Heterogeneous composite substrate and preparation method and application thereof

The amorphous silicon layer is converted into a SiO2 layer through oxygen ion implantation technology, which solves the problem of insufficient performance of silicon-based semiconductor materials under high temperature and high pressure, significantly improves the resistance and bonding strength of the composite substrate, and improves device performance.

CN119092398APending Publication Date: 2024-12-06TJ INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411199029.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The composite substrates of existing silicon-based semiconductor materials have poor resistance under high temperature and high pressure, and the bonding strength of the amorphous silicon layer is insufficient, which affects device performance.

Method used

The oxygen-rich layer is introduced through oxygen ion implantation technology, which converts part of the amorphous silicon layer into a SiO2 layer, improves bonding strength and reduces the thermal resistance of the bonding interface, and improves substrate performance.

Benefits of technology

The high temperature and high pressure resistance of the heterogeneous composite substrate is significantly improved, the bonding strength between the silicon substrate and the silicon carbide layer is enhanced, the thermal resistance is reduced, and the overall performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092398A_ABST
    Figure CN119092398A_ABST
Patent Text Reader

Abstract

The invention provides a heterogeneous composite substrate and a preparation method and application thereof. The preparation method comprises the following steps: preparing a silicon substrate and a silicon carbide substrate, performing oxidation on the surface of one side of the silicon substrate to form a SiO2 layer, and performing non-oxygen ion implantation on the surface of one side of the silicon carbide substrate to form a damaged layer; respectively carrying out oxygen ion implantation on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer; bonding to obtain a bonding body with a silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate structure; and carrying out annealing treatment on the bonding body to enable at least part of the amorphous silicon layer to be converted into a SiO2 layer, and then carrying out splitting treatment to enable the bonding body to be split along the damage layer to obtain a residual material layer and the heterogeneous composite substrate. According to the invention, at least part of the amorphous silicon layer is converted into the SiO2 layer, so that the high-temperature and high-pressure resistance of the heterogeneous composite substrate is improved, the thermal resistance of a bonding interface is reduced, and the bonding strength is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor devices, and in particular relates to a heterogeneous composite substrate and a preparation method and application thereof. Background Art

[0002] Nowadays, silicon-based semiconductor materials composed of insulating substrates and silicon carbide combine the advantages of silicon on insulators and silicon carbide, and are suitable for preparing high-temperature and high-power devices. The preparation scheme is to transfer the silicon carbide film to the silicon oxide substrate in a bonding manner by ion implantation combined with stripping technology in the silicon carbide substrate. The commonly used bonding method is room temperature bonding technology. Since the bonding process does not require high temperature to be applied to the composite substrate prepared in this way, the warping problem caused by the difference in thermal expansion coefficients of heterogeneous materials during bonding can be solved. However, when silicon carbide is directly bonded to silicon oxide using room temperature bonding technology, the bonding interface bonding strength is poor. Therefore, the prior art introduces amorphous silicon between silicon oxide and silicon carbide, and bonds through amorphous silicon as an intermediate layer to improve the bonding strength. The prepared composite substrate includes silicon oxide layer-amorphous silicon layer-silicon carbide layer in sequence. However, as a semiconductor layer, the amorphous silicon layer has poor high temperature and high voltage resistance performance than the silicon carbide layer, and its existence directly affects the high temperature and high pressure resistance performance of the composite substrate.

[0003] Therefore, how to improve the high temperature and high pressure resistance of the composite substrate is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a heterogeneous composite substrate and a preparation method and application thereof. In the process step, the present invention introduces an oxygen-rich layer by means of oxygen ion implantation, so that at least part of the amorphous silicon layer is converted into a SiO2 layer, thereby converting the amorphous silicon layer with semiconductor properties into a silicon oxide layer with insulating properties. This preparation method effectively improves the high temperature and high pressure resistance of the heterogeneous composite substrate, while also reducing the thermal resistance of the bonding interface, increasing the bonding strength between the silicon substrate and the silicon carbide layer, and significantly improving the performance of the heterogeneous composite substrate.

[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0007] (1) preparing a silicon substrate and a silicon carbide substrate, performing oxidation on one surface of the silicon substrate to form a SiO2 layer, and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer;

[0008] (2) implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer;

[0009] (3) depositing a first amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer, and depositing a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; or, depositing an amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate;

[0010] Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate;

[0011] (4) performing an annealing treatment on the bonded body so that at least a portion of the amorphous silicon layer is converted into a SiO2 layer, and then performing a splitting treatment so that the bonded body is split along the damaged layer to obtain a residual layer and the heterogeneous composite substrate.

[0012] The present invention introduces an oxygen-rich layer by means of oxygen ion implantation in the process step, so that at least part of the amorphous silicon layer is converted into a SiO2 layer, thereby converting the amorphous silicon layer with semiconductor properties into a silicon oxide layer with insulating properties. This preparation method effectively improves the high temperature and high pressure resistance of the heterogeneous composite substrate, while also reducing the thermal resistance of the bonding interface, increasing the bonding strength between the silicon substrate and the silicon carbide layer, and significantly improving the performance of the heterogeneous composite substrate.

[0013] It should be noted that the residual layer can be recycled and reused as a silicon carbide substrate.

[0014] Preferably, the non-oxygen ions in step (1) include hydrogen ions and / or helium ions.

[0015] Preferably, the depth of the non-oxygen ion implantation in step (1) is 0.8-1.2 μm, for example, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm or 1.2 μm.

[0016] Preferably, the depth of oxygen ion implantation on the surface of the SiO2 layer in step (2) is 4-30 nm, for example, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm.

[0017] In the present invention, if the depth of oxygen ion implantation on the surface of the SiO2 layer is too shallow, the probability of sputtering is high, which may affect the surface roughness. Moreover, if the depth is too shallow, the set dose becomes smaller accordingly, and the corresponding concentration becomes smaller. Since the concentration required for the conversion of the amorphous silicon layer into SiO2 is relatively large, the probability of the conversion of the amorphous silicon layer into SiO2 becomes smaller. If the depth of oxygen ion implantation on the surface of the SiO2 layer is too deep, it cannot effectively diffuse into the amorphous silicon layer, and the amorphous silicon layer cannot be converted into SiO2, that is, the probability of the conversion of the amorphous silicon layer into SiO2 becomes smaller.

[0018] Preferably, the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate in step (2) is 2-30 nm, for example, it can be 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm.

[0019] In the present invention, if the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is too shallow, the probability of sputtering is high, which may affect the surface roughness. In addition, if the depth is too shallow, the probability of the amorphous silicon layer being converted into SiO2 will be reduced. If the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is too deep, it will not be able to effectively diffuse into the amorphous silicon layer, thereby reducing the probability of the amorphous silicon layer being converted into SiO2.

[0020] Preferably, the oxygen ion implantation method in step (2) includes a channel implantation method.

[0021] Preferably, the parameters of the channel implantation method include:

[0022] The oxygen ion implantation energy is 1-100kev, for example, 1kev, 10kev or 100kev, and the oxygen ion implantation dose is 1×10 16 -1×10 18 Ions / cm 2 , for example, it can be 1×10 16 Ions / cm 2 , 5×10 16 Ions / cm 2 , 1×10 17 Ions / cm 2 , 5×101 7 Ions / cm 2 or 1×10 18 Ions / cm 2 etc., the Tilt angle is 0~60°, for example, it can be 0, 10°, 20°, 30°, 40°, 50° or 60°, etc., the Twist angle is 0~90°, for example, it can be 0, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80° or 90°, etc.

[0023] It should be noted that if the silicon substrate or silicon carbide substrate itself has a tilt angle, it needs to be superimposed. For example, the tilt angle of the silicon substrate is 17°, and it itself has a tilt angle of 4°, which is 21° after superposition.

[0024] Preferably, during the oxygen ion implantation process of the ion implantation surface of the silicon carbide substrate in step (2), the implantation temperature is 20-800°C, for example, it can be 20°C, 50°C, 100°C, 200°C, 400°C, 600°C or 800°C, preferably 500-650°C.

[0025] In the present invention, the injection temperature during oxygen ion injection is controlled to be 20-800°C, which can reduce damage to the silicon carbide substrate, that is, dynamic annealing is performed to repair lattice damage, and preferably 500-650°C, because of the characteristics of silicon carbide itself, the diffusion coefficient of the element is small, and as the temperature increases, the injected ions are more likely to reach the target depth, that is, the O concentration can be relatively increased, and it is more convenient to combine with amorphous silicon. If the injection temperature is low, it may cause increased damage to silicon carbide, which is not conducive to subsequent repair and affects device performance; if the injection temperature is high, high-temperature diffusion may occur, that is, the injection depth becomes deeper, which is not conducive to the subsequent diffusion of O.

[0026] Preferably, the bonding parameters in step (3) include:

[0027] The bonding pressure is 10-100 kN, for example, 10 kN, 30 kN, 50 kN, 70 kN or 90 kN, and the vacuum degree is less than 1×10 -6 Pa, for example, can be 8×10 -7 Pa, 5×10 -7 Pa, 3×10 -7 Pa or 1×10 -7 Pa, etc., the bonding temperature is 20-30°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, etc.

[0028] Preferably, in the bonding body, the thickness of the amorphous silicon layer is 2-10 nm, for example, 2 nm, 4 nm, 6 nm, 8 nm or 10 nm.

[0029] Preferably, the annealing treatment temperature in step (4) is 600-900°C, for example, 600°C, 700°C, 800°C or 900°C, and the annealing time is 60-600min, for example, 660min, 100min, 200min, 300min, 400min, 500min or 600min.

[0030] In the present invention, if the annealing temperature is too low, O cannot diffuse into the amorphous silicon layer, which is not conducive to the subsequent conversion of the amorphous silicon layer into SiO2; if the annealing temperature is too high, it may bring certain thermal stress, causing deformation, and may cause peeling prematurely.

[0031] Preferably, the conversion rate of the SiO2 layer in step (4) is ≥50%, for example, it can be 50%, 60%, 70% or 80%.

[0032] Preferably, the temperature of the splitting treatment in step (4) is 800-1200°C, for example, it can be 800°C, 900°C, 1000°C, 1100°C or 1200°C, and the time is 1-60min, for example, it can be 1min, 5min, 10min, 20min, 30min, 40min, 50min or 60min, etc.

[0033] Preferably, after the splitting treatment in step (4), thinning treatment and heat treatment are also performed.

[0034] It should be noted that the purpose of the thinning process and the heat treatment is to increase the oxygen permeability and improve the conversion rate of the amorphous silicon layer into SiO2.

[0035] Preferably, the temperature of the heat treatment is 600-1100°C, for example, 600°C, 700°C, 800°C, 900°C, 1000°C or 1100°C.

[0036] Preferably, the preparation method comprises the following steps:

[0037] (1) preparing a silicon substrate and a silicon carbide substrate, performing thermal oxidation on one surface of the silicon substrate to form a SiO2 layer at a temperature of 800-1200° C. (e.g., 800° C., 900° C., 1000° C., 1100° C., or 1200° C.), and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer;

[0038] Wherein, the non-oxygen ions include hydrogen ions and / or helium ions, and the depth of non-oxygen ion implantation is 0.8-1.2 μm;

[0039] (2) using a channel implantation method, at a temperature of 20-800° C., implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer;

[0040] The depth of oxygen ion implantation on the surface of the SiO2 layer is 4-30 nm, and the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is 2-30 nm;

[0041] (3) depositing a first amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer, and depositing a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; or, depositing an amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate;

[0042] Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate;

[0043] The bonding parameters include: bonding pressure of 10-100 kN, vacuum degree of <1×10 -6 Pa, bonding temperature is 20-30°C;

[0044] (4) In an inert atmosphere or an oxygen atmosphere, the bonded body is annealed at a temperature of 600-1100° C. for 60-600 min, so that at least 50% of the amorphous silicon layer is converted into a SiO2 layer; then, the bonded body is split along the damaged layer to obtain a residual layer and a heterogeneous composite substrate precursor; then, the silicon carbide substrate in the heterogeneous composite substrate precursor is thinned, and then, a heat treatment is performed at 600-1100° C. in an oxygen atmosphere to obtain the heterogeneous composite substrate.

[0045] In a second aspect, the present invention provides a heterogeneous composite substrate, which is prepared by the preparation method described in the first aspect.

[0046] In a third aspect, the present invention provides a heterogeneous composite substrate as described in the second aspect, wherein the heterogeneous composite substrate is used for preparing a semiconductor device.

[0047] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] The present invention introduces an oxygen-rich layer by means of oxygen ion implantation in the process step, so that at least part of the amorphous silicon layer is converted into a SiO2 layer, thereby converting the amorphous silicon layer with semiconductor properties into a silicon oxide layer with insulating properties. This preparation method effectively improves the high temperature and high pressure resistance of the heterogeneous composite substrate, while also reducing the thermal resistance of the bonding interface, increasing the bonding strength between the silicon substrate and the silicon carbide layer, and significantly improving the performance of the heterogeneous composite substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is a process flow chart provided for Example 1 of the present invention. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Example 1

[0053] This embodiment provides a method for preparing a heterogeneous composite substrate, and its process flow chart is as follows: Figure 1 As shown, the preparation method comprises the following steps:

[0054] (1) preparing a silicon substrate and a silicon carbide substrate, performing thermal oxidation at 1000° C. on one surface of the silicon substrate to form a SiO2 layer with a thickness of 200 nm, and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer;

[0055] Wherein, the non-oxygen ions are hydrogen ions, and the implantation depth is 1 μm;

[0056] (2) using a channel implantation method, at a temperature of 600° C., implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer;

[0057] The depth of oxygen ion implantation on the surface of the SiO2 layer is 20 nm, and the implantation parameters include:

[0058] The oxygen ion implantation energy is 8kev and the oxygen ion implantation dose is 1×10 17 Ions / cm 2 , Tilt angle is 7°, Twist angle is 23°;

[0059] The depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is 20 nm, and the implantation parameters include:

[0060] The oxygen ion implantation energy is 12kev and the oxygen ion implantation dose is 1.4×10 17 Ions / cm 2 , Tilt angle is 17°, Twist angle is 0°;

[0061] (3) depositing a first sub-amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer, and depositing a second sub-amorphous silicon layer on the ion implantation surface of the silicon carbide substrate;

[0062] Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate, wherein the thickness of the amorphous silicon layer is 6 nm;

[0063] The bonding parameters include: bonding pressure of 50 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0064] (4) performing an annealing treatment at 750°C in an oxygen atmosphere for 120 min; then performing a splitting treatment at 1000°C for 20 min, so that the bonded body is split along the damaged layer to obtain a residual layer and a heterogeneous composite substrate precursor; thinning the silicon carbide substrate in the heterogeneous composite substrate precursor to obtain a silicon carbide layer with a thickness of 0.5 μm, and then performing a heat treatment at 950°C in an oxygen atmosphere for 120 min, so that the amorphous silicon layer is converted to obtain the heterogeneous composite substrate.

[0065] Example 2

[0066] This embodiment provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0067] (1) preparing a silicon substrate and a silicon carbide substrate, performing thermal oxidation at 1000° C. on one surface of the silicon substrate to form a SiO2 layer with a thickness of 200 nm, and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer;

[0068] Wherein, the non-oxygen ions are hydrogen ions, and the implantation depth is 1 μm;

[0069] (2) using a channel implantation method, at a temperature of 500° C., implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer;

[0070] The depth of oxygen ion implantation on the surface of the SiO2 layer is 15 nm, and the implantation parameters include:

[0071] The oxygen ion implantation energy is 6keV and the oxygen ion implantation dose is 7.6×10 16 Ions / cm 2 , Tilt angle is 7°, Twist angle is 23°;

[0072] The depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is 15 nm, and the implantation parameters include:

[0073] The oxygen ion implantation energy is 8kev and the oxygen ion implantation dose is 9.5×1017 Ions / cm 2 , Tilt angle is 17°, Twist angle is 0°;

[0074] (3) depositing an amorphous silicon layer with a thickness of 10 nm on the oxygen ion implanted surface of the SiO2 layer;

[0075] Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate;

[0076] The bonding parameters include: bonding pressure of 10 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0077] (4) performing an annealing treatment at 850°C in an oxygen atmosphere for 180 min; then performing a splitting treatment at 850°C for 50 min, so that the bonded body is split along the damaged layer to obtain a residual layer and a heterogeneous composite substrate precursor; thinning the silicon carbide substrate in the heterogeneous composite substrate precursor to obtain a silicon carbide layer with a thickness of 0.35 μm, and then performing a heat treatment at 900°C in an oxygen atmosphere for 180 min, so that the amorphous silicon layer is converted to obtain the heterogeneous composite substrate.

[0078] Example 3

[0079] This embodiment provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0080] (1) preparing a silicon substrate and a silicon carbide substrate, performing thermal oxidation at 1000° C. on one surface of the silicon substrate to form a SiO2 layer with a thickness of 200 nm, and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer;

[0081] Wherein, the non-oxygen ions are hydrogen ions, and the implantation depth is 1 μm;

[0082] (2) using a channel implantation method, at a temperature of 650° C., implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer;

[0083] The depth of oxygen ion implantation on the surface of the SiO2 layer is 30 nm, and the implantation parameters include:

[0084] The oxygen ion implantation energy is 12kev and the oxygen ion implantation dose is 1.5×10 17 Ions / cm 2, Tilt angle is 7°, Twist angle is 23°;

[0085] The depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is 30 nm, and the implantation parameters include:

[0086] The oxygen ion implantation energy is 18kev and the oxygen ion implantation dose is 2.1×10 17 Ions / cm 2 , Tilt angle is 17°, Twist angle is 0°;

[0087] (3) depositing an amorphous silicon layer with a thickness of 10 nm on the ion implantation surface of the silicon carbide substrate;

[0088] Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate;

[0089] The bonding parameters include: bonding pressure of 70 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0090] (4) performing an annealing treatment at 800°C in an oxygen atmosphere for 60 minutes; then performing a splitting treatment at 1100°C for 15 minutes, so that the bonded body is split along the damaged layer to obtain a residual layer and a heterogeneous composite substrate precursor; thinning the silicon carbide substrate in the heterogeneous composite substrate precursor to obtain a silicon carbide layer with a thickness of 0.85 μm, and then performing a heat treatment in an oxygen atmosphere at 1100°C for 60 minutes, so that the amorphous silicon layer is converted to obtain the heterogeneous composite substrate.

[0091] Example 4

[0092] The difference between this embodiment and embodiment 1 is that no thinning process is performed in step (4).

[0093] The rest of the preparation methods and parameters were the same as those in Example 1.

[0094] Example 5

[0095] The difference between this embodiment and embodiment 1 is that no thinning treatment is performed in step (4), and the atmosphere for the annealing treatment and the splitting treatment is a nitrogen atmosphere.

[0096] The rest of the preparation methods and parameters were the same as those in Example 1.

[0097] Example 6

[0098] The difference between this embodiment and embodiment 1 is that the depth of oxygen ion implantation into the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate in step (2) is 1 nm.

[0099] The rest of the preparation methods and parameters were the same as those in Example 1.

[0100] Example 7

[0101] The difference between this embodiment and embodiment 1 is that the depth of oxygen ion implantation into the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate in step (2) is both 100 nm.

[0102] The rest of the preparation methods and parameters were the same as those in Example 1.

[0103] Example 8

[0104] The difference between this embodiment and embodiment 1 is that the temperature of oxygen ion implantation in step (2) is 20°C.

[0105] The rest of the preparation methods and parameters were the same as those in Example 1.

[0106] Example 9

[0107] The difference between this embodiment and embodiment 1 is that the temperature of oxygen ion implantation in step (2) is 800°C.

[0108] The rest of the preparation methods and parameters were the same as those in Example 1.

[0109] Example 10

[0110] The difference between this embodiment and embodiment 1 is that the temperature of the annealing treatment in step (4) is 500°C.

[0111] The rest of the preparation methods and parameters were the same as those in Example 1.

[0112] Embodiment 11

[0113] The difference between this embodiment and embodiment 1 is that the temperature of the annealing treatment in step (4) is 1000°C.

[0114] The rest of the preparation methods and parameters were the same as those in Example 1.

[0115] Comparative Example 1

[0116] The difference between this comparative example and Example 1 is that in step (3), the first sub-amorphous silicon layer is not deposited on the oxygen ion implanted surface of the SiO2 layer, nor is the second sub-amorphous silicon layer deposited on the ion implanted surface of the silicon carbide substrate.

[0117] The rest of the preparation methods and parameters were the same as those in Example 1.

[0118] Comparative Example 2

[0119] The difference between this comparative example and Example 1 is that step (2) is not performed.

[0120] The rest of the preparation methods and parameters were the same as those in Example 1.

[0121] Performance Testing

[0122] The bonding strength, interface thermal resistance and thermal conductivity of the heterogeneous composite substrates prepared in the above embodiments and comparative examples were tested.

[0123] The specific test conditions include: conversion rate is evaluated by XRD; bonding strength is tested by opening crack; and interface thermal resistance is tested by Time-domain thermoreflectance (TDTR).

[0124] The test results are shown in Table 1.

[0125] Table 1

[0126]

[0127]

[0128] analyze:

[0129] As can be seen from the above table, the present invention introduces an oxygen-rich layer by means of oxygen ion implantation in the process step, so that at least part of the amorphous silicon layer is converted into a SiO2 layer, thereby converting the amorphous silicon layer with semiconductor properties into a silicon oxide layer with insulating properties. This preparation method effectively improves the high temperature and high pressure resistance of the heterogeneous composite substrate, while also reducing the thermal resistance of the bonding interface, increasing the bonding strength between the silicon substrate and the silicon carbide layer, and significantly improving the performance of the heterogeneous composite substrate.

[0130] By comparing Example 1 with Examples 6-7, it can be seen that if the depth of oxygen ion implantation into the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate is too shallow, the probability of sputtering is relatively high, which may affect the surface roughness. In addition, if the depth is too shallow, the set dose becomes smaller accordingly, and the corresponding concentration becomes smaller. Since the concentration required for the conversion of the amorphous silicon layer into SiO2 is relatively large, the probability of the conversion of the amorphous silicon layer into SiO2 becomes smaller. If the depth of oxygen ion implantation into the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate is too deep, it cannot effectively diffuse into the amorphous silicon layer, and the amorphous silicon layer cannot be converted into SiO2, that is, the probability of the conversion of the amorphous silicon layer into SiO2 becomes smaller.

[0131] By comparing Example 1 with Examples 8-9, it can be seen that if the injection temperature is low, it may cause increased damage to silicon carbide, which is not conducive to subsequent repair and affects device performance; if the injection temperature is high, high-temperature diffusion may occur, that is, the injection depth becomes deeper, which is not conducive to the subsequent diffusion of O and has a certain impact on the conversion of the amorphous silicon layer into SiO2.

[0132] By comparing Example 1 with Examples 10-11, it can be seen that if the annealing temperature is too low, O cannot diffuse into the amorphous silicon layer, which is not conducive to the subsequent conversion of the amorphous silicon layer into SiO2; if the annealing temperature is too high, it may bring certain thermal stresses, causing deformation, and may cause peeling prematurely, which will have a certain impact on the conversion of the amorphous silicon layer into SiO2.

[0133] By comparing Example 1 with Comparative Example 1, it can be seen that if the amorphous silicon layer is not provided, the bonding strength is poor, and there is a risk of the top SiC layer falling off in subsequent processes, which makes the composite substrate meaningless, and the falling film layer will bring certain risks to subsequent processes and equipment.

[0134] By comparing Example 1 with Comparative Example 2, it can be seen that if the conversion process of the amorphous silicon layer is not performed, the thermal resistance of the bonding interface is large, indicating that the composite substrate has poor performance and large damage compared to the single crystal substrate, and the quality factor of the subsequent device is poor, which is not conducive to production and affects the device performance.

[0135] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a heterogeneous composite substrate, characterized in that: The preparation method comprises the following steps: (1) preparing a silicon substrate and a silicon carbide substrate, performing oxidation on one surface of the silicon substrate to form a SiO2 layer, and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer; (2) implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer; (3) depositing a first amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer, and depositing a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; or, depositing an amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate; (4) performing an annealing treatment on the bonded body so that at least a portion of the amorphous silicon layer is converted into a SiO2 layer, and then performing a splitting treatment so that the bonded body is split along the damaged layer to obtain a residual layer and the heterogeneous composite substrate.

2. The preparation method according to claim 1, characterized in that: The non-oxygen ions in step (1) include hydrogen ions and / or helium ions; Preferably, the depth of the non-oxygen ion implantation in step (1) is 0.8-1.2 μm.

3. The preparation method according to claim 1 or 2, characterized in that: The depth of oxygen ion implantation on the surface of the SiO2 layer in step (2) is 4-30 nm; Preferably, the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate in step (2) is 2-30 nm.

4. The preparation method according to any one of claims 1 to 3, characterized in that The oxygen ion implantation method in step (2) includes a channel implantation method; Preferably, the parameters of the channel implantation method include: The oxygen ion implantation energy is 1-100kev, and the oxygen ion implantation dose is 1×10 16 -1×10 18 Ions / cm 2 , the Tilt angle is 0~60°, and the Twist angle is 0~90°.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In the process of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate in step (2), the implantation temperature is 20-800° C., preferably 500-650° C.; Preferably, during the process of oxygen ion implantation into the surface of the SiO2 layer in step (2), the implantation temperature is 20-800°C, preferably 500-650°C.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The bonding parameters of step (3) include: The bonding pressure is 10-100kN, and the vacuum degree is less than 1×10 -6 Pa, bonding temperature is 20-30°C; Preferably, in the bonding body, the thickness of the amorphous silicon layer is 2-10 nm.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The temperature of the annealing treatment in step (4) is 600-900°C and the time is 60-600 min; preferably, the conversion rate of the SiO2 layer in step (4) is ≥50%; Preferably, the temperature of the splitting treatment in step (4) is 800-1200°C and the time is 1-60 min. Preferably, after the splitting treatment in step (4), thinning treatment and heat treatment are also performed; Preferably, the heat treatment temperature is 600-1100°C.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) preparing a silicon substrate and a silicon carbide substrate, performing thermal oxidation on one surface of the silicon substrate to form a SiO2 layer at a temperature of 800-1200° C., and performing non-oxygen ion implantation on one surface of the silicon carbide substrate to form a damaged layer; Wherein, the non-oxygen ions include hydrogen ions and / or helium ions, and the depth of non-oxygen ion implantation is 0.8-1.2 μm; (2) using a channel implantation method, at a temperature of 20-800° C., implanting oxygen ions on the surface of the SiO2 layer and the ion implantation surface of the silicon carbide substrate to form an oxygen-rich layer; The depth of oxygen ion implantation on the surface of the SiO2 layer is 4-30 nm, and the depth of oxygen ion implantation on the ion implantation surface of the silicon carbide substrate is 2-30 nm; (3) depositing a first amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer, and depositing a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; or, depositing an amorphous silicon layer on the oxygen ion implantation surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; Bonding the ion implanted surface of the silicon carbide substrate and the oxygen ion implanted surface of the SiO2 layer to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate; The bonding parameters include: bonding pressure of 10-100 kN, vacuum degree of <1×10 -6 Pa, bonding temperature is 20-30°C; (4) In an inert atmosphere or an oxygen atmosphere, the bonded body is annealed at a temperature of 600-1100° C. for 60-600 min, so that at least 50% of the amorphous silicon layer is converted into a SiO2 layer; then, the bonded body is split along the damaged layer to obtain a residual layer and a heterogeneous composite substrate precursor; then, the silicon carbide substrate in the heterogeneous composite substrate precursor is thinned, and then, a heat treatment is performed at 600-1100° C. in an oxygen atmosphere to obtain the heterogeneous composite substrate.

9. A heterogeneous composite substrate, characterized in that: The heterogeneous composite substrate is prepared by the preparation method according to any one of claims 1 to 8.

10. A heterogeneous composite substrate as claimed in claim 9, characterized in that: The heterogeneous composite substrate is used for preparing semiconductor devices.