Long-life high-voltage-resistant photoconductive switch and manufacturing method thereof

By adopting snap-on electrode structure and sandblasting treatment in the photoconductive switch, the voltage withstand and life problems of the photoconductive switch under the strong field are solved, and the electric field uniformity and photogenerated carrier uniformity are improved, which significantly increases the voltage and life of the photoconductive switch. Improves the device's withstand voltage and life.

CN119092559APending Publication Date: 2024-12-06XIAN UNIV OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411188316.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing photoconductive switches are prone to flashover or breakdown along the surface under strong fields, resulting in a decrease in voltage and life. Existing improved methods such as complex threaded through-hole structures and lack of illumination cross-section homogenization, making it difficult to effectively improve the device. Pressure withstand and life.

Method used

Two alloy electrodes are arranged on the semiconductor substrate. Each electrode has a block-shaped external metal electrode on the surface and is connected by a copper strip, combined with sandblasting and grinding to form a snap-on electrode unit. The cross-section of the external metal electrode is smooth. Chamfered or arc-shaped, bonded with conductive silver glue, and insulated to improve electric field uniformity and photogenerated carrier uniformity.

Benefits of technology

It significantly improves the voltage withstandability and service life of the photoconductive switch, reduces leakage current caused by surface and cutting surface defects, enhances the degree of light homogenization on the light irradiation cross-section, simplifies the process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092559A_ABST
    Figure CN119092559A_ABST
Patent Text Reader

Abstract

The invention discloses a long-life high-voltage-resistant photoconductive switch which comprises a semiconductor substrate, two alloy electrodes are arranged on each of the upper surface and the lower surface of the semiconductor substrate, and a blocky external metal electrode is further arranged on the surface of each alloy electrode; the two external metal electrodes located at the same end of the semiconductor substrate are connected through a copper strip. The surface of the whole body of the semiconductor substrate is subjected to sand blasting and polishing treatment except the alloy electrode covering part, and the whole body of the long-service-life high-voltage-resistance photoconductive switch is packaged. Due to the uniformity of an electric field in the semiconductor substrate and the uniformity of photon-generated carriers, the service life of the photoconductive switch is prolonged. The invention further discloses a manufacturing method of the long-service-life high-voltage-resistance photoconductive switch.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of pulse power technology, and in particular relates to a long-life high-voltage photoconductive switch, and also relates to a method for manufacturing the long-life high-voltage photoconductive switch. Background Art

[0002] As a power switch device combining ultrafast light pulses with optoelectronic semiconductors (MΩ or even GΩ dark state resistance), photoconductive switches have the advantages of ultrafast response, high voltage resistance, fast rising edge, narrow pulse, low trigger jitter, low inductance and long life, small size, solid-state and easy integration compared to traditional power switches. In high-multiplication mode, photoconductive switches can generate 10 3 -10 5 The output power is increased by 3-5 orders of magnitude compared to the linear mode. This makes it possible to achieve miniaturization and integration of ultra-high power microwave systems, ultra-fast electronic systems, and high-power ultra-short pulses with the help of high repetition rate, high-power photoconductive switches and arrays. The output power of the photoconductive switch has a positive excitation relationship with the switch bias, so improving the voltage resistance and working life of the photoconductive switch is the key to improving the performance of the pulse power system.

[0003] However, previous experiments have found that photoconductive switches will experience surface flashover or breakdown under strong fields, and different degrees of ablation will occur at the gold-semiconductor contact and on the chip, which will damage the withstand voltage and life of the switch device. Studies have shown that this device damage is closely related to local surface defects introduced by the growth and processing of the semiconductor substrate, uneven light intensity in the illumination section, and the ohmic contact of the photoconductive switch electrode. Conventional photoconductive switches are composed of a pair of ohmic electrodes and a semi-insulating photoelectric semiconductor substrate. Depending on the position of the ohmic electrode on the semiconductor substrate, photoconductive switches are divided into coplanar structure, skew structure and bulk structure. The electrodes are mostly planar sheet structures, and there are a large number of metal tips or semiconductor lattice defects on the electrodes and the semiconductor substrate. Under bias, these metal tips absorb charges and participate in the superposition of the spatial electric field, making the electric field in the semiconductor substrate area between the two electrodes non-uniformly distributed, and forming electric field maxima at the triple point where the ohmic electrode, semiconductor substrate and environmental medium contact and at the semiconductor surface defects. When illuminated, the lattice defects on the surface of the semiconductor substrate form random space charge regions due to the capture of photogenerated carriers, and form localized accumulation of carriers in the non-uniform electric field. Under the action of the external electric field, the local strong carrier movement produces a high-concentration conductive channel and releases Joule heat. The damage to the photoconductive switch will begin to accumulate from these conductive channels and further lead to the occurrence of switch breakdown. Therefore, improving the processing technology, enhancing the homogenization of the electric field and the homogenization of the triggering light are effective methods to improve the withstand voltage and life of the photoconductive switch. In existing research, related work has been carried out to achieve electric field homogenization through electrode morphology optimization.

[0004] In the patent "202011433128.9, an outer conductor electrode structure for homogenizing the electric field of a planar photoconductive switch, a photoconductive switch device and a method" applied by Xi'an Jiaotong University, an arc-shaped chamfered structure is introduced to the external electrode, which alleviates the electric field strength distortion at the edge of the device electrode to a certain extent. However, the non-uniformity of the electric field in the semiconductor substrate cannot be ignored.

[0005] The application number of the National University of Defense Technology of the People's Liberation Army of China is 202310742332.6 "An outer conductor electrode structure for homogenizing the electric field of a planar photoconductive switch, a photoconductive switch device and a method", which discloses a method for connecting a chamfered planar electrode to an external photoconductive switch using a threaded through hole. The first external electrode structure and the first ohmic electrode are aligned, the conductive silver glue is coated, solidified, the second external electrode structure is installed and the insulating medium is potted, which can effectively avoid the concentration of metal tips at the edge of the ohmic electrode, the substrate and the insulating medium triple point, and play a role in homogenizing the electric field distribution at the edge of the ohmic electrode. However, the processing technology is relatively complex and difficult to implement, and there is a lack of spot homogenization of the incident light in the illumination section on the semiconductor substrate, which has limited ability to improve the withstand voltage and life of the photoconductive switch.

[0006] How to further improve the uniformity of the electric field in the semiconductor transport zone between electrodes by adjusting the electrode material, morphology and structure; and improve the uniformity and output characteristics of photogenerated carriers in photoconductive switches by improving lattice defects are issues that need to be urgently addressed in the field of photoconductive switch research.

[0007] Based on the analysis of background technical problems, it is found that the concentration of surface defects near the interface between the photoconductive switch substrate, metal electrode, semiconductor substrate and environmental medium is relatively high. Under strong field, these defects will be charged after adsorbing ionized charges, forming a non-uniform spatial electric field. Non-uniform illumination, device surface defects and internal non-uniform electric field distribution aggravate the local accumulation of charges, forming a non-uniform current channel and greatly increasing the local temperature. When the temperature is higher than the melting point of the electrode and the photoconductive switch substrate, it causes annealing of the electrode and ablation of the substrate, which damages the withstand voltage and service life of the photoconductive switch. Summary of the invention

[0008] The first object of the present invention is to provide a long-life and high-voltage photoconductive switch, the life of which is improved due to the uniformity of the electric field and the uniformity of photogenerated carriers inside the semiconductor substrate.

[0009] The second object of the present invention is to provide a method for manufacturing a long-life and high-voltage-resistant photoconductive switch, thereby preparing a long-life and high-voltage-resistant photoconductive switch to improve the uniformity of the electric field inside the semiconductor substrate and the uniformity of photogenerated carriers, thereby achieving the purpose of increasing the life of the photoconductive switch.

[0010] The first technical solution adopted by the present invention is a long-life and high-voltage-resistant photoconductive switch, including a semiconductor substrate, two alloy electrodes are arranged on the upper surface and the lower surface of the semiconductor substrate, and a block-shaped external metal electrode is also arranged on the surface of each alloy electrode; the two external metal electrodes located at the same end of the semiconductor substrate are connected by a copper strip; the entire surface of the semiconductor substrate is sandblasted and polished except for the alloy electrode covered part, and the long-life and high-voltage-resistant photoconductive switch is encapsulated throughout.

[0011] The present invention is also characterized in that:

[0012] The edge of the cross section of the external metal electrode is a smooth chamfer or the cross section of the external metal electrode is an arc shape.

[0013] The second technical solution adopted by the present invention is a method for manufacturing a long-life high-voltage photoconductive switch, comprising the following steps:

[0014] Step 1, cleaning the semiconductor substrate, and implanting oxygen ions into one surface of the semiconductor substrate;

[0015] Step 2, obtaining a bonding surface required for the alloy electrode on the surface of the semiconductor substrate processed in step 1;

[0016] Step 3, preparing an alloy electrode on the surface of the semiconductor substrate treated in step 2;

[0017] Step 4, pre-treating the surface of the semiconductor substrate into which oxygen ions are not implanted;

[0018] Step 5, preparing an alloy electrode on the surface of the semiconductor substrate treated in step 4;

[0019] Step 6, alloying the sample obtained in step 5;

[0020] Step 7: polishing the sample surface;

[0021] Step 8: Use conductive silver glue to bond the external metal electrode to the corresponding alloy electrode, and connect the two external metal electrodes arranged on the upper and lower surfaces of the same end of the semiconductor substrate through copper tape;

[0022] Step 9: encapsulate the sample obtained in step 8.

[0023] The present invention is also characterized in that:

[0024] In step 1, the oxygen ion implantation energy is 10keV-60keV, and the implantation concentration is 1×10 15 / cm 2 ;

[0025] Step 2 specifically comprises: cleaning the semiconductor substrate, applying photoresist on the surface of the semiconductor substrate where oxygen ions are implanted, and after pre-baking, exposure, development and post-baking, wet etching is performed to expose the surface of the semiconductor substrate on the bonding surface where the subsequent alloy electrode is located;

[0026] Step 3 is specifically as follows: cleaning the semiconductor substrate, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate injected with oxygen ions with thicknesses of 40A°, 50A°, 610A°, 75A°, 35A°, and 1900A°, respectively.

[0027] Step 4 specifically comprises: cleaning the semiconductor substrate, applying photoresist on the surface of the semiconductor substrate not implanted with oxygen ions, and after pre-baking, exposure, development and post-baking, wet etching is performed to expose the surface of the semiconductor substrate not implanted with oxygen ions;

[0028] Step 5 specifically comprises: cleaning the semiconductor substrate, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate where oxygen ions are not injected, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively;

[0029] Step 6 is specifically as follows: clean the semiconductor substrate, alloy it in an alloy furnace, heat it to 260°C-360°C, hold it for 25s, the surface of the semiconductor substrate injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate not injected with oxygen ions forms the cathode of the photoconductive switch.

[0030] Step 7 is specifically as follows: using quartz sand with a particle size of 0.05mm-1mm to sandblast the entire semiconductor substrate except for the alloy electrode bonding area, or using sandpaper with the same particle size to polish until the original polished surface is no longer visible.

[0031] The material of the semiconductor substrate is GaAs.

[0032] The alloy electrode is an Au / Ge / Ni alloy electrode.

[0033] The beneficial effects of the present invention are:

[0034] (1) The long-life and high-voltage photoconductive switch of the present invention has a longer life due to the uniformity of the electric field inside the semiconductor substrate and the uniformity of the photogenerated carriers.

[0035] (2) The method for manufacturing a long-life high-voltage photoconductive switch of the present invention improves the uniformity of the electric field in the photoconductive switch, reduces the leakage current caused by defects on the surface and cut surface of the photoconductive switch, and enhances the light homogenization degree on the light irradiation cross section, significantly improving the voltage resistance and service life of the photoconductive switch. The method of the present invention is simple and easy to implement, and can be widely applied to all current photoconductive switches, with the advantages of low cost, convenient operation, and strong voltage resistance improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the structure of the long-life high-voltage photoconductive switch of the present invention, wherein the cross section of the external metal electrode has a smooth chamfer;

[0037] Figure 2 It is a schematic structural diagram of a long-life high-voltage photoconductive switch of the present invention, wherein the cross section of the external metal electrode is an arc shape;

[0038] Figure 3 yes Figure 2 A top view of the long-life and high-voltage photoconductive switch of the present invention;

[0039] Figure 4 yes Figure 2 The electric field distribution around the external metal electrode photoconductive switch of the long-life high-voltage photoconductive switch;

[0040] Figure 5 yes Figure 2 The electric field distribution at the interface between the external metal electrode and the semiconductor substrate on the left side of the long-life high-voltage photoconductive switch;

[0041] Figure 6 yes Figure 2 The electric field distribution at the interface between the external metal electrode and the semiconductor substrate 2 in the middle right side of the long-life high-voltage photoconductive switch;

[0042] Figure 7 It is a schematic diagram of the structure of a photoconductive switch with a coplanar structure of a single-sided external metal electrode;

[0043] Figure 8 yes Figure 7 The electric field distribution around the photoconductive switch coplanar with the single-sided external metal electrode;

[0044] Fig. 9 yes Figure 7 The electric field distribution at the interface between the left external electrode and the semiconductor substrate 2 in the photoconductive switch in which the single-side external metal electrode is coplanar;

[0045] Fig.10 yes Figure 7 The electric field distribution at the interface between the right external electrode and the semiconductor substrate in a photoconductive switch with a single-side external metal electrode coplanar;

[0046] Fig.11 It is a schematic diagram of the photoconductive switch structure with coplanar Au / Ge / Ni alloy electrodes in the traditional planar;

[0047] Fig.12 yes Fig.11 Electric field distribution around a photoconductive switch with coplanar Au / Ge / Ni alloy electrodes;

[0048] Fig.13 yes Fig.11 The electric field distribution at the interface between the left Au / Ge / Ni alloy electrode and the semiconductor substrate in a conventional planar Au / Ge / Ni alloy electrode coplanar photoconductive switch;

[0049] Fig.14 yes Fig.11 The electric field distribution at the interface between the right Au / Ge / Ni alloy electrode and the semiconductor substrate in a conventional planar Au / Ge / Ni alloy electrode coplanar photoconductive switch;

[0050] Fig.15 It is a schematic diagram of the structure of the photoconductive switch with planar Au / Ge / Ni alloy electrodes on different surfaces;

[0051] Fig.16 yes Fig.15 Electric field distribution around the photoconductive switch with Au / Ge / Ni alloy electrodes on different planes;

[0052] Fig.17 yes Fig.15 The electric field distribution near the Au / Ge / Ni alloy electrode and the semiconductor substrate on the left side of the photoconductive switch of the structure;

[0053] Fig.18 yes Fig.15 Electric field distribution near the Au / Ge / Ni alloy electrode on the right side of the photoconductive switch and the semiconductor substrate.

[0054] In the figure, 1. external metal electrode, 2. semiconductor substrate, 3. alloy electrode, 4. copper tape. DETAILED DESCRIPTION

[0055] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0056] The present invention proposes a long-life high-voltage photoconductive switch, such as Figure 2 and Figure 3As shown, it includes a semiconductor substrate 2, two alloy electrodes 3 are arranged on the upper surface and the lower surface of the semiconductor substrate 2, and a block-shaped external metal electrode 1 is also arranged on the surface of each alloy electrode 3; the two external metal electrodes 1 located at the same end of the semiconductor substrate 2 are connected by a copper belt 4, and the two external metal electrodes 1 arranged on the upper and lower surface sides corresponding to each end of the semiconductor substrate 2 and the copper belt 4 between the two external metal electrodes 1 constitute a snap-on electrode unit; the entire surface of the semiconductor substrate 2 is sandblasted and polished except for the part covered by the alloy electrode 3, and the long-life high-voltage photoconductive switch is encapsulated throughout.

[0057] like Figure 1-2 As shown, the edge of the cross section of the external metal electrode 1 is a smooth chamfer or the cross section of the external metal electrode 1 is an arc. The external metal electrode 1 is a copper electrode. The material of the semiconductor substrate 2 is GaAs. The alloy electrode 3 is an Au / Ge / Ni alloy electrode.

[0058] Unlike the conventional photoconductive switch electrode design in which only one electrode is provided on one side in the coplanar electrodes and the non-planar electrodes, in the photoconductive switch proposed by the present invention, four electrodes are formed at both ends of the semiconductor substrate 2, and the two external metal electrodes 1 on the left are connected to the same potential, and the two external metal electrodes 1 on the right are connected to the same potential. When the photogenerated carriers reach the vicinity of the external metal electrode 1, they can be absorbed by the upper and lower two external metal electrodes 1 with the same potential, thereby greatly reducing the current density of the single electrode and alleviating the problem of electrode ablation caused by local overheating. The external metal electrode 1 not only forms a more uniform electric field inside the semiconductor substrate 2, but also homogenizes the electric field of the air layer adjacent to the semiconductor substrate 2 into a uniform electric field, greatly reducing the vertical component of the electric field at the interface, and avoiding the problem of flashover on the interface surface from the external electrode to the semiconductor substrate 2 that is prone to occur after the conventional external electrode is introduced.

[0059] The external metal electrode 1 in the snap-on electrode unit is bonded to the traditional ohmic electrode Au / Ge / Ni alloy electrode 3 through silver paste, and can also replace the traditional Au / Ge / Ni alloy electrode 3, and is directly connected to the semiconductor substrate 2 through silver paste to form an electrode, and then the upper and lower external metal electrodes 1 are tightly connected with a metal copper belt 4 to eliminate gas impurities between the electrodes, the semiconductor substrate and the copper belt; the semiconductor substrate 2 is sandblasted with quartz sand with a particle size of 0.05mm-1mm or polished with sandpaper of the same particle size to form rough protrusions of micrometer or even submillimeter order on the surface of the semiconductor substrate 2 to replace the traditional Si3N4 passivation process; the photoconductive switch is insulated and packaged with transparent epoxy resin or shadowless glue to improve the insulation level.

[0060] The purpose of sandblasting and grinding the semiconductor substrate 2 is to form micrometer-level uniform point-shaped protrusions. These uniform protrusions can achieve a light-homogenizing effect similar to that of frosted glass for the incident light, forming a relatively uniform laser speckle, so that the irradiated light that passes through the surface of the photoconductive switch and enters the interior of the device is homogenized again, promoting the uniform distribution of carriers in the switch body, and effectively alleviating the possibility of damage to the switch device caused by the local strong current density caused by the uneven charge distribution. At the same time, due to the change in the propagation direction, the absorption depth of the incident light is reduced, and the photogenerated carriers are more susceptible to those charged surface defects. The direction of the photogenerated carrier flow changes randomly continuously, realizing the homogenization of the photocurrent, and avoiding the formation of current filaments, greatly improving the service life of the photoconductive switch device.

[0061] The present invention also provides a method for manufacturing the above-mentioned long-life high-voltage photoconductive switch, and the specific steps are as follows:

[0062] Step 1: Clean the semiconductor substrate 2, and implant oxygen ions into one surface of the semiconductor substrate 2. The oxygen ion implantation energy is 10keV-60keV, and the implantation concentration is 1×10 15 / cm 2 ;

[0063] Step 2, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 where oxygen ions are injected, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 on the bonding surface where the subsequent alloy electrode 3 is located;

[0064] Step 3, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 injected with oxygen ions, with thicknesses of 40 Å, 50 Å, 610 Å, 75 Å, 35 Å, and 1900 Å, respectively;

[0065] Step 4, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 not implanted with oxygen ions, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 not implanted with oxygen ions;

[0066] Step 5, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 where oxygen ions are not injected, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively;

[0067] Step 6, clean the semiconductor substrate 2, alloy it in an alloy furnace, heat it to 260℃-360℃, hold it for 25s, the surface of the semiconductor substrate 2 injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate 2 not injected with oxygen ions forms the cathode of the photoconductive switch.

[0068] Step 7: Use quartz sand with a particle size of 0.05 mm to 1 mm to sandblast the entire semiconductor substrate 2 except for the bonding portion of the alloy electrode 3, or use sandpaper with the same particle size to polish until the original polished surface is no longer visible.

[0069] Step 8: Use conductive silver glue to bond the external metal electrode 1 to the corresponding alloy electrode 3, connect the two external metal electrodes 1 arranged on the upper and lower surfaces of the same end of the semiconductor substrate 2 through the copper tape 4, and the copper tape 4 tightly wraps the two external metal electrodes 1 to form a snap-on structure; the external metal electrode 1 is connected to the external circuit through a wire;

[0070] Step 9: Use transparent epoxy resin or shadowless adhesive to insulate and package the photoconductive switch and the entire electrode to improve the insulation level.

[0071] Example 1

[0072] Long life and high withstand voltage photoconductive switch, such as Figure 2 and Figure 3 As shown, it includes a semiconductor substrate 2, two alloy electrodes 3 are arranged on the upper surface and the lower surface of the semiconductor substrate 2, and a block-shaped external metal electrode 1 is also arranged on the surface of each alloy electrode 3; the two external metal electrodes 1 located at the same end of the semiconductor substrate 2 are connected by a copper belt 4, and the two external metal electrodes 1 arranged on the upper and lower surface sides corresponding to each end of the semiconductor substrate 2 and the copper belt 4 between the two external metal electrodes 1 constitute a snap-on electrode unit; the entire surface of the semiconductor substrate 2 is sandblasted and polished except for the part covered by the alloy electrode 3, and the long-life high-voltage photoconductive switch is encapsulated throughout.

[0073] like Figure 2 As shown, the cross section of the external metal electrode 1 is an arc shape. The external metal electrode 1 is a copper electrode. The material of the semiconductor substrate 2 is GaAs. The alloy electrode 3 is an Au / Ge / Ni alloy electrode.

[0074] like Figure 4-Figure 6 In the electric field simulation diagram shown, the solid lines near the semiconductor substrate 2 are equipotential lines, and the color depth reflects the strength of the electric field. Figure 4-Figure 6 It can be seen that the direction of the electric field in the semiconductor substrate 2 is parallel to the substrate plane. When the electrode gap is 45μm and the voltage is ±1kV, the electric field extreme value at the triple point is 160kV / cm, the uniform field strength inside the switch is 80kV / cm, and the electric field amplitude uniformity is good.

[0075] Comparative Example 1

[0076] The photoconductive switch with a coplanar structure of a single-sided external metal electrode has a structure such as Figure 7As shown, a semiconductor substrate 2 is included. Two alloy electrodes 3 are arranged on one side of the semiconductor substrate 2. An external metal electrode 1 is arranged on the upper surface of each alloy electrode 3.

[0077] Figure 7-Figure 10 The structure diagram of the photoconductive switch with a single-side external metal electrode 1 coplanar, the electric field distribution diagram around the photoconductive switch, the electric field distribution near the critical point between the left external metal electrode 1 and the semiconductor substrate 2, and the electric field distribution near the contact between the right external metal electrode 1 and the semiconductor substrate 2 are given. In the electric field simulation diagram, the solid lines near the semiconductor substrate 2 are equipotential lines, and the color depth represents the strength of the electric field. Figure 8-Figure 10 It can be seen that since the external metal electrode 1 is only on the same side of the semiconductor substrate 2, the equipotential surface is a curved surface around the contact point, and the direction of the electric field strength gradually differs greatly. When the electrode gap is 45μm, when the two electrodes are pressurized with ±1kV, the electric field extreme value at the triple point is 260kV / cm, and the internal uniform field strength is 70kV / cm. Figure 3 .d The electric field uniformity in the photoconductive switch semiconductor substrate 2 with a single-sided curved surface and a metal electrode 1 on the same plane is lower than Figure 6 The electric field condition of the photoconductive switch with external metal electrodes of the present invention.

[0078] Comparative Example 2

[0079] The conventional planar Au / Ge / Ni alloy electrode coplanar photoconductive switch has a structure such as Fig.11 As shown, it includes a semiconductor substrate 2, and two alloy electrodes 3 are arranged on one side of the semiconductor substrate 2;

[0080] Figure 11-Figure 14 The structural diagram of the photoconductive switch with a planar Au / Ge / Ni alloy electrode coplanar structure, the electric field distribution diagram around the photoconductive switch, the electric field distribution near the contact between the Au / Ge / Ni alloy electrode 3 and the semiconductor substrate 2, and the electric field distribution near the contact between the Au / Ge / Ni alloy electrode 3 and the semiconductor substrate 2 on the right are given respectively. In the electric field simulation diagram, the solid lines near the semiconductor substrate 2 are equipotential lines, and the color depth represents the strength of the electric field. Figure 12-14 It can be seen that the equipotential surface is a curved surface around the contact point, and the direction of the electric field strength varies greatly from point to point, with two components perpendicular to the semiconductor substrate. The direction of the electric field strength gradually differs below Figure 6 The electric field condition of the photoconductive switch with external metal electrodes of the present invention.

[0081] Comparative Example 3

[0082] The photoconductive switch with Au / Ge / Ni alloy electrodes on different surfaces has a structure such as Fig.15 As shown, it includes a semiconductor substrate 2, and an alloy electrode 3 is respectively arranged on two opposite sides of the semiconductor substrate 2;

[0083] Figure 15-18 The structure diagram of the photoconductive switch with the planar Au / Ge / Ni alloy electrode 3 in an out-of-plane structure, the electric field distribution diagram around the photoconductive switch, the electric field distribution near the contact between the left-side planar Au / Ge / Ni alloy electrode 3 and the semiconductor substrate 2, and the electric field distribution near the contact between the right-side planar Au / Ge / Ni alloy electrode 3 and the semiconductor substrate 2 are respectively given. In the electric field simulation diagram, the solid lines in the semiconductor substrate 2 are equipotential lines, and the color represents the magnitude of the electric field strength. It can be seen from the figure that the equipotential surface is a curved surface around the contact point, and the direction of the electric field strength varies greatly from point to point, and there is an electric field strength component perpendicular to the semiconductor substrate 2. Fig.18 The electric field uniformity in the semiconductor substrate of the traditional planar Au / Ge / Ni alloy electrode 3 is lower than Figure 6 The electric field condition of the photoconductive switch with external metal electrodes of the present invention.

[0084] It can be seen that the external metal electrode structure 1 proposed in the present invention can form a more uniform electric field distribution in and near the semiconductor substrate 2. In the photoconductive switch proposed in the present invention, four electrodes are formed at both ends of the semiconductor substrate 2, the two external metal electrodes 1 on the left are connected to the same potential, and the two external metal electrodes 1 on the right are connected to the same potential. When the photogenerated carriers reach the vicinity of the external metal electrode 1, they can be absorbed by the upper and lower external metal electrodes 1 with the same potential, thereby greatly reducing the current density of the single electrode and alleviating the problem of electrode ablation caused by local overheating. The external metal electrode 1 not only forms a more uniform electric field inside the semiconductor substrate 2, but also homogenizes the electric field of the air layer adjacent to the semiconductor substrate 2 into a uniform electric field, greatly reducing the vertical component of the electric field at the interface, and avoiding the problem of flashover on the interface surface from the external electrode to the semiconductor substrate 2 that is prone to occur after the introduction of conventional external electrodes. The semiconductor substrate 2 is sandblasted with quartz sand of 0.05mm-1mm particle size or polished with sandpaper of the same particle size to form rough protrusions of micrometer or even sub-millimeter magnitude on the surface of the semiconductor substrate 2 to replace the traditional Si3N4 passivation process; the voltage resistance and service life of the photoconductive switch are significantly improved; and the photoconductive switch is insulated and packaged with transparent epoxy resin or shadowless glue to improve the insulation level.

[0085] In Example 1 and Comparative Examples 1-3, the external metal electrode 1 is a copper electrode, the semiconductor substrate 2 is made of GaAs, and the alloy electrode 3 is an Au / Ge / Ni alloy electrode.

[0086] Example 2

[0087] Long life and high withstand voltage photoconductive switch, such as Figure 1As shown, it includes a semiconductor substrate 2, two alloy electrodes 3 are arranged on the upper surface and the lower surface of the semiconductor substrate 2, and a block-shaped external metal electrode 1 is also arranged on the surface of each alloy electrode 3; the two external metal electrodes 1 located at the same end of the semiconductor substrate 2 are connected by a copper belt 4, and the two external metal electrodes 1 arranged on the upper and lower surface sides corresponding to each end of the semiconductor substrate 2 and the copper belt 4 between the two external metal electrodes 1 constitute a snap-on electrode unit; the entire surface of the semiconductor substrate 2 is sandblasted and polished except for the part covered by the alloy electrode 3, and the long-life high-voltage photoconductive switch is encapsulated throughout. The edge of the cross section of the external metal electrode 1 is a smooth chamfer.

[0088] The method for making a long-life high-voltage photoconductive switch has the following specific steps:

[0089] Step 1: Clean the semiconductor substrate 2, and implant oxygen ions into one surface of the semiconductor substrate 2. The oxygen ion implantation energy is 10 keV and the implantation concentration is 1×10 15 / cm 2 ;

[0090] Step 2, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 where oxygen ions are injected, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 on the bonding surface where the subsequent alloy electrode 3 is located;

[0091] Step 3, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 injected with oxygen ions, with thicknesses of 40 Å, 50 Å, 610 Å, 75 Å, 35 Å, and 1900 Å, respectively;

[0092] Step 4, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 not implanted with oxygen ions, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 not implanted with oxygen ions;

[0093] Step 5, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 where oxygen ions are not injected, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively;

[0094] Step 6, clean the semiconductor substrate 2, alloy it in an alloy furnace, heat it to 260°C, hold it for 25s, the surface of the semiconductor substrate 2 injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate 2 not injected with oxygen ions forms the cathode of the photoconductive switch.

[0095] Step 7: Use quartz sand with a particle size of 0.05 mm to sandblast the entire semiconductor substrate 2 except for the bonding portion of the alloy electrode 3, or use sandpaper with the same particle size to polish until the original polished surface is no longer visible.

[0096] Step 8: Use conductive silver glue to bond the external metal electrode 1 to the corresponding alloy electrode 3, connect the two external metal electrodes 1 arranged on the upper and lower surfaces of the same end of the semiconductor substrate 2 through the copper tape 4, and the copper tape 4 tightly wraps the two external metal electrodes 1 to form a snap-on structure; the external metal electrode 1 is connected to the external circuit through a wire;

[0097] Step 9: Use transparent epoxy resin or shadowless adhesive to insulate and package the photoconductive switch and the entire electrode to improve the insulation level.

[0098] Example 3

[0099] The photoconductive switch structure of this embodiment is the same as that of the second embodiment.

[0100] The method for making a long-life high-voltage photoconductive switch has the following specific steps:

[0101] Step 1: Clean the semiconductor substrate 2, and implant oxygen ions into one surface of the semiconductor substrate 2. The oxygen ion implantation energy is 60 keV and the implantation concentration is 1×10 15 / cm 2 ;

[0102] Step 2, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 where oxygen ions are injected, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 on the bonding surface where the subsequent alloy electrode 3 is located;

[0103] Step 3, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 injected with oxygen ions, with thicknesses of 40 Å, 50 Å, 610 Å, 75 Å, 35 Å, and 1900 Å, respectively;

[0104] Step 4, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 not implanted with oxygen ions, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 not implanted with oxygen ions;

[0105] Step 5, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 where oxygen ions are not injected, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively;

[0106] Step 6, clean the semiconductor substrate 2, alloy it in an alloy furnace, heat it to 360°C, hold it for 25s, the surface of the semiconductor substrate 2 injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate 2 not injected with oxygen ions forms the cathode of the photoconductive switch.

[0107] Step 7: Use quartz sand with a particle size of 1 mm to sandblast the entire semiconductor substrate 2 except for the bonding portion of the alloy electrode 3, or use sandpaper with the same particle size to polish until the original polished surface is no longer visible.

[0108] Step 8: Use conductive silver glue to bond the external metal electrode 1 to the corresponding alloy electrode 3, connect the two external metal electrodes 1 arranged on the upper and lower surfaces of the same end of the semiconductor substrate 2 through the copper tape 4, and the copper tape 4 tightly wraps the two external metal electrodes 1 to form a snap-on structure; the external metal electrode 1 is connected to the external circuit through a wire;

[0109] Step 9: Use transparent epoxy resin or shadowless adhesive to insulate and package the photoconductive switch and the entire electrode to improve the insulation level.

[0110] Example 4

[0111] The photoconductive switch structure of this embodiment is the same as that of the second embodiment.

[0112] The method for making a long-life high-voltage photoconductive switch has the following specific steps:

[0113] Step 1: Clean the semiconductor substrate 2, and implant oxygen ions into one surface of the semiconductor substrate 2. The oxygen ion implantation energy is 50 keV and the implantation concentration is 1×10 15 / cm 2 ;

[0114] Step 2, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 where oxygen ions are injected, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 on the bonding surface where the subsequent alloy electrode 3 is located;

[0115] Step 3, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 injected with oxygen ions, with thicknesses of 40 Å, 50 Å, 610 Å, 75 Å, 35 Å, and 1900 Å, respectively;

[0116] Step 4, cleaning the semiconductor substrate 2, applying photoresist on the surface of the semiconductor substrate 2 not implanted with oxygen ions, and after pre-baking, exposure, development and post-baking, wet etching is used to expose the surface of the semiconductor substrate 2 not implanted with oxygen ions;

[0117] Step 5, cleaning the semiconductor substrate 2, and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate 2 where oxygen ions are not injected, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively;

[0118] Step 6, clean the semiconductor substrate 2, alloy it in an alloy furnace, heat it to 300°C, hold it for 25s, the surface of the semiconductor substrate 2 injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate 2 not injected with oxygen ions forms the cathode of the photoconductive switch.

[0119] Step 7: Use quartz sand with a particle size of 0.06 mm to sandblast the entire semiconductor substrate 2 except for the bonding portion of the alloy electrode 3, or use sandpaper with the same particle size to polish until the original polished surface is no longer visible.

[0120] Step 8: Use conductive silver glue to bond the external metal electrode 1 to the corresponding alloy electrode 3, connect the two external metal electrodes 1 arranged on the upper and lower surfaces of the same end of the semiconductor substrate 2 through the copper tape 4, and the copper tape 4 tightly wraps the two external metal electrodes 1 to form a snap-on structure; the external metal electrode 1 is connected to the external circuit through a wire;

[0121] Step 9: Use transparent epoxy resin or shadowless adhesive to insulate and package the photoconductive switch and the entire electrode to improve the insulation level.

Claims

1. Long-life and high-voltage photoconductive switch, characterized in that: The invention comprises a semiconductor substrate (2), wherein two alloy electrodes (3) are arranged on the upper surface and the lower surface of the semiconductor substrate (2), and a block-shaped external metal electrode (1) is also arranged on the surface of each alloy electrode (3); the two external metal electrodes (1) located at the same end of the semiconductor substrate (2) are connected by a copper strip (4); the entire surface of the semiconductor substrate (2) is sandblasted and polished except for the area covered by the alloy electrodes (3), and a long-life high-voltage photoconductive switch is encapsulated throughout.

2. The long-life high-voltage photoconductive switch according to claim 1, characterized in that: The edge of the cross section of the external metal electrode (1) is a smooth chamfer or the cross section of the external metal electrode (1) is an arc shape.

3. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 1, characterized in that: The steps include: Step 1, cleaning the semiconductor substrate (2), and implanting oxygen ions into one surface of the semiconductor substrate (2); Step 2, obtaining a bonding surface required for the alloy electrode (3) on the surface of the semiconductor substrate (2) processed in step 1; Step 3, preparing an alloy electrode (3) on the surface of the semiconductor substrate (2) treated in step 2; Step 4, pre-treating the surface of the semiconductor substrate (2) not implanted with oxygen ions; Step 5, preparing an alloy electrode (3) on the surface of the semiconductor substrate (2) treated in step 4; Step 6, alloying the sample obtained in step 5; Step 7: polishing the sample surface; Step 8: Use conductive silver glue to bond the external metal electrode (1) to the corresponding alloy electrode (3), and connect the two external metal electrodes (1) arranged on the upper and lower surfaces of the same end of the semiconductor substrate (2) through the copper tape (4); Step 9: encapsulate the sample obtained in step 8.

4. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 3, characterized in that: In step 1, the oxygen ion implantation energy is 10keV-60keV, and the implantation concentration is 1×10 15 / cm 2 .

5. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 3, characterized in that: Step 2 specifically comprises: cleaning the semiconductor substrate (2), applying photoresist on the surface of the semiconductor substrate (2) where oxygen ions are implanted, and after pre-baking, exposure, development and post-baking, wet etching is performed to expose the surface of the semiconductor substrate (2) on the bonding surface where the subsequent alloy electrode (3) is located; Step 3 specifically comprises: cleaning the semiconductor substrate (2), and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate (2) injected with oxygen ions to a thickness of 40 Å, 50 Å, 610 Å, 75 Å, 35 Å, and 1900 Å, respectively.

6. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 3, characterized in that: Step 4 specifically comprises: cleaning the semiconductor substrate (2), applying photoresist on the surface of the semiconductor substrate (2) where oxygen ions are not implanted, and after pre-baking, exposure, development and post-baking, wet etching is performed to expose the surface of the semiconductor substrate (2) where oxygen ions are not implanted; Step 5 specifically comprises: cleaning the semiconductor substrate (2), and sequentially evaporating metals Ni, Ge, Au, Ge, Ni, and Au on the surface of the semiconductor substrate (2) where oxygen ions have not been implanted, with thicknesses of 50 Å, 45 Å, 620 Å, 85 Å, 30 Å, and 2300 Å, respectively; Step 6 specifically comprises: cleaning the semiconductor substrate (2), alloying in an alloy furnace, heating at a temperature of 260° C.-360° C., holding time of 25 seconds, the surface of the semiconductor substrate (2) injected with oxygen ions forms the anode of the photoconductive switch, and the surface of the semiconductor substrate (2) not injected with oxygen ions forms the cathode of the photoconductive switch.

7. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 3, characterized in that: Step 7 specifically includes: using quartz sand with a particle size of 0.05 mm to 1 mm to sandblast the entire semiconductor substrate (2) except for the bonding portion of the alloy electrode (3), or using sandpaper with the same particle size to grind until the original polished surface is no longer visible.

8. The method for manufacturing a long-life high-voltage photoconductive switch according to claim 3, characterized in that: The material of the semiconductor substrate (2) is GaAs.

9. The long-life high-voltage photoconductive switch according to claim 2, characterized in that: The alloy electrode (3) is an Au / Ge / Ni alloy electrode.

Citation Information

Patent Citations

  • Outer conductor electrode structure of homogenized planar photoconductive switch electric field, photoconductive switch device and method

    CN112563345A

  • External electrode structure of photoconductive switch and connection method of external electrode structure and photoconductive switch

    CN116864544A