Solar cell and photovoltaic module
By setting texture structures and tunneling oxide layers of different thicknesses on the silicon substrate of the solar cell, the problem of tunneling oxide layers reducing the electron recombination rate is solved, and the efficiency and electrochemical performance of the solar cell are improved.
Patent Information
- Application Number
- CN202411170344.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The tunneling oxide layer in existing solar cells reduces the electron recombination rate of the battery surface poorly and reduces the conversion efficiency of the solar cell.
The texture structure is set on the silicon substrate of the solar cell. The thickness of the tunnel oxide layer on the end and sides is different. A thicker tunnel oxide layer is set on the sides to reduce the interfacial state density and improve the passivation effect. The side surfaces in the comprehensive texture structure are arranged. A tunneling oxide layer of corresponding thickness is provided with defects in the end face to reduce surface recombination and improve carrier collection rate.
By setting the tunneling oxide layer of corresponding thicknesses by the defects of the side and end surfaces in the integrated texture structure, a better passivation effect is achieved, and the efficiency and electrochemical performance of the solar cell are improved.
Smart Images

Figure CN119092557A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar photovoltaic technology, and in particular to a solar cell and a photovoltaic module. Background Art
[0002] Solar cells are devices that directly convert light energy into electrical energy. Some solar cells are provided with a tunneling oxide layer, which together with the doped polysilicon layer constitutes a passivation contact structure. The main function of the tunneling oxide layer is to reduce the electron recombination rate on the surface of the cell. However, the tunneling oxide layer in the prior art has a poor effect in reducing the electron recombination rate on the surface of the cell, which reduces the conversion efficiency of the solar cell. Summary of the invention
[0003] In view of this, the present invention proposes a solar cell and a photovoltaic module, aiming to partially or completely solve the technical problem that the tunneling oxide layer in the existing solar cells is poor in reducing the electron recombination rate on the cell surface, thereby reducing the conversion efficiency of the solar cell.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] In a first aspect, an embodiment of the present invention provides a solar cell, comprising a silicon substrate, a tunneling oxide layer and a doping layer stacked in sequence; a side of the silicon substrate close to the tunneling oxide layer is a first surface, and along the thickness direction of the silicon substrate, the silicon substrate is provided with at least one first surface, and the first surface is provided with a texture structure, and the texture structure includes an end face and a side face arranged in the thickness direction of the silicon substrate; along the thickness direction of the silicon substrate, the thickness of the tunneling oxide layer on the end face is a first thickness; along the direction away from the side face, the thickness of the tunneling oxide layer on the side face is a second thickness; the first thickness is less than the second thickness.
[0006] Optionally, the ratio of the second thickness to the first thickness is W, 1<W≤4.
[0007] Optionally, the first thickness is greater than or equal to 0.1 nm; preferably, the first thickness is in the range of 0.5 nm-1.5 nm.
[0008] Optionally, the second thickness is greater than or equal to 0.3 nm; preferably, the second thickness is in the range of 0.5 nm-2 nm.
[0009] Optionally, the density of the tunneling oxide layer on the end surface is less than the density of the tunneling oxide layer on the side surface.
[0010] Optionally, along the thickness direction of the silicon substrate, the height range from the end face to the first surface is 1um-10um; preferably, the height range from the end face to the first surface is 1um-2um.
[0011] Optionally, the end face and the side face form a tower base, and the tower base protrudes from the first surface, or the tower base is recessed in the first surface.
[0012] Optionally, the tower base protruding from the first surface includes at least two tower-shaped protrusions stacked in sequence to form a pyramid shape.
[0013] Optionally, in a top view, the width of the tower base is in the range of 5um-80um; preferably, the width of the tower base is in the range of 10um-30um.
[0014] Optionally, along the thickness direction of the silicon substrate, the thickness of the tunnel oxide layer on the surface of the first surface except the tower base is a third thickness, and the third thickness is less than the second thickness.
[0015] Optionally, along the thickness direction of the silicon substrate, the thickness range of the doping layer is 50nm-300nm; preferably, the thickness range of the doping layer is 80nm-180nm.
[0016] Optionally, the doped layer is a first doped layer, and the solar cell further includes a second passivation layer and a second doped layer; the first surface is respectively provided with the tunneling oxide layer and the second passivation layer, the tunneling oxide layer and the second passivation layer are spaced apart, the surface of the tunneling oxide layer facing away from the silicon substrate is connected to the first doped layer, and the surface of the second passivation layer facing away from the silicon substrate is connected to the second doped layer.
[0017] Optionally, the doping type of the first doping layer is opposite to the doping type of the second doping layer.
[0018] In a second aspect, an embodiment of the present invention provides a photovoltaic module, which includes a cover plate, a back plate, and a solar cell as described above disposed between the cover plate and the back plate.
[0019] In the solar cell of the present invention, along the thickness direction of the silicon substrate, the thickness of the tunneling oxide layer on the end face is a first thickness; along the direction away from the side face, the thickness of the tunneling oxide layer on the side face is a second thickness; the first thickness is less than the second thickness; that is, a thicker tunneling oxide layer is set on the side face with more defects to reduce the interface state density and improve the passivation effect. The solar cell of the embodiment of the present application sets a tunneling oxide layer of corresponding thickness according to the defects of the side face and the end face in the comprehensive texture structure, reduces the surface recombination of the texture structure, achieves a better passivation effect, and balances the carrier collection rate, thereby improving the efficiency and electrochemical performance of the solar cell.
[0020] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for describing the embodiments are briefly introduced below.
[0022] Figure 1 is a schematic structural diagram of a solar cell in an embodiment of the present invention;
[0023] Figure 2 is a structural diagram of a first texture structure in an embodiment of the present invention;
[0024] Figure 3 is a schematic structural diagram of a second texture structure in an embodiment of the present invention;
[0025] Figure 4 is a schematic structural diagram of a third texture structure in an embodiment of the present invention;
[0026] Figures 5 to 7 A schematic diagram showing the steps of preparing a solar cell in an embodiment of the present invention is shown;
[0027] Figures 8 to 12 A schematic diagram showing the steps of preparing another solar cell in an embodiment of the present invention is shown;
[0028] Fig.13 A transmission electron microscope test image 1 of a solar cell according to an embodiment of the present invention;
[0029] Fig.14 FIG2 is a second transmission electron microscope test image of a solar cell according to an embodiment of the present invention.
[0030] Description of reference numerals:
[0031] 10-silicon substrate; 11-first surface; 12-texture structure; 13-end surface; 14-side surface; 15-second surface; 16-tower base;
[0032] 21-tunneling oxide layer; 22-doping layer; 23-first doping layer; 24-first passivation layer; 25-second doping layer; 26-first anti-reflection layer; 27-second passivation layer; 28-third passivation layer; 29-third anti-reflection layer; 30-second anti-reflection layer; 31-third doping layer;
[0033] 41 - first electrode; 42 - second electrode; 51 - transparent conductive layer; 52 - first opening; 53 - second opening. DETAILED DESCRIPTION
[0034] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can also be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0035] The present application embodiment discloses a solar cell, referring to Figures 1 to 4 As shown, the solar cell includes a silicon substrate 10, a tunneling oxide layer 21 and a doping layer 22 stacked in sequence; the side of the silicon substrate 10 close to the tunneling oxide layer 21 is a first surface 11, and the thickness direction of the silicon substrate 10 is the thickness direction of the silicon substrate 10. Figure 1 In the direction of the middle arrow Z, the silicon substrate 10 is provided with at least one first surface 11, the first surface 11 is provided with a texture structure 12, and the texture structure 12 includes an end face 13 and a side face 14 arranged in the thickness direction of the silicon substrate 10; along the thickness direction of the silicon substrate 10, the thickness of the tunneling oxide layer 21 on the end face 13 is a first thickness; along the direction away from the side face 14 (the direction away from the side face 14 refers to Figure 1 The thickness of the tunnel oxide layer 21 on the side surface 14 is the second thickness; the first thickness is less than the second thickness.
[0036] Among them, in the solar cell, the silicon substrate 10 is provided with at least one first surface 11 along the thickness direction of the silicon substrate 10. In the case where the silicon substrate 10 is provided with one first surface 11, the silicon substrate 10 has a first surface 11 and a second surface 15, and the first surface 11 and the second surface 15 are relatively distributed, that is, one of the first surface 11 and the second surface 15 is the front side of the silicon substrate 10, and the other of the first surface 11 and the second surface 15 is the back side of the silicon substrate 10. In the case where the silicon substrate 10 is provided with two first surfaces 11, one of the two first surfaces 11 is the front side of the silicon substrate 10, and the other is the back side of the silicon substrate 10.
[0037] A texture structure 12 is provided on the first surface 11 of the silicon substrate 10. The texture structure 12 can improve the light capture efficiency, reduce the reflection of light, increase the diffusion and absorption of light inside the solar cell, and thus improve the photoelectric conversion efficiency. The texture structure 12 includes an end face 13 provided in the thickness direction of the silicon substrate 10. The end face 13 is an approximately parallel face, and the end face 13 is approximately parallel to the first surface 11; the side face 14 has an angle with the first surface 11 and intersects with the end face 13. Specifically, one end of the texture structure 12 in the positive direction in the arrow Z direction is the end face 13. For further reference, Figure 1 As shown, the end surface 13 is the highest surface in the texture structure 12, and the end surface 13 is higher than the side surface 14; or, the other end of the texture structure 12 in the negative direction in the arrow Z direction is the end surface 13, and further reference is made to Figure 4 As shown, the texture structure 12 has an end surface 13 recessed from the first surface 11 to form a groove bottom. The end surface 13 is the lowest surface in the texture structure 12 , and is lower than the side surface 14 .
[0038] In a solar cell, the tunneling oxide layer 21 is a very thin oxide film made of silicon dioxide (SiO2) or other similar oxide materials. The tunneling oxide layer 21 is usually used as a charge selection layer, which allows electrons to pass through while blocking holes. The tunneling oxide layer 21 is used to provide a low-resistance path for electrons to tunnel from the silicon substrate 10 to the doping layer 22, which can reduce the energy loss of electrons when passing through the interface and help prevent the recombination of photogenerated charges inside the solar cell. The doping layer 22 refers to a polycrystalline silicon film containing impurity elements (such as group V elements and group III elements), and the specific doping elements depend on the doping type in the doping layer 22. The doping layer 22 can effectively collect and transmit photogenerated charges. The tunneling oxide layer 21 and the doping layer 22 play an important role in improving the efficiency and stability of solar cells.
[0039] The inventors found in the study that after the silicon substrate 10 is polished, the texture structure 12 on the first surface 11 of the silicon substrate 10 has more defects on the side 14, which increases the surface recombination, reduces the tunneling ability, and affects the collection of carriers. The tunneling oxide layer 21 usually allows majority carriers to pass through and prevents minority carriers from passing through. The passivation contact structure formed by the tunneling oxide layer 21 and the doping layer 22 can block the transmission of minority carriers and selectively allow majority carriers to pass through, effectively reducing surface recombination and reducing the impact of surface recombination on the efficiency of solar cells.
[0040] In the embodiment of the present application, along the thickness direction of the silicon substrate 10, the thickness of the tunneling oxide layer 21 on the end face 13 is the first thickness; along the direction away from the side face 14, the thickness of the tunneling oxide layer 21 on the side face 14 is the second thickness; the first thickness is less than the second thickness; that is, a thicker tunneling oxide layer 21 is set on the side face 14 with more defects to reduce the interface state density and improve the passivation effect. The solar cell of the embodiment of the present application comprehensively sets the tunneling oxide layer 21 of the corresponding thickness according to the defects of the side face 14 and the end face 13 in the texture structure 12, reduces the surface recombination of the texture structure 12, achieves a better passivation effect, balances the carrier collection effect, and improves the efficiency and electrochemical performance of the solar cell.
[0041] Optionally, in one embodiment, referring to Figure 2 As shown, the end face 13 and the side face 14 form a raised tower base. The raised tower base can reduce light reflection and increase light absorption, thereby improving the efficiency of the solar cell.
[0042] At this time, the end face 13 is the highest surface in the texture structure 12 , the end face 13 is higher than the side face 14 , the end face 13 is a plane approximately parallel to the first surface 11 , the side face 14 intersects with the end face 13 , and there is an angle between the side face 14 and the first surface 11 .
[0043] Optionally, in another embodiment, referring to Figure 3 As shown, the end face 13 and the side face 14 form a concave tower base. In the above structure of the embodiment of the present application, the end face 13 is the lowest surface in the texture structure 12, the end face 13 is lower than the side face 14, the end face 13 is a plane approximately parallel to the first surface 11, and there is an angle between the side face 14 and the first surface 11. The concave tower base can be used as a light trapping structure to increase the internal reflection of light, thereby improving the absorption of light.
[0044] Optionally, the ratio of the second thickness to the first thickness is W, 1<W≤4. When the ratio of the second thickness to the first thickness is within the above range, the tunneling ability of the tunneling oxide layer and the defect conditions of the side surface 14 and the end surface 13 in the comprehensive texture structure 12 can be taken into account at the same time, the surface recombination of the texture structure 12 is reduced, the carrier collection rate is balanced, and a better passivation effect is achieved.
[0045] The embodiment of the present application does not specifically limit the ratio of the second thickness to the first thickness, as long as it meets the usage requirements. For example, the ratio W of the second thickness to the first thickness is at least one of 1.1, 1.3, 1.5, 1.7, 1.9, 2.1, 2.5, 3, 3.2, 3.4, 3.5, 3.8, and 4.
[0046] Optionally, the first thickness is greater than 0.1nm. In the embodiment of the present application, when the first thickness is within the above range, the tunnel oxide layer 21 can reduce the influence of the surface recombination on the end face 13 and achieve a better passivation effect. It can be understood that the embodiment of the present application does not specifically limit the first thickness, and it only needs to meet the use requirements. For example, the first thickness is at least one of 0.1nm, 0.2nm, 0.3nm, 0.4nm, 0.5nm, 0.6nm, 0.7nm, 0.8nm, 0.9nm, 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, and 2nm.
[0047] Optionally, the first thickness ranges from 0.5nm to 1.5nm. When the first thickness is within the above range, the tunneling oxide layer 21 has good tunneling capability while reducing the influence of surface recombination on the end face 13 and achieving a better passivation effect, thereby achieving efficient charge carrier separation and transmission. It is understandable that the first thickness is not specifically limited in the embodiment of the present application. For example, the first thickness is at least one of 0.5nm, 0.55nm, 0.6nm, 0.65nm, 0.7nm, 0.75nm, 0.8nm, 0.85nm, 0.9nm, 0.95nm, 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, and 1.5nm.
[0048] Optionally, the second thickness is greater than 0.3nm. In the embodiment of the present application, when the second thickness is within the above range, the tunneling oxide layer 21 can reduce the influence of the surface recombination on the side 14, reduce the interface state density, and achieve a better passivation effect. It can be understood that the embodiment of the present application does not specifically limit the second thickness, and it is sufficient to meet the use requirements. For example, the second thickness is at least one of 0.3nm, 0.4nm, 0.5nm, 0.6nm, 0.7nm, 0.8nm, 0.9nm, 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, and 2.5nm.
[0049] Optionally, the second thickness ranges from 0.5nm to 2nm. When the second thickness in the embodiment of the present application is within the above range, the tunneling oxide layer 21 has good tunneling ability while reducing the influence of the surface recombination on the side 14 and achieving a better passivation effect, thereby achieving efficient charge carrier separation and transmission. It is understandable that the embodiment of the present application does not specifically limit the second thickness. For example, the second thickness is at least one of 0.5nm, 0.6nm, 0.7nm, 0.8nm, 0.9nm, 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, and 2nm.
[0050] Optionally, the density of the tunnel oxide layer 21 on the end surface 13 is smaller than the density of the tunnel oxide layer 21 on the side surface 14 .
[0051] The compactness refers to the number of pores in the tunnel oxide layer 21 and whether these pores can be effectively filled. In the embodiment of the present application, the compactness of the tunnel oxide layer 21 on the side 14 is relatively large, which can better reduce surface recombination and provide better interface passivation effect, thereby improving the efficiency and electrochemical performance of the solar cell.
[0052] Optionally, the texture structure 12 includes a raised tower base 16, and the raised tower base 16 includes at least two tower-shaped protrusions stacked in sequence to form a pyramid shape, and the tower-shaped protrusion closest to the silicon substrate 10 is connected to the first surface 11. Figure 4 , which shows a schematic diagram of a structure in which a tower base 16 is two tower-shaped protrusions stacked in sequence to form a pyramid shape, the pyramid shape has three end faces 13, and the left and right sides of the pyramid shape are side faces 14, and the side faces 14 are in a stepped structure.
[0053] The functions of the tower base 16 include reducing the reflection loss of light, increasing the diffuse reflection of light on the silicon surface, thereby improving the light absorption rate, and providing support. The tower base 16 can improve the performance and efficiency of solar cells.
[0054] Optionally, along the thickness direction of the silicon substrate 10 , the height range from the end surface 13 to the first surface 11 is 1 um-10 um.
[0055] Further references Figure 1As shown, it shows a schematic diagram of the structure of the height H from the end face 13 to the first surface 11. When the height H of the end face 13 is within the above range along the thickness direction of the silicon substrate 10, the texture structure 12 can better change the microstructure of the first surface 11 to reduce the reflection of light, increase the diffusion and absorption of light inside the solar cell, and thus improve the photoelectric conversion efficiency. It can be understood that the embodiment of the present application does not specifically limit the height H from the end face 13 to the first surface 11. For example, H is at least one of 1um, 2um, 3um, 4um, 5um, 6um, 7um, 8um, 9um, and 10um.
[0056] Optionally, along the thickness direction of the silicon substrate 10 , the height range from the end surface 13 to the first surface 11 is 1 um-2 um.
[0057] In the embodiment of the present application, when the height H from the end face 13 to the first surface 11 is within the above range, the texture structure 12 further changes the microstructure of the first surface 11 to reduce the reflection of light, increase the diffusion and absorption of light inside the solar cell, further improve the photoelectric conversion efficiency, and also help to reduce the recombination center and enhance the passivation effect. It is understandable that the embodiment of the present application does not specifically limit the height H from the end face 13 to the first surface 11. For example, H is at least one of 1um, 1.1um, 1.2um, 1.3um, 1.4um, 1.5um, 1.6um, 1.7um, 1.8um, 1.9um, and 2um.
[0058] Optionally, in a top-down perspective, the width range of the tower base 16 is 5um-80um. And when the width of the tower base 16 is within the above range, the microstructure of the first surface 11 can be preferably changed to reduce the reflection of light, increase the diffusion and absorption of light inside the solar cell, thereby improving the photoelectric conversion efficiency. It is understandable that the embodiment of the present application does not specifically limit the width range of the tower base 16. For example, the width of the tower base 16 is at least one of 5um, 10um, 15um, 20um, 25um, 30um, 35um, 40um, 45um, 50um, 55um, 60um, 65um, 70um, 75um, and 80um.
[0059] The width of the tower base 16 refers to the width of the tower base 16 in a cross section perpendicular to the extension direction of the tower base 16 in a top-down perspective. The top-down perspective refers to the perspective of looking down at the solar cell from a high place.
[0060] Optionally, in a top-down perspective, the width range of the tower base 16 is 10um-30um. When the width of the tower base 16 is within the above range, the microstructure of the first surface 11 can be further changed to reduce the reflection of light, increase the diffusion and absorption of light inside the solar cell, thereby improving the photoelectric conversion efficiency, and also helping to reduce the recombination center and enhance the passivation effect. It is understandable that the present application embodiment does not specifically limit the width range of the tower base 16. For example, the width of the tower base 16 is at least one of 10um, 12um, 14um, 16um, 18um, 20um, 22um, 24um, 25um, 26um, 28um, and 30um.
[0061] Optionally, the thickness of the doping layer 22 is in the range of 50nm-300nm along the thickness direction of the silicon substrate 10. The doping layer 22 is disposed on the surface of the tunneling oxide layer 21 away from the silicon substrate 10. When the thickness of the doping layer 22 is in the above range, the photogenerated charges can be effectively collected and transmitted.
[0062] It will be appreciated that the embodiments of the present application do not limit the specific thickness of the doping layer 22. For example, the thickness of the doping layer 22 is at least one of 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 175 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, and 300 nm.
[0063] Optionally, along the thickness direction of the silicon substrate 10, the thickness range of the doping layer 22 is 80nm-180nm. When the thickness of the doping layer 22 is within the above range, the doping layer 22 can effectively collect and transmit photogenerated charges. The embodiment of the present application does not limit the specific thickness of the doping layer 22. For example, the thickness of the doping layer 22 is at least one of 80nm, 85nm, 90nm, 95nm, 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 145nm, 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, and 180nm.
[0064] Optional, see Figure 1 As shown, along the thickness direction of the silicon substrate 10 (the thickness direction of the silicon substrate 10 refers to Figure 1 The thickness of the tunnel oxide layer 21 on the surface of the first surface 11 except the tower base 16 is a third thickness, and the third thickness is less than the second thickness.
[0065] The inventors found in the study that the side 14 of the texture structure 12 has more defects, which increases the surface recombination and reduces the tunneling ability of the texture structure as a whole. Along the direction away from the side 14, the thickness of the tunneling oxide layer 21 on the side 14 is the second thickness; along the thickness direction of the silicon substrate 10, the thickness of the tunneling oxide layer 21 on the surface of the first surface 11 except the tower base 16 is the third thickness; the second thickness is greater than the third thickness, that is, a thicker tunneling oxide layer 21 is set on the side 14 with more defects to reduce the interface state density, enhance tunneling, and improve the passivation effect, while ensuring good carrier collection and improving the efficiency and electrochemical performance of the solar cell.
[0066] Optional, see Figures 8 to 12 As shown, the doping layer 22 is the first doping layer 23, and the solar cell also includes a second passivation layer 27 and a second doping layer 25; the first surface 11 is respectively provided with a tunneling oxide layer 21 and a second passivation layer 27, the tunneling oxide layer 21 and the second passivation layer 27 are arranged at intervals, the surface of the tunneling oxide layer 21 facing away from the silicon substrate 10 is connected to the first doping layer 23, and the surface of the second passivation layer 27 facing away from the silicon substrate 10 is connected to the second doping layer 25.
[0067] At this time, the doping layer 22 and the first doping layer 23, and the second passivation layer 27 and the second doping layer 25 are all located on the same surface of the silicon substrate 10. The solar cell may be a back contact cell.
[0068] The interval between the tunnel oxide layer 21 and the second passivation layer 27 is set as follows: in the plane extension direction of the silicon substrate 10, Fig.12 In the direction of the middle arrow B, the tunnel oxide layer 21 and the second passivation layer 27 are alternately arranged on the first surface 11 , and the two are in contact or non-contact in the plane extension direction of the silicon substrate 10 .
[0069] Optionally, the doping type of the first doping layer 23 is opposite to the doping type of the second doping layer 25. One of the first doping layer 23 and the second doping layer 25 is an N-type doping layer, and the other of the first doping layer 23 and the second doping layer 25 is a P-type doping layer.
[0070] The types of the first doping layer 23 and the second doping layer 25 are set according to the use requirements. For the N-type doping layer, the doping element is at least one of nitrogen, phosphorus, arsenic, antimony, etc. For the P-type doping layer, the doping element includes at least one of boron, aluminum, gallium, indium, etc. The N-type doping layer is an electron transport layer, and the P-type doping layer is a hole transport layer.
[0071] Optional, see Figures 5 to 7As shown, the solar cell further includes a third doping layer 31, a third passivation layer 28 and a third anti-reflection layer 29; along the thickness direction of the silicon substrate 10, the third doping layer 31, the third passivation layer 28 and the third anti-reflection layer 29 are provided on the second surface 15 of the silicon substrate 10 away from the first surface 11, and the third doping layer 31 is connected to the second surface 15. At this time, the tunneling oxide layer 21 is provided on the first surface 11, and the surface of the tunneling oxide layer 21 away from the silicon substrate 10 is connected to the doping layer 22.
[0072] At this time, the third doping layer 31 , the third passivation layer 28 , the third anti-reflection layer 29 , the tunneling oxide layer 21 , and the doping layer 22 are respectively located on two opposite surfaces of the silicon substrate 10 .
[0073] Optionally, one of the doped layer 22 and the third anti-reflection layer 29 is an N-type doped layer, and the other of the doped layer 22 and the third anti-reflection layer 29 is a P-type doped layer. The N-type doped layer is an electron transport layer, and the P-type doped layer is a hole transport layer.
[0074] In the solar cell of the embodiment of the present application, when the doping layer 22 is a doped polysilicon layer, the passivation contact structure formed by the tunneling oxide layer 21 and the doped polysilicon layer can block the transmission of minority carriers and selectively allow majority carriers to pass through, thereby effectively reducing surface recombination.
[0075] Solar cells are cells that include a passivated contact structure, for example, topcon, back contact cell, hybrid cell, tandem cell, bifacial cell, and the like.
[0076] Along the thickness direction of the silicon substrate 10, the thickness of the tunneling oxide layer 21 on the end face 13 is a first thickness; along the direction away from the side face 14, the thickness of the tunneling oxide layer 21 on the side face 14 is a second thickness; the first thickness is less than the second thickness; that is, a thicker tunneling oxide layer 21 is set on the side face 14 with more defects, and a thinner tunneling oxide layer 21 is set on the end face 13. Providing a thicker tunneling oxide layer on the side face 14 with more defects can reduce the interface state density and improve the passivation effect. In the solar cell comprehensive texture structure of the embodiment of the present application, a tunneling oxide layer of corresponding thickness is set according to the defect conditions of the side face 14 and the end face 13, which reduces the surface recombination of the texture structure, achieves a better passivation effect, and balances the carrier collection rate, thereby improving the efficiency and electrochemical performance of the solar cell.
[0077] The invention also provides a photovoltaic module, which includes a cover plate, a back plate, and a solar cell arranged between the cover plate and the back plate; the solar cell includes the solar cell as described above.
[0078] The embodiments of the present application do not specifically limit whether the photovoltaic module includes other structures. For example, the photovoltaic module may also include: a first packaging film disposed between the cover plate and the solar cell, and a second packaging film disposed between the back plate and the solar cell.
[0079] In the solar cell of the photovoltaic module of the embodiment of the present application, a tunneling oxide layer 21 of corresponding thickness is set according to the degree of defects on the side surface 14 and the end surface 13 of the texture structure 12, thereby reducing the surface recombination of the texture structure 12, achieving a better passivation effect, and improving the efficiency and electrochemical performance of the solar cell.
[0080] The present invention is further described in detail below with reference to specific embodiments.
[0081] Embodiment 1
[0082] The preparation process of solar cells, refer to Figures 8 to 12 As shown, the preparation process includes the following steps:
[0083] 101 , polishing and cleaning the silicon substrate 10 .
[0084] In this step, the silicon substrate 10 is polished and cleaned by a wet polishing scheme, which mainly includes two steps of cleaning and alkaline polishing.
[0085] The cleaning steps are: use SC1 (using a mixture of ammonium hydroxide and hydrogen peroxide solution, mainly used to remove organic matter and particles) in the RCA cleaning process (RCA standard cleaning method) for cleaning, and then use deionized water to neutralize the residual chemicals in the SC1 cleaning.
[0086] The alkaline polishing step is: use KOH (potassium hydroxide) to remove the surface damage layer of the silicon substrate 10 caused by cutting, and the surface of the silicon substrate 10 is polished. Then, high-efficiency SC1 cleaning is performed. Then SC2 (acidic solution, mainly composed of a mixture of hydrofluoric acid, hydrogen peroxide and water) is used to remove the residual metal ions. Finally, after 5% wt (weight) hydrofluoric acid cleaning, the surface of the silicon substrate 10 is polished. The polishing thickness range of the front and back of the silicon substrate 10 is 5μm-10μm, and the polished silicon substrate 10 forms the morphology of the texture structure 12.
[0087] The silicon substrate 10 in this step is an N-type silicon substrate.
[0088] 102 , forming a tunneling oxide layer 21 and a first doping layer 23 on the first surface 11 of the silicon substrate 10 .
[0089] In this step, in the LPCVD equipment, the temperature range is set to 540°C-580°C, oxygen is introduced as the oxygen source, the process time is 10 minutes, and SiO2 (silicon oxide) is prepared by thermal oxidation; the oxygen in the chamber of the LPCVD equipment is evacuated, the temperature is continued to be raised to 600°C, silane is introduced, the process time is 10 minutes, and polysilicon is deposited; and then the first doping layer 23 is formed by phosphorus diffusion.
[0090] The SiO2 obtained by controlling the above process parameters forms SiO2 of different thicknesses on the end face and side face of the texture structure of the first surface 11, and a thinner tunneling oxide layer 21 is deposited on the end face 13, and a thicker tunneling oxide layer 21 is deposited on the side face 14, which can effectively reduce the surface recombination of the side face 14, thereby improving the passivation effect. TEM test data such as Fig.13 and Fig.14 , Fig.13 A test diagram showing a tunnel oxide layer 21 deposited on the side 14 is shown. Fig.14 The test diagram of the end face 13 depositing the tunnel oxide layer 21 is shown. Fig.13 and Fig.14 It can be seen that a thicker tunnel oxide layer 21 is deposited on the side surface 14 relative to the end surface 13 , which is beneficial to passivating defects on the side surface, reducing defect state density, and improving the passivation effect.
[0091] The first doping layer 23 in this step is an N-type doping layer.
[0092] 103, such as Figure 8 As shown, a first passivation layer 24 and a first anti-reflection layer 26 are formed on the second surface 15 of the silicon substrate 10 .
[0093] In this step, a CVD device may be used to deposit the first passivation layer 24 on the second surface 15 of the silicon substrate 10 , and a first anti-reflection layer 26 may be deposited on the surface of the first passivation layer 24 facing away from the silicon substrate 10 .
[0094] 104, such as Fig. 9 As shown, a portion of the tunnel oxide layer 21 and the first doping layer 23 are etched away to form a first opening 52 .
[0095] In this step, a portion of the tunnel oxide layer 21 and the first doping layer 23 are etched away to form a first opening 52 , and the first opening 52 is used for depositing the second passivation layer 27 and the second doping layer 25 .
[0096] 105, such as Fig.10 As shown, a second passivation layer 27 and a second doping layer 25 are formed on the first surface 11 of the silicon substrate 10 .
[0097] In this step, a second passivation layer 27 and a second doping layer 25 are formed on the entire first surface 11 of the silicon substrate 10 . The second passivation layer 27 is connected between the first surface 11 and the second doping layer 25 .
[0098] The second doping layer 25 in this step is a P-type doping layer.
[0099] 106, such as Fig.11 As shown, a transparent conductive layer 51 is deposited on the side of the silicon substrate 10 where the first surface 11 is provided.
[0100] In this step, a transparent conductive layer 51 is deposited entirely on the side of the silicon substrate 10 where the first surface 11 is provided.
[0101] The transparent conductive layer 51 (TCO, Transparent Conductive Oxide) has good transparency and conductivity. The transparent conductive layer 51 directly faces the sunlight, and the main function of the transparent conductive layer 51 is to laterally transmit carriers.
[0102] 107, such as Fig.12 As shown, at least a portion of the transparent conductive layer 51 is removed to form a second opening 53 .
[0103] In this step, a portion of the transparent conductive layer 51 between the P region and the N region is removed to form a second opening 53. The second opening 53 completely insulates the P region and the N region and has the advantages of good insulation reliability and insulation effect.
[0104] 108, such as Fig.12 As shown, a first electrode 41 is prepared on the transparent conductive layer 51 corresponding to the N region, and a second electrode 42 is prepared on the transparent conductive layer 51 corresponding to the P region.
[0105] The first electrode 41 and the second electrode 42 are both metal electrodes. For example, the materials of the first electrode 41 and the second electrode 42 are metal materials such as silver and copper.
[0106] Embodiment 2
[0107] The preparation process of solar cells, refer to Figures 5 to 8 As shown, the preparation process includes the following steps:
[0108] 201 , polishing and cleaning the silicon substrate 10 .
[0109] Referring to the above step 101, this embodiment will not elaborate on it any more.
[0110] 202 , forming a tunneling oxide layer 21 and a doping layer 22 on the first surface 11 of the silicon substrate 10 .
[0111] In this step, in the LPCVD equipment, the temperature range is set to 540°C-580°C, oxygen is introduced as the oxygen source, the process time is 10 minutes, and SiO2 (silicon oxide) is prepared by thermal oxidation; the oxygen in the chamber of the LPCVD equipment is evacuated, the temperature is continued to be raised to 600°C, silane is introduced, the process time is 10 minutes, and polysilicon is deposited; and then a doping layer 22 is formed by phosphorus diffusion.
[0112] 203, such as Figure 5 As shown, a third doping layer 31 , a third passivation layer 28 and a third anti-reflection layer 29 are formed on the second surface 15 of the silicon substrate 10 .
[0113] In this step, a CVD device can be used to deposit a third doped layer 31 on the second surface 15 of the silicon substrate 10, a third passivation layer 28 is deposited on the surface of the third doped layer 31 facing away from the silicon substrate 10, and a third anti-reflection layer 29 is deposited on the surface of the third passivation layer 28 facing away from the silicon substrate 10.
[0114] 204, such as Figure 6 As shown, a second anti-reflection layer 30 is formed on the first surface 11 of the silicon substrate 10 .
[0115] In this step, a second anti-reflection layer 30 is formed on the entire first surface 11 of the silicon substrate 10 . The second anti-reflection layer 30 is connected to the surface of the doping layer 22 facing away from the silicon substrate 10 .
[0116] 205, such as Figure 7 As shown, a first electrode 41 is fabricated on the second anti-reflection layer 30 , and a second electrode 42 is fabricated on the third anti-reflection layer 29 .
[0117] The first electrode 41 and the second electrode 42 are both metal electrodes. For example, the materials of the first electrode 41 and the second electrode 42 both include silver.
[0118] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0119] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. For the embodiments of the device, electronic device, computer-readable storage medium and computer program products containing instructions, since they are basically similar to the method embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiments.
[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A solar cell, characterized in that: The solar cell comprises a silicon substrate (10), a tunneling oxide layer (21) and a doping layer (22) which are stacked in sequence; A surface of the silicon substrate (10) close to the tunnel oxide layer (21) is a first surface (11); along the thickness direction of the silicon substrate (10), the silicon substrate (10) is provided with at least one first surface (11); the first surface (11) is provided with a texture structure (12); the texture structure (12) comprises an end surface (13) and a side surface (14) arranged in the thickness direction of the silicon substrate (10); Along the thickness direction of the silicon substrate (10), the thickness of the tunneling oxide layer (21) on the end face (13) is a first thickness; along the direction away from the side face (14), the thickness of the tunneling oxide layer (21) on the side face (14) is a second thickness; and the first thickness is less than the second thickness.
2. The solar cell according to claim 1, characterized in that A ratio of the second thickness to the first thickness is W, 1<W≤4.
3. The solar cell according to claim 1 or 2, characterized in that: The first thickness is greater than or equal to 0.1 nm; preferably, the first thickness is in the range of 0.5 nm-1.5 nm.
4. The solar cell according to claim 1 or 2, characterized in that: The second thickness is greater than or equal to 0.3 nm; preferably, the second thickness is in the range of 0.5 nm-2 nm.
5. The solar cell according to claim 1, characterized in that: The compactness of the tunneling oxide layer (21) on the end surface (13) is smaller than the compactness of the tunneling oxide layer (21) on the side surface (14).
6. The solar cell according to claim 1, characterized in that Along the thickness direction of the silicon substrate (10), the height range from the end face (13) to the first surface (11) is 1um-10um; preferably, the height range from the end face (13) to the first surface (11) is 1um-2um.
7. The solar cell according to claim 1, characterized in that The end surface (13) and the side surface (14) form a tower base, and the tower base protrudes from the first surface (11), or the tower base is recessed in the first surface (11).
8. The solar cell according to claim 7, characterized in that: The tower base (16) protruding from the first surface (11) comprises at least two tower-shaped protrusions stacked in sequence in a pyramid shape.
9. The solar cell according to claim 7, characterized in that: In a top view, the width of the tower base (16) ranges from 5um to 80um; preferably, the width of the tower base (16) ranges from 10um to 30um.
10. The solar cell according to claim 7, characterized in that: Along the thickness direction of the silicon substrate (10), the thickness of the tunnel oxide layer (21) on the surface of the first surface (11) other than the tower base (16) is a third thickness, and the third thickness is less than the second thickness.
11. The solar cell according to claim 1, characterized in that: Along the thickness direction of the silicon substrate (10), the thickness of the doping layer (22) ranges from 50 nm to 300 nm; preferably, the thickness of the doping layer (22) ranges from 80 nm to 180 nm.
12. The solar cell according to claim 1, characterized in that The doping layer (22) is a first doping layer (23), and the solar cell further comprises a second passivation layer (27) and a second doping layer (25); The first surface (11) is provided with the tunneling oxide layer (21) and the second passivation layer (27), respectively; the tunneling oxide layer (21) and the second passivation layer (27) are arranged at an interval; the surface of the tunneling oxide layer (21) facing away from the silicon substrate (10) is connected to the first doped layer (23); and the surface of the second passivation layer (27) facing away from the silicon substrate (10) is connected to the second doped layer (25).
13. The solar cell according to claim 12, characterized in that: The doping type of the first doping layer (23) is opposite to the doping type of the second doping layer (25).
14. A photovoltaic module, characterized in that: The photovoltaic assembly includes a cover plate, a back plate, and a solar cell according to any one of claims 1 to 13 disposed between the cover plate and the back plate.
Citation Information
Patent Citations
Back junction solar cell with tunnel oxide
CN105845769A
Solar cell, formation method thereof and photovoltaic module
CN115732576A
Solar cell and photovoltaic module
CN116093191A
Preparation method of solar cell, solar cell and photovoltaic module
CN118352430A
Solar cell, method for manufacturing the same, and photovoltaic module
EP4297104A2