturing a composite substrate according to claim 1 , wherein the thin film is a Langmuir-Blodgett film or a self-organized monomolecular film. 4 . The method for manufacturing a composite substrate according to claim 1 , wherein the thin film is deposited by any one method selected from the group consisting of a physical vapor growth method, a chemical vapor growth method, and a wet deposition method. 5 . The method for manufacturing a composite substrate according to claim 4 , wherein the deposition of the thin film is performed by using a Langmuir-Blodgett method or an evaporation polymerization method. 6 . The method for manufacturing a composite substrate according to claim 1 , wherein a thickness of the thin film is not less than 0.3 nm and not more than 100 nm.
7. The method for manufacturing a composite substrate according to any one of claims 1 to 6, wherein the heat treatment includes a first heat treatment, and the first heat treatment is performed in a vacuum environment or an inert gas environment at a temperature of 300° C. to 1000° C., In the first heat treatment, the thin film is carbonized.
8. The method for manufacturing a composite substrate according to claim 7, wherein before the first heat treatment, the thin film is subjected to heat treatment at a heating rate of not less than 100°C / minute and not more than 18000°C / minute and selected from any one of the group consisting of resistance heating, lamp annealing and high-frequency induction heating.
9. The method for manufacturing a composite substrate according to claim 7 or 8, wherein the first heat treatment is performed at 1×10 -4 N / m 2 In a vacuum environment below 1×10 4 N / m 2 Above 1×10 6 N / m 2 The following inert gas atmosphere was used for the experiment.
10. The method for manufacturing a composite substrate according to any one of claims 7 to 9, wherein the heat treatment includes a second heat treatment, the second heat treatment being performed at a temperature of 1000° C. to 2000° C. after the first heat treatment, In the second heat treatment, the thin film is formed as a carbon-containing layer.
11. The method for manufacturing a composite substrate according to any one of claims 1 to 10, further comprising the following steps: After the thin film is formed as a carbon-containing layer, an epitaxial layer grown via the carbon-containing layer on the SiC single crystal substrate is formed. 12 . The method for manufacturing a composite substrate according to claim 11 , wherein the deposition of the epitaxial layer is performed by any one method selected from the group consisting of a physical vapor growth method and a chemical vapor growth method. 13 . The method for manufacturing a composite substrate according to claim 11 , wherein the epitaxial layer is formed at a substrate temperature of 1000° C. to 2000° C.
14. A composite substrate comprising: a SiC single crystal substrate having an off angle; and a carbon-containing layer disposed in contact with the surface of the SiC single crystal substrate and comprising any one of a stacked body formed by stacking a reconstructed surface layer and a graphene layer or a graphene layer; and In a case where the outermost surface of the SiC single crystal substrate is a Si termination surface, the stacked body is arranged above the SiC single crystal substrate, and the graphene layer of the stacked body is one layer or two layers, When the outermost surface of the SiC single crystal substrate is a C-terminated surface, one or two graphene layers are arranged on the SiC single crystal substrate. The composite substrate according to claim 14 , wherein the off angle is not less than 0.5° and not more than 10°. 16 . The composite substrate according to claim 14 , wherein the SiC single crystal substrate has a crystal structure of either a hexagonal crystal or a cubic crystal. 17 . The composite substrate according to claim 14 , wherein the carbon-containing layer includes one graphene layer.
18. The composite substrate according to any one of claims 14 to 17, further comprising an epitaxial layer, wherein the epitaxial layer is arranged above the graphene layer included in the carbon-containing layer. The epitaxial layer has the same crystal system as that of the SiC single crystal substrate.
Citation Information
Patent Citations
Method for producing graphene / sic composite material and graphene / sic composite material obtained by same
WO2010023934A1