Nano silicon-carbon composite material as well as preparation method and application thereof
By using a heterogeneous carbon layer structure to coat nanosilicon in lithium-ion batteries, combining mechanized crushing and high-temperature roasting technology, the problems caused by the volume changes of silicon negative electrode materials in lithium-ion batteries are solved, and the first Coulomb efficiency and the first delivery are improved. The specific capacity achieves the improvement of the structural stability of the material and the lithium ion transmission performance.
Patent Information
- Application Number
- CN202310655946.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
The silicon negative electrode material in lithium-ion batteries has structural damage and electrolyte consumption due to volume changes. It is difficult for the prior art to simultaneously improve the first Coulomb efficiency and first deliques of nano silicon.
A heterogeneous carbon layer structure is adopted, with amorphous carbon as the inner layer, graphene as the outer layer, and the outer surface of nano-silicon is coated with the carbon layer. The mass fraction of silicon is 60% to 80%, and the mass fraction of carbon is 10. % to 30%, the mass fraction of nitrogen is 0.5 to 5%, and the mass fraction of oxygen is 1 to 10%. Nano-silicon-carbon composite materials are prepared by mechanized crushing and high-temperature calcination.
It significantly improves the first Coulomb efficiency and first deliquency specific capacity of nano-silicon, ensuring the structural stability of the material and lithium ion transmission performance.
Smart Images

Figure BDA0004268161760000131 
Figure HDA0004268161770000011 
Figure HDA0004268161770000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries and discloses a nano silicon-carbon composite material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are a common power source for communication electronics and electric vehicles. The negative electrode material used commercially is mainly graphite, with a theoretical specific capacity of only 372 mAh g -1 , which can no longer meet the market's growing urgent demand for high energy density. The theoretical specific capacity of silicon is much higher than that of graphite, but the volume changes greatly during charging and discharging (the rate of change is about 300%), causing silicon to break and pulverize. On the one hand, it can destroy the electrode material structure and cause silicon to lose electrical contact; on the other hand, it can cause the SEI film to grow excessively, consuming a large amount of electrolyte, which is a problem that must be solved for the commercialization of silicon negative electrodes.
[0003] Nano-sizing can significantly suppress the adverse effects of silicon volume changes, but the increase in specific surface area brings about the problem of reduced first coulomb efficiency. One solution is to embed silicon into a carbon matrix and use carbon media to improve the structural stability of the material, but the material obtained by this method has a low silicon content and it is inevitable that silicon contacts the electrolyte. Another solution is to coat the carbon layer on the outside of silicon. Nano-sizing cannot completely eliminate the expansion stress, so the thickness of the carbon layer must be sufficient to resist the expansion stress of nano silicon, while also ensuring the transfer effect of lithium ions. The external carbon layer matrix of the prior art coated silicon is generally amorphous carbon, which is difficult to balance the above contradictions. It is very difficult to directly coat the graphene layer on the silicon surface, so there are few documents on graphene layer coated silicon. For this reason, the prior art creates a gap between silicon and its external carbon layer to reserve space for nano silicon charging expansion, but the introduction of the gap is cumbersome, and it causes part of the silicon to be out of electrical contact, affecting lithium ion transmission. In addition, the gap between silicon and the external carbon layer in industrial rolling is easy to cause the carbon layer to be destroyed. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and improve the first coulombic efficiency and the first lithium removal specific capacity of nano-silicon. To achieve this purpose, the present invention provides the following technical solutions.
[0005] 1. A nano-silicon-carbon composite material, wherein the outer surface of the nano-silicon is covered with a heterogeneous carbon layer, the inner layer of the heterogeneous carbon layer is amorphous carbon, and the outer layer is graphene.
[0006] 2. A composite material according to any of the above, wherein, based on the composite material, the mass fraction of silicon is 60% to 80%, preferably 70% to 80%; the mass fraction of carbon is 10% to 30%, preferably 10% to 20%.
[0007] 3. A composite material according to any of the preceding claims, wherein the heterogeneous carbon layer contains nitrogen.
[0008] 4. A composite material according to any of the foregoing, wherein, based on the composite material, the mass fraction of nitrogen is 0.5% to 5%, and the mass fraction of oxygen is 1% to 10%.
[0009] 5. A composite material according to any of the foregoing, wherein, based on the composite material, the mass fraction of nitrogen is 1% to 2%, and the mass fraction of oxygen is 4% to 9%.
[0010] 6. A composite material according to any of the above, wherein the median particle size of the nano-silicon is 5 to 150 nm.
[0011] 7. According to any of the aforementioned composite materials, the thickness of the heterogeneous carbon layer is 2nm to 10nm, preferably 3nm to 8nm.
[0012] 8. According to any of the aforementioned composite materials, the thickness of the graphene is 1 nm to 6 nm, preferably 2 nm to 5 nm.
[0013] 9. A composite material according to any of the preceding claims, wherein in an XPS N1s analysis of the composite material, the molar fraction of pyrrolic nitrogen is 70% to 90% based on the total molar amount of nitrogen species.
[0014] 10. A composite material according to any of the preceding claims, wherein the composite material has a particle size of 1 μm to 5 μm.
[0015] 11. A method for preparing a nano silicon-carbon composite material, comprising:
[0016] S1: dispersing elemental silicon in a solution containing a first carbon source, and obtaining nano-silicon slurry by mechanical crushing; the first carbon source is an organic carboxylic acid or carboxylic acid ester containing a hydroxyl group;
[0017] S2: adding dopamine or its ammonium salt to the nano-silicon slurry obtained in S1 to react and obtain a nano-silicon precursor;
[0018] S3: calcining the nano silicon precursor in S2 at high temperature under inert gas to obtain the nano silicon carbon composite material.
[0019] 12. The preparation method according to 11, wherein the elemental silicon is single crystal silicon or polycrystalline silicon.
[0020] 13. According to any of the above-mentioned preparation methods, wherein, in S1, the first carbon source is selected from one or more of tartaric acid, citric acid, lactobionic acid, malic acid and ascorbic acid, preferably ascorbic acid; preferably, the mass ratio of the first carbon source to silicon is 1:0.2 to 1:5.
[0021] 14. According to any of the above-mentioned preparation methods, wherein the mechanized crushing method is sand grinding (the particle size of silicon after sand grinding can be 5nm to 150nm, generally 30nm to 100nm).
[0022] 15. A preparation method according to any of the above, wherein in S1, the solvent is ethanol, isopropanol, n-butanol, hexane or cyclohexane; preferably isopropanol or ethanol.
[0023] 16. A preparation method according to any of the above, wherein the solid content in S1, calculated as silicon, is 2% to 20%.
[0024] 17. A preparation method according to any of the above-mentioned methods, wherein the mass ratio of dopamine or its ammonium salt to the first carbon source is 0.1:1 to 2:1, preferably 0.3:1 to 1.2:1.
[0025] 18. According to any of the above-mentioned preparation methods, wherein, in S2, the solvent is removed after the reaction to obtain the nano-silicon precursor, and the solvent removal method is preferably spray drying.
[0026] 19. According to any of the above-mentioned preparation methods, wherein, in S3, the temperature of the high-temperature calcination is 800°C to 1000°C.
[0027] 20. A nano-silicon-carbon composite material prepared according to any of the above-mentioned preparation methods.
[0028] 21. A negative electrode material for a lithium-ion battery, comprising any of the aforementioned nano-silicon-carbon composite materials.
[0029] 22. A negative electrode for a lithium-ion battery, comprising any of the aforementioned nano-silicon-carbon composite materials.
[0030] 23. A lithium-ion battery, comprising any one of the aforementioned nano-silicon-carbon composite materials.
[0031] Compared with the prior art, the present invention designs and manufactures a nano-silicon-carbon composite material with a novel carbon coating structure. The carbon coating is a heterogeneous carbon layer with a thickness of less than 10nm, an inner layer is an amorphous carbon layer, and an outer layer is a graphene layer. The presence of the graphene layer not only provides sufficient strength for the thin coating layer, but also ensures good lithium ion transmission performance, significantly improving the first coulomb efficiency and first lithium removal specific capacity of nano-silicon.
[0032] Other features and advantages of the present invention will be described in detail in the detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a TEM image of the nano-silicon-carbon composite material prepared according to the method of Preparation Example 1.
[0034] Figure 2 XPS N of the nano-silicon-carbon composite material prepared according to the method of Preparation Example 1 1s Spectrum.
[0035] Figure 3 This is the first charge and discharge curve of the nano-silicon-carbon composite material prepared according to the method of Preparation Example 1.
[0036] Figure 4 This is a TEM image of the nano-silicon-carbon composite material prepared according to the method of Comparative Preparation Example 2.
[0037] Figure 5 This is the XRD diagram of the nano-silicon precursor and micron silicon raw material of the nano-silicon-carbon composite material prepared according to the method of Preparation Example 1.
[0038] Figure 6 This is a particle size distribution diagram of nano-silicon prepared according to step 1 of Preparation Example 1. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with specific implementations, but it should be noted that the protection scope of the present invention is not limited by these specific implementations and principle explanations, but is determined by the claims.
[0040] In the present invention, except for the contents explicitly described, any matters or items not mentioned are directly applicable to the contents known in the art without any changes. Moreover, any embodiment described herein can be freely combined with one or more other embodiments described herein, and the technical solutions or technical ideas formed thereby are regarded as part of the original disclosure or record of the present invention, and should not be regarded as new contents not disclosed or anticipated herein, unless a person skilled in the art considers that the combination is obviously unreasonable.
[0041] All features disclosed in the present invention may be combined arbitrarily, and these combinations shall be understood as the contents disclosed or recorded in the present invention, unless a person skilled in the art considers that the combination is obviously unreasonable, and shall be deemed to be specifically disclosed and recorded in the present invention. The numerical points disclosed in this specification, unless otherwise specified, include not only the numerical points specifically disclosed in the embodiments, but also the endpoints of each numerical range in the specification, and the range of any combination of these numerical points shall be deemed to be the range disclosed or recorded in the present invention.
[0042] The technical and scientific terms in the present invention shall be based on their definitions if they are defined, and shall be understood according to the general meaning in the art if no definitions are given.
[0043] The term "nanosilicon" is defined as silicon having a median particle size (D50) of 5 nm to 500 nm.
[0044] The term "graphene" refers to a layered carbon structure with a thickness of less than 10 nm, rather than an amorphous structure, which can be clearly observed under a high-resolution transmission electron microscope, and the interlayer spacing is approximately 0.33 nm to 0.34 nm.
[0045] The term "inert gas" is defined as a gas that has no appreciable effect on the electrochemical performance of the composite material.
[0046] The term "soluble" means soluble in the solvent in which it is used.
[0047] A first aspect of the present invention provides a nano-silicon-carbon composite material, wherein the outer surface of the nano-silicon is coated with a heterogeneous carbon layer, the inner layer of the heterogeneous carbon layer is amorphous carbon, and the outer layer is graphene.
[0048] According to the composite material of the first aspect of the present invention, the two-dimensional plane of the graphene is in a covering orientation relative to the surface of the composite material.
[0049] According to the composite material of the first aspect of the present invention, there is no limitation on the form of nano-silicon, which may be nano-particles, nano-wires or nano-sheets.
[0050] According to the composite material of the first aspect of the present invention, the median particle size of the nano-silicon is 5 nm to 150 nm, preferably 30 nm to 100 nm.
[0051] According to the composite material of the first aspect of the present invention, based on the composite material, the mass fraction of silicon is 60% to 80%, preferably 70% to 80%; the mass fraction of carbon is 10% to 30%, preferably 10% to 20%.
[0052] According to the composite material of the first aspect of the present invention, in some embodiments, based on the composite material, the mass fraction of silicon is 70% to 80%, the mass fraction of carbon is 10% to 20%, the mass fraction of nitrogen is 0.5% to 5%, and the mass fraction of oxygen is 1% to 10%.
[0053] According to the composite material of the first aspect of the present invention, in some embodiments, based on the composite material, the mass fraction of silicon is 70% to 80%, the mass fraction of carbon is 10% to 20%, the mass fraction of nitrogen is 1% to 2%, and the mass fraction of oxygen is 4% to 9%.
[0054] According to the composite material of the first aspect of the present invention, the heterogeneous carbon layer contains nitrogen.
[0055] According to the composite material of the first aspect of the present invention, in some embodiments, in the XPS N1s analysis of the composite material, the molar fraction of pyrrolic nitrogen is 70% to 90% based on the total molar amount of nitrogen species. It is believed that pyrrolic nitrogen is more conducive to lithium ion transmission and improves the conductivity of the carbon layer.
[0056] According to the composite material of the first aspect of the present invention, the thickness of the heterogeneous carbon layer is 2 nm to 10 nm, preferably 3 nm to 8 nm.
[0057] According to the composite material of the first aspect of the present invention, the thickness of the graphene is 1 nm to 6 nm, preferably 2 nm to 5 nm.
[0058] According to the composite material of the first aspect of the present invention, the secondary particle size of the composite material can be 1 μm to 5 μm. The secondary particle size is related to the drying form and operating conditions of the material. For example, different types of spray dryers and different operating conditions can be used to obtain products with different secondary particle sizes. These are all existing knowledge in the field, and those skilled in the art can select appropriate equipment and operating conditions according to actual needs.
[0059] The second aspect of the present invention provides a method for preparing a nano-silicon-carbon composite material, comprising: S1 dispersing elemental silicon in a solution containing a first carbon source, and obtaining a nano-silicon slurry by mechanized crushing; the first carbon source is a hydroxyl-containing organic carboxylic acid or carboxylate; S2 adding dopamine or its ammonium salt to the nano-silicon slurry obtained in S1, and reacting to obtain a nano-silicon precursor; S3 high-temperature calcining the nano-silicon precursor in S2 under an inert gas to obtain the nano-silicon-carbon composite material.
[0060] According to the preparation method provided in the second aspect of the present invention, there is no particular limitation on the form of elemental silicon, which may be single crystal silicon and / or polycrystalline silicon.
[0061] According to the preparation method provided by the second aspect of the present invention, the first carbon source is a hydroxyl-containing organic carboxylic acid or carboxylate. The present invention has found that adding a hydroxyl-containing organic carboxylic acid or carboxylate during the mechanical crushing process can inhibit the oxidation of silicon during the crushing process. It is believed that the hydroxyl-containing organic carboxylic acid or carboxylate reacts with the highly reactive silicon sites generated in situ during the crushing, uniformly covers the silicon surface, and reduces the reaction of silicon with alcohol solvents or trace oxygen in the environment. At the same time, the surface of mechanically crushed silicon is rough, and it is relatively flat after being treated with the first carbon source.
[0062] According to the preparation method provided by the second aspect of the present invention, in S1, the first carbon source can be selected from one or more of tartaric acid, citric acid, lactobionic acid, malic acid and ascorbic acid, preferably ascorbic acid. Preferably, the mass ratio of the first carbon source to silicon is 1:0.2 to 1:5, preferably 1:0.5 to 1:5.
[0063] According to the preparation method provided in the second aspect of the present invention, the mechanized crushing method is preferably sand milling. In some embodiments, the particle size of the silicon after sand milling can be 5nm to 150nm, generally 30nm to 100nm.
[0064] According to the preparation method provided in the second aspect of the present invention, in S1, the solvent is ethanol, isopropanol, n-butanol, hexane, cyclohexane or isooctane; preferably isopropanol or ethanol.
[0065] According to the preparation method provided in the second aspect of the present invention, in some embodiments, in S1, the solid content calculated as silicon is 2% to 20%, preferably 3% to 15%.
[0066] According to the preparation method provided by the second aspect of the present invention, it is believed that the abundant alcoholic hydroxyl groups and carboxyl hydroxyl groups in the first carbon source have strong binding force with the phenolic hydroxyl groups and amino groups in dopamine, so that dopamine is evenly distributed on the surface of the nano-silicon precursor.
[0067] According to the preparation method provided by the second aspect of the present invention, the mass ratio of dopamine or its ammonium salt to the first carbon source is 0.1:1 to 2:1, preferably 0.3:1 to 1.2:1, and more preferably 0.4:1 to 1:1.
[0068] According to the preparation method provided by the second aspect of the present invention, in S2, the reaction temperature is room temperature, such as 20°C to 40°C.
[0069] According to the preparation method provided by the second aspect of the present invention, in S2, the solvent is removed after the reaction to obtain the nano-silicon precursor. The present invention has no limitation on the method of removing the solvent, and spray drying is preferred.
[0070] According to the preparation method provided in the second aspect of the present invention, the temperature of the high-temperature calcination is 800°C to 1000°C.
[0071] The third aspect of the present invention provides a nano-silicon-carbon composite material prepared according to any of the aforementioned preparation methods.
[0072] A fourth aspect of the present invention provides a lithium-ion battery negative electrode material, which contains any of the aforementioned nano-silicon-carbon composite materials.
[0073] A fifth aspect of the present invention provides a lithium-ion battery negative electrode, which contains any of the aforementioned nano-silicon-carbon composite materials.
[0074] A sixth aspect of the present invention provides a lithium-ion battery, which contains any of the aforementioned nano-silicon-carbon composite materials.
[0075] The present invention will be described in detail below through examples.
[0076] The carbon layer structure on the silicon surface was characterized by transmission electron microscopy (TEM). The model of the TEM used was JEM-2100 (JEOL Ltd.), and the test conditions of the TEM were: the acceleration voltage was 200 kV.
[0077] Instruments and methods for elemental analysis: Carbon content was tested on a TA5000 thermal analyzer in an air atmosphere with a heating rate of 10°C / min over a temperature range from room temperature (25°C) to 1000°C. Nitrogen and oxygen content were tested on an ON5500 nitrogen and oxygen analyzer produced by Gangyan NAK Testing Technology Co., Ltd. with high-purity helium as the carrier gas.
[0078] Instrument and method for particle size test: The average particle size of nano silicon after sand grinding was measured by the British Mastersizer 3000 particle size analyzer, and the parameter setting was: the light shielding degree was 5.99%. The average particle size of the finished material was measured by the British Mastersizer 2000 particle size analyzer, and the parameter setting was: the light shielding degree was 10%.
[0079] XPS test instruments and methods: X-ray photoelectron spectroscopy was performed on an ESCALab250 X-ray photoelectron spectrometer equipped with Thermo Avantage V5.926 software from Thermo Scientific. The excitation source was monochromatic Al Kα X-ray with an energy of 1486.6 eV and a power of 150 W. The penetration energy used for narrow scanning was 30 eV. The basic vacuum during the analysis was 6.5 × 10 -10 mbar, data processing was performed on Thermo Avantage software, and the sensitivity factor method was used for quantitative analysis in the analysis module. The samples were dried in a helium atmosphere at 150°C and 1 standard atmosphere for 3 hours before testing.
[0080] Electrochemical testing instrument: CT3002A battery testing system of Wuhan Blue Electric Electronics Co., Ltd.
[0081] Sand mill model: Suzhou Weige Nano Technology Co., Ltd. VB0.6Q nano sand mill
[0082] Spray dryer model: B-290 from BUCHI, Switzerland, including B-295 inert gas circulation device, using nitrogen as carrier gas for spray drying.
[0083] The raw materials in the following examples, unless otherwise specified, were commercially available.
[0084] Preparation Examples 1 to 3 are used to illustrate the nano-silicon-carbon composite material and the preparation method thereof of the present invention.
[0085] Preparation Example 1
[0086] (1) 50 g of silicon powder (single crystal silicon, silicon purity of 99.999%, particle size of 2 to 10 μm) was added to 1500 mL of isopropanol solution containing 25 g of ascorbic acid, and the mixture was sand-milled in a sand mill under nitrogen protection for 8 h, and then taken out to obtain ascorbic acid-coated nano-silicon slurry;
[0087] (2) taking 100 mL of the nano-silicon slurry prepared in step (1), stirring and dispersing the mixture, adding 0.67 g of dopamine hydrochloride, and continuing stirring at room temperature for 1 h to obtain a nano-silicon slurry coated with dopamine and ascorbic acid by in-situ reaction, and then spray drying the nano-silicon precursor;
[0088] (3) The obtained nano-silicon precursor was placed in a porcelain boat and heated in a tube furnace at 5°C min under an argon atmosphere. -1 The temperature was raised to 900°C at a rate of , then kept at that temperature for 3 hours, and naturally cooled to room temperature to obtain a nano-silicon-carbon composite material.
[0089] Preparation Example 2
[0090] (1) 50 g of silicon powder (single crystal silicon, silicon purity of 99.999%, particle size of 2 to 10 μm) was added to 1500 mL of isopropanol solution containing 50 g of citric acid, and the mixture was sand-milled in a sand mill under nitrogen protection for 8 h, and then taken out to obtain a citric acid-coated nano-silicon slurry;
[0091] (2) taking 100 mL of the nano-silicon slurry prepared in step (1), stirring and dispersing it thoroughly, adding 3.33 g of dopamine hydrochloride, and continuing stirring at room temperature for 1 hour to obtain a nano-silicon slurry coated with dopamine and citric acid in situ reaction, and then spray drying to obtain a nano-silicon precursor;
[0092] (3) Place the nano-silicon precursor in a porcelain boat and heat it in a tube furnace at 5°C min under an argon atmosphere. -1 The temperature was raised to 800° C., then kept at that temperature for 3 h, and naturally cooled to room temperature to obtain a nano-silicon-carbon composite material.
[0093] Preparation Example 3
[0094] (1) 50 g of silicon powder (single crystal silicon, silicon purity of 99.999%, average particle size of 2 to 10 μm) was added to 1500 mL of isopropanol solution containing 50 g of L-malic acid, and the mixture was sand-milled in a sand mill under nitrogen protection for 8 h, and then taken out to obtain L-malic acid-coated nano-silicon slurry;
[0095] (2) taking 100 mL of the nano-silicon slurry prepared in step (1), stirring and dispersing it thoroughly, adding 1.67 g of dopamine hydrochloride, and continuing to stir for 1 h to obtain a nano-silicon slurry coated with dopamine and L-malic acid by in-situ reaction, and then spray drying to obtain a nano-silicon precursor;
[0096] (3) Place the nano-silicon precursor in a porcelain boat and heat it in a tube furnace at 5°C min under an argon atmosphere. -1 The temperature was raised to 800° C., then kept at that temperature for 3 h, and naturally cooled to room temperature to obtain a nano-silicon-carbon composite material.
[0097] Comparative Preparation Example 1
[0098] A nano-silicon-carbon composite material was prepared according to the method of Preparation Example 1, except that no organic acid was added in step (1), and step (2) was not included. The nano-silicon slurry in step (1) was directly spray-dried to obtain a nano-silicon precursor, and then step (3) was performed.
[0099] Comparative Preparation Example 2
[0100] The nano-silicon-carbon composite material was prepared according to the method of Preparation Example 1, except that step (2) was not included, and the nano-silicon slurry of step (1) was directly spray-dried to obtain a nano-silicon precursor, and then step (3) was performed.
[0101] Comparative Preparation Example 3
[0102] A nano-silicon-carbon composite material was prepared according to the method of Preparation Example 1, except that no organic acid was added in step (1), and 1.0 g of dopamine hydrochloride was added in step (2).
[0103] Test Examples 1 to 3 are used to illustrate the electrochemical performance of the nano-silicon-carbon composite material of the present invention.
[0104] Test cases 1 to 3
[0105] The nano-silicon-carbon composite materials prepared in Preparation Examples 1 to 3 were mixed with acetylene black and a binder (the binder was sodium carboxymethyl cellulose and styrene-butadiene rubber, the mass ratio of the two was 1:1) at a mass ratio of 8:1:1 to form a slurry, which was coated on a copper foil and dried to obtain an electrode sheet. The prepared electrode sheet was used as the positive electrode, the metal lithium sheet was used as the negative electrode, and a Celgard 2400 type separator was selected, and 1 mol L -1 LiPF6 (using a mixed solvent with a volume ratio of ethylene carbonate: dimethyl carbonate: diethyl carbonate = 1:1:1) was used as the electrolyte to assemble a button half-cell in a glove box, and the battery was charged and discharged using a blue power system. The parameters were set to: current density 200mAg -1 , the voltage range is 0.01~1.5V.
[0106] Comparative test examples 1 to 3
[0107] The test was carried out according to the method of Test Example 1, except that the nano-silicon-carbon composite material was replaced by the products of Comparative Preparation Examples 1 to 3 respectively.
[0108] Table 1
[0109]
[0110] It can be seen from Test Examples 1 to 3 and Comparative Test Examples 1 to 3 in Table 1 that the lithium desorption specific capacity and the first coulombic efficiency of Test Examples 1 to 3 are significantly higher than those of Comparative Test Examples 1 to 3.
[0111] The composition of the product prepared according to Preparation Example 1 after elemental analysis is: Si 75.17%, C17.11%, O 6.40%, N 1.32%. The composition of the product prepared according to Comparative Preparation Example 2 after elemental analysis is: Si 74.38%, C 16.66%, O8.96%. The silicon content and carbon content of the two are comparable. As can be seen from Table 1, the first coulombic efficiency and the first lithium removal specific capacity of Test Example 1 are significantly higher than those of Comparative Test Example 2, indicating that the carbon coating structure of the present invention is more beneficial to improving the performance of silicon negative electrode materials. Figure 4 It can be seen that the carbon coating layer of the product prepared according to Comparative Preparation Example 2 has no layered structure under a transmission electron microscope and is amorphous carbon. Figure 1 It can be seen that for the product prepared according to Preparation Example 1, under a transmission electron microscope, the silicon surface is covered with a 3nm to 8nm thick heterogeneous carbon layer, the inner layer has no layered structure and is amorphous carbon, and the outer layer has an obvious layered structure with an interlayer spacing of about 0.33 nanometers, which is a graphene layer; the products prepared according to other preparation examples of the present invention also have the same characteristics.
[0112] The oxygen content of the product prepared according to Preparation Example 1 was 6.40% by elemental analysis; the oxygen content of the product prepared according to Comparative Preparation Example 1 was 13.51% by elemental analysis, indicating that the preparation method of the present invention inhibits the oxidation of nano-silicon.
[0113] Depend on Figure 2 It can be seen that the surface of the product prepared according to Preparation Example 1 is doped with nitrogen. Figure 2 As can be seen from Table 2, the nitrogen species on the surface of the product prepared according to Preparation Example 1 are mainly pyrrolic nitrogen, which is believed to be beneficial to the transmission of lithium ions.
[0114] Table 2
[0115] Nitrogen species Peak position / eV Peak area / % Pyridine Nitrogen 398 14.5 Pyrrolidine 399.60 71.6 Graphitic Nitrogen 400.9 13.9
[0116] Depend on Figure 5 It can be seen that the XRD patterns of the product prepared according to Preparation Example 1, its nano-silicon precursor and raw material micron silicon.
[0117] Depend on Figure 6 It can be seen that the median particle size of the nano-silicon prepared according to step 1 of preparation example 1 is 30 nm to 50 nm, and the nano-silicon prepared according to step 1 of other preparation examples and comparative preparation examples of the present invention also has the same characteristics.
Claims
1. A nano silicon-carbon composite material, characterized in that: The outer surface of the nano-silicon is covered with a heterogeneous carbon layer, the inner layer of the heterogeneous carbon layer is amorphous carbon, and the outer layer is graphene.
2. The composite material according to claim 1, characterized in that Taking the composite material as a reference, the mass fraction of silicon is 60% to 80%, and the mass fraction of carbon is 10% to 30%.
3. The composite material according to claim 1, characterized in that The heterogeneous carbon layer contains nitrogen, and in the XPS N1s analysis of the composite material, the molar fraction of pyrrolic nitrogen is 70% to 90% based on the total molar amount of nitrogen species.
4. The composite material according to claim 1, characterized in that Based on the composite material, the mass fraction of nitrogen is 0.5% to 5%, and the mass fraction of oxygen is 1% to 10%.
5. The composite material according to claim 1, characterized in that Based on the composite material, the mass fraction of nitrogen is 1% to 2%, and the mass fraction of oxygen is 4% to 9%.
6. The composite material according to claim 1, characterized in that The median particle size of the nano-silicon is 5nm to 150nm.
7. The composite material according to claim 1, characterized in that The thickness of the heterogeneous carbon layer is 3nm-8nm.
8. The composite material according to claim 1, characterized in that The thickness of the graphene is 1nm to 6nm.
9. A method for preparing a nano silicon-carbon composite material, comprising: S1 disperses elemental silicon in a solution containing a first carbon source, and obtains nano-silicon slurry by mechanical crushing; The first carbon source is a hydroxyl-containing organic carboxylic acid or carboxylic acid ester; S2: adding dopamine or its ammonium salt to the nano-silicon slurry obtained in S1 to react and obtain a nano-silicon precursor; S3: calcining the nano silicon precursor in S2 at high temperature under inert gas to obtain the nano silicon carbon composite material.
10. The preparation method according to claim 9, characterized in that: The elemental silicon is single crystal silicon or polycrystalline silicon.
11. The preparation method according to claim 9, characterized in that: In S1, the first carbon source is selected from one or more of tartaric acid, citric acid, lactobionic acid, malic acid and ascorbic acid; and the mass ratio of the first carbon source to silicon is 1:0.2 to 1:
5.
12. The preparation method according to claim 9, characterized in that: The mechanized crushing method is sand grinding, and the particle size of silicon after sand grinding is 5nm to 150nm.
13. The preparation method according to claim 9, characterized in that: In S1, the solvent is ethanol, isopropanol, n-butanol, hexane or cyclohexane.
14. The preparation method according to claim 9, characterized in that: The mass ratio of the dopamine or its ammonium salt to the first carbon source is 0.3:1 to 1.2:
1.
15. The preparation method according to claim 9, characterized in that: In S2, the solvent is removed after the reaction to obtain the nano-silicon precursor, and the solvent removal method is spray drying.
16. The preparation method according to claim 9, characterized in that: In S3, the temperature of the high temperature calcination is 800°C to 1000°C.
17. A nano-silicon-carbon composite material obtained by the preparation method according to any one of claims 9 to 16.
18. A negative electrode material for a lithium ion battery, characterized in that: A nano-silicon-carbon composite material comprising any one of claims 1 to 8 and 17.
19. A negative electrode for a lithium ion battery, characterized in that: A nano-silicon-carbon composite material comprising any one of claims 1 to 8 and 17.
20. A lithium ion battery, characterized in that: A nano-silicon-carbon composite material comprising any one of claims 1 to 8 and 17.
Citation Information
Cited By
Lithium ion battery negative electrode material and preparation method and application thereof
CN119447208A