Positive electrode material, preparation method, positive electrode plate and secondary battery

By using co-doped lithium-containing transition metal sulfide and lithium halide positive electrode materials in all solid state batteries, the problems of slow reaction kinetics and low utilization rate are solved, and the performance of high energy density is achieved.

CN119092653APending Publication Date: 2024-12-06NIO BATTERY TECH (ANHUI) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310668371.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The slow reaction kinetics, low utilization rate and low loading of the positive electrode material in all solid state batteries lead to a reduced energy density.

Method used

The lithium-containing transition metal sulfide is used to co-dopize with the lithium halide to form a positive electrode material with excellent electron conduction and ion conduction. The material is prepared by mechanical ball milling to reduce the use of solid electrolyte and carbon materials.

Benefits of technology

The ion and electron conductivity of the positive electrode material of all solid state battery is significantly improved, the electrochemical reaction kinetics are enhanced, and the energy density of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a positive electrode material. The positive electrode material comprises a first sulfide and a solid solution, the first sulfide comprises at least one lithium-containing transition metal sulfide, the lithium-containing transition metal sulfide has the chemical formula of LixMySz, M is selected from metal elements of the first subgroup, the fourth subgroup, the fifth subgroup, the sixth subgroup or the eighth subgroup, and x, y and z are optionally selected from numbers greater than 0; the solid solution comprises Li2S and a halide of lithium; the halide of lithium is selected from at least one of LiCl, LiBr and LiI.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of energy storage technology, and in particular to a positive electrode material, a method for preparing the positive electrode material, and a positive electrode sheet and a secondary battery comprising the positive electrode material. Background Art

[0002] Cathode materials such as sulfide, lithium cobalt oxide and ternary materials are widely used in all-solid-state batteries, but these materials have weak electronic and ionic conductivity. Since electrochemical reactions can only occur at the triple interface where active materials, ionic conductors and electronic conductors meet; therefore, in order to build a good path for lithium ions and electrons, cathode materials are usually mixed with solid electrolytes and carbon materials by mechanical grinding. In the composite cathode obtained, the contact between active materials and ionic and electronic conductors is usually not good, which limits the electrochemical performance of all-solid-state batteries.

[0003] The main methods to solve these problems are usually (1) using solid electrolytes with high ionic conductivity. There are three main types of solid electrolytes: oxide electrolytes (ionic conductivity of 10 -4 -10 -6 S / cm), polymer electrolyte (ionic conductivity <10 -6 S / cm), sulfide electrolyte (ionic conductivity is 10 -2 -10 -4 S / cm); among them, sulfide electrolytes have the highest ionic conductivity, comparable to that of liquid batteries. Therefore, sulfide electrolytes are the research focus in solid-state batteries. (2) Some new methods (such as constructing core-shell structures, in situ growth, and bottom-up methods) have been developed to synthesize homogeneous composite electrodes and improve the electronic or ionic conductivity of positive electrode materials in sulfide all-solid-state batteries. Despite this, solid-state batteries, especially positive electrode materials in sulfide electrolyte solid-state batteries, are still plagued by slow electrochemical reaction kinetics, low utilization rate, and low loading capacity; the most important of which is that with the addition of solid electrolytes and carbon materials to the positive electrode, the content of active substances in the positive electrode material gradually decreases, which directly leads to a decrease in the energy density of the solid-state battery. Therefore, how to reduce the content of solid electrolytes and carbon materials in the positive electrode material, thereby improving the energy density of the all-solid-state battery, is an urgent problem to be solved. Summary of the invention

[0004] In view of the problems of slow reaction kinetics, low utilization rate and low loading capacity of positive electrode materials in all-solid-state secondary batteries in the prior art, the present invention co-dopes lithium-containing transition metal sulfides and lithium halides with sulfides to improve the ionic conductivity and electronic conductivity of the positive electrode materials in the all-solid-state batteries, thereby obtaining a new type of positive electrode material for all-solid-state batteries with both excellent electronic conductivity and ionic conductivity.

[0005] The present disclosure provides a positive electrode material, which includes a first sulfide and a solid solution.

[0006] In one aspect of the present disclosure, the first sulfide comprises at least one lithium-containing transition metal sulfide having Li x M y S z A chemical formula wherein M is selected from metal elements of the first subgroup, the fourth subgroup, the fifth subgroup, the sixth subgroup or the eighth subgroup, and x, y, and z are selected from numbers greater than 0.

[0007] In one aspect of the present disclosure, the solid solution comprises Li2S and a lithium halide; the lithium halide is selected from at least one of LiCl, LiBr and LiI.

[0008] In one aspect of the present disclosure, the Li x M y S z Selected from Li2FeS2, LiMoS2, Li2TiS3, Li3NbS4, Li3CuS2 or LiVS2.

[0009] In one aspect of the present disclosure, the ratio of the molar amounts of the first sulfide and the solid solution is selected from 10-0.1.

[0010] In one aspect of the present disclosure, in the solid solution, the molar ratio of the lithium halide and Li2S is selected from 0-1.

[0011] In one aspect of the present disclosure, preferably, in the solid solution, the molar ratio of the lithium halide to Li2S is selected from 0.1-1.

[0012] In one aspect of the present disclosure, preferably, in the solid solution, the molar ratio of the lithium halide to Li2S is selected from 0.1-0.3.

[0013] In one aspect of the present disclosure, the ionic conductivity of the positive electrode material is 2.0×10 -4 ~8.5×10 -4 Scm -1 .

[0014] In one aspect of the present disclosure, the electronic conductivity of the positive electrode material is greater than 0.1 S cm -1 .

[0015] The present disclosure provides a method for preparing the aforementioned positive electrode material, the method comprising the following steps:

[0016] In an inert atmosphere, at least one of Li2S and S, M b S c and lithium halide to obtain the positive electrode material; wherein the M b S c At least one selected from molybdenum sulfide, iron sulfide, vanadium sulfide, niobium sulfide, copper sulfide and titanium sulfide, and b and c are selected from positive integers.

[0017] In one aspect of the present disclosure, at least one of Li2S and S, M b S c The molar ratio of niobium to lithium halide is selected from (5-13):(1-3):(1-3).

[0018] In one aspect of the present disclosure, preferably, at least one of Li2S and S, M b S c The molar ratio of lithium halide to lithium halide is selected from (6-7): (1-2.5): (1-2).

[0019] In one aspect of the present disclosure, the mixing comprises a ball milling process.

[0020] In one aspect of the present disclosure, the time of the ball milling process is selected from 40-100 hours.

[0021] In one aspect of the present disclosure, the rotation speed of the ball milling process is selected from 300-700 rpm.

[0022] In one aspect of the present disclosure, during the ball milling process, the ball milling media is selected from ZrO2.

[0023] In one aspect of the present disclosure, preferably, M is selected from Mo, V, Fe, Nb, Cu, Ti.

[0024] In one aspect of the present disclosure, b and c are selected from positive integers as long as they can form a chemical formula of M b S c of metal sulfides.

[0025] In one aspect of the present disclosure, preferably, the cathode material is a sulfide cathode material, and more preferably, the sulfide cathode material comprises Li2S and / or S.

[0026] In one aspect of the present disclosure, preferably, M b S c More preferably, the M b S c Selected from FeS.

[0027] In one aspect of the present disclosure, preferably, LiX is selected from lithium iodide.

[0028] The present disclosure also provides a positive electrode sheet, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material, wherein the positive electrode active material comprises the positive electrode material described above or the positive electrode material prepared according to the method described above.

[0029] The present disclosure also provides a secondary battery, which includes the above-mentioned positive electrode plate.

[0030] In one aspect of the present disclosure, the secondary battery involved in the present disclosure is an all-solid-state secondary battery.

[0031] The present disclosure also provides a method for preparing a secondary battery, the method comprising: applying a pressure of 300-400 MPa to a positive electrode active material and a solid electrolyte comprising a positive electrode material; placing a negative electrode active material on the surface of the solid electrolyte away from the positive electrode active material; and then using two metal rods as conductors and pressing them to both sides of the positive electrode and the negative electrode by applying a pressure of 100-200 MPa.

[0032] In one aspect of the present disclosure, the metal rod is a stainless steel rod.

[0033] In one aspect of the present disclosure, the compaction density of the positive electrode is selected from 2.0-3.0 g / cm 2 .

[0034] In one aspect of the present disclosure, in a secondary battery, the negative electrode active material is a Li—In alloy.

[0035] In this disclosure, M b S c It can be used to improve the electronic conductivity of the positive electrode material of the secondary battery and achieve high electrochemical reaction kinetics of the positive electrode.

[0036] In the present disclosure, LiX can be used to mix with Li2S and / or S to improve the ionic conductivity of the positive electrode material.

[0037] In this disclosure, M b S c With Li 2-a S generates a lithium-containing transition metal sulfide phase with high electronic conductivity, thereby improving the electronic conductivity of the positive electrode material; in addition, the added LiX halide and Li2S generate a Li2S-LiX solid solution phase with high ionic conductivity, thereby improving the ionic conductivity of the positive electrode material.

[0038] Beneficial effects:

[0039] In the present disclosure, lithium-containing transition metal sulfides, lithium halides and sulfides are co-doped to obtain a positive electrode material having both excellent electronic conductivity and ionic conductivity. The content of metal sulfide and lithium halide is adjusted at the same time, and the energy density of the positive electrode material of the all-solid-state battery is improved without adding any solid electrolyte and carbon material. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present disclosure clearer, the technical solution of the present disclosure will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present disclosure. The embodiments of the present disclosure should not be interpreted as limiting the present disclosure.

[0041] the term:

[0042] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0043] In this article, the terms "comprises", "comprising" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device that includes the element.

[0044] In the description herein, unless otherwise specified, “above” and “below” include the number.

[0045] Unless otherwise specified, the terms used in this disclosure have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the various parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this disclosure).

[0046] The term "about" is used to describe and illustrate small changes. When used in conjunction with an event or situation, the term may refer to an example in which the event or situation occurs precisely and an example in which the event or situation occurs very approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. In addition, amounts, ratios, and other numerical values ​​are sometimes presented in this article in a range format. It should be understood that such a range format is for convenience and simplicity, and should be flexibly understood to include not only numerical values ​​explicitly designated as range limits, but also all individual numerical values ​​or subranges encompassed within the range, as if each numerical value and subrange were explicitly designated.

[0047] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.

[0048] The present disclosure is further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.

[0050] positive electrode:

[0051] In some embodiments of the present disclosure, the positive electrode includes a positive electrode sheet, and the positive electrode sheet includes a current collector and a positive electrode material disposed on the current collector. In some embodiments of the present disclosure, the positive electrode current collector may be aluminum (Al), but is not limited thereto.

[0052] In some embodiments of the present disclosure, the positive electrode material includes a first sulfide and a solid solution.

[0053] In some embodiments of the present disclosure, the first sulfide includes at least one lithium-containing transition metal sulfide having Li x M y S zA chemical formula wherein M is selected from metal elements of the first subgroup, the fourth subgroup, the fifth subgroup, the sixth subgroup or the eighth subgroup, and x, y, and z are selected from numbers greater than 0.

[0054] In some embodiments of the present disclosure, the solid solution comprises Li2S and a lithium halide; the lithium halide is selected from at least one of LiCl, LiBr and LiI.

[0055] In some embodiments of the present disclosure, the Li x M y S z Selected from Li2FeS2, LiMoS2, Li2TiS3, Li3NbS4, Li3CuS2 or LiVS2.

[0056] In some embodiments of the present disclosure, the molar ratio of the first sulfide to the solid solution is selected from 10-0.1.

[0057] In some embodiments of the present disclosure, in the solid solution, the molar ratio of the lithium halide to Li2S is selected from 0-1.

[0058] In some embodiments of the present disclosure, the M b S c At least one selected from the group consisting of molybdenum sulfide, iron sulfide, vanadium sulfide, niobium sulfide, copper sulfide, and titanium sulfide.

[0059] In some embodiments of the present disclosure, the positive electrode material further includes a binder, and optionally includes a conductive material. The binder improves the bonding between the positive electrode active material particles, and also improves the bonding between the positive electrode active material and the current collector. In some embodiments of the present disclosure, the binder includes, but is not limited to: polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin, nylon, etc. In some embodiments of the present disclosure, the conductive material includes, but is not limited to: carbon-based materials, metal-based materials, conductive polymers, and mixtures thereof. In some embodiments of the present disclosure, the carbon-based material is selected from natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments of the present disclosure, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum, silver. In some embodiments, the conductive polymer is a polyphenylene derivative.

[0060] negative electrode:

[0061] The materials, composition and manufacturing method of the negative electrode that can be used in the embodiment of the present application include any technology disclosed in the prior art.

[0062] In some embodiments of the present disclosure, the negative electrode includes a negative electrode active material, and the negative electrode active material includes one or more of lithium metal, a composite material containing lithium metal, a carbon-based material such as artificial graphite, natural graphite or hard carbon, silicon and a silicon-containing composite material or lithium titanate.

[0063] In some preferred embodiments of the present disclosure, the negative electrode active material includes a Li—In alloy.

[0064] In some embodiments, the negative electrode active material may include a binder and optionally a conductive material to impart conductivity to the electrode. The binder improves the bonding of the negative electrode active material particles to each other and the bonding of the negative electrode active material to the current collector. Non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0065] Solid electrolyte

[0066] The materials, compositions and manufacturing methods of the solid electrolyte that can be used in the embodiments of the present application include any technology disclosed in the prior art.

[0067] According to some embodiments of the present application, the solid electrolyte includes one or more of a garnet structure solid electrolyte, a NASICON structure solid electrolyte, an organic polymer solid electrolyte, an antiperovskite solid electrolyte or a sulfide solid electrolyte. According to some specific embodiments of the present application, the garnet structure solid electrolyte includes Li7La3Zr2O 12 or Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 etc. Non-limiting examples of NASICON structured solid electrolytes include Li 1.3 Al 0.3 Ti 1.7(PO4)3, etc. Non-limiting examples of organic polymer solid electrolytes include polyethylene oxide (-[-CH2─CH2─O-]- n ) or polyacrylonitrile (C3H3N) n ), etc. Non-limiting examples of antiperovskite solid electrolytes include Li3OX (X=Cl or Br), etc. Non-limiting examples of sulfide solid electrolytes include Li6PS5Cl, Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 wait.

[0068] In some preferred embodiments of the present disclosure, the solid electrolyte comprises Li3PS4.

[0069] Secondary battery:

[0070] According to some embodiments of the present disclosure, the secondary battery is a lithium secondary battery. In some embodiments of the present disclosure, the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery or a lithium ion polymer secondary battery.

[0071] According to some embodiments of the present disclosure, the secondary battery may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0072] According to some embodiments of the present disclosure, the shape of the secondary battery is not particularly limited, and it may be cylindrical, square, or any other shape.

[0073] In some embodiments of the present disclosure, the present application further provides a battery module. The battery module includes the above-mentioned secondary battery. The battery module of the present application uses the above-mentioned secondary battery, and therefore has at least the same advantages as the secondary battery. The number of secondary batteries contained in the battery module of the present application can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.

[0074] In some embodiments of the present disclosure, the present application further provides a battery pack, which includes the above-mentioned battery module. The number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0075] In some embodiments of the present disclosure, the electrochemical device of the present application includes, but is not limited to: all kinds of primary batteries, secondary batteries, fuel cells, solar cells or capacitors.

[0076] Device:

[0077] The present disclosure also provides a device, which includes at least one of the above-mentioned secondary battery, battery module or battery pack.

[0078] In some embodiments, the device includes, but is not limited to: electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, power storage systems, etc. In order to meet the device's requirements for high power and high energy density of lithium-ion batteries, a battery pack or battery module may be used.

[0079] In other embodiments, the device may be a mobile phone, a tablet computer, a laptop computer, etc. The device is usually required to be light and thin, and a lithium-ion battery may be used as a power source.

[0080] The present disclosure is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.

[0081] The present disclosure is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.

[0082] Examples and Comparative Examples

[0083] Experimental methods:

[0084] Ionic conductivity test:

[0085] The evaluation of the ionic conductivity of the synthesized positive electrode material includes the following steps: first, cold pressing Li3PS4 / positive electrode material / Li3PS4 at a pressure of 360MPa in a mold battery, and then laminating Li-In alloy on both sides of the three-layer sheet and applying a pressure of 120MPa to prepare a test cell with a five-layer structure of Li-In / Li3PS4 / positive electrode material / Li3PS4 / Li-In, with electron blocking electrodes on both sides and positive electrode material in the middle. The ionic conductivity of the material is tested using the DC polarization method.

[0086] Electronic conductivity test:

[0087] The evaluation of the electronic conductivity of the synthesized positive electrode material includes the following steps: cold pressing the material powder in a mold battery at a pressure of 360MPa, with stainless steel cylinders at both ends of the mold, that is, a sandwich structure test battery with stainless steel ion blocking electrodes on both sides and a positive electrode material layer in the middle is obtained. The electronic conductivity of the material is tested using the DC polarization method.

[0088] Charge and discharge capacity test:

[0089] The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa; Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4; two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa; the above steps are all carried out in a dry glove box filled with argon.

[0090] Electrochemical tests were carried out at a current density of 0.13 mA cm-2 at 25 °C, with discharge and charge cut-off voltages of 0 and 3.0 V, respectively.

[0091] Example 1

[0092] Embodiment 1 comprises the following steps:

[0093] (1) Preparation of positive electrode composite material:

[0094] 2.7565 g of Li2S, 1.7581 g of FeS and 2.6769 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0095] (2) Preparation of batteries:

[0096] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0097] Example 2

[0098] Embodiment 2 comprises the following steps:

[0099] (1) Preparation of positive electrode composite material:

[0100] 3.1011 g of Li2S, 1.9779 g of FeS and 1.3385 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0101] (2) Preparation of batteries:

[0102] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0103] Example 3

[0104] Embodiment 3 comprises the following steps:

[0105] (1) Preparation of positive electrode composite material:

[0106] 2.9403 g of Li2S, 1.4065 g of FeS and 2.6769 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0107] (2) Preparation of batteries:

[0108] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0109] Example 4

[0110] Embodiment 4 comprises the following steps:

[0111] (1) Preparation of positive electrode composite material:

[0112] 2.7565 g of Li2S, 1.7581 g of FeS, 1.9236 g of S and 2.6769 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0113] (2) Preparation of batteries:

[0114] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0115] Example 5

[0116] Embodiment 5 comprises the following steps:

[0117] (1) Preparation of positive electrode composite material:

[0118] 2.7565 g of Li2S, 1.7581 g of FeS and 0.8478 g of LiCl were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in a ZrO2 ball mill and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0119] (2) Preparation of batteries:

[0120] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0121] Example 6

[0122] Embodiment 6 comprises the following steps:

[0123] (1) Preparation of positive electrode composite material:

[0124] 2.7565 g of Li2S, 1.7581 g of FeS and 1.737 g of LiBr were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0125] (2) Preparation of batteries:

[0126] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0127] Example 7

[0128] Embodiment 7 comprises the following steps:

[0129] (1) Preparation of positive electrode composite material:

[0130] 2.7565 g of Li2S, 1.7581 g of FeS, 0.4239 g of LiCl and 0.8685 g of LiBr were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0131] (2) Preparation of batteries:

[0132] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0133] Example 8

[0134] Embodiment 8 comprises the following steps:

[0135] (1) Preparation of positive electrode composite material:

[0136] Weigh 2.7565 g of Li2S, 3.9616 g of V2S3 and 2.6769 g of LiI and mix them manually in a mortar for 30 minutes to obtain a mixture, and then put the mixture into ZrO2 ball milling beads and perform mechanical ball milling at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps are all carried out in a dry argon-filled glove box.

[0137] (2) Preparation of batteries:

[0138] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0139] Example 9

[0140] Embodiment 9 comprises the following steps:

[0141] (1) Preparation of positive electrode composite material:

[0142] 2.9403 g of Li2S, 1.792 g of TiS2 and 2.6769 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0143] (2) Preparation of batteries:

[0144] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0145] Comparative Example 1

[0146] Comparative Example 1 comprises the following steps:

[0147] (1) Preparation of positive electrode composite material:

[0148] 2.7565 g of Li2S and 1.7581 g of FeS were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0149] (2) Preparation of batteries:

[0150] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0151] Comparative Example 2

[0152] Comparative Example 2 comprises the following steps:

[0153] (1) Preparation of positive electrode composite material:

[0154] 2.7565 g of Li2S and 2.6769 g of LiI were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture, and then the mixture was placed in ZrO2 ball milling beads and mechanically ball milled at 500 rpm for 80 hours to obtain a composite positive electrode material; the above steps were all carried out in a dry argon-filled glove box.

[0155] (2) Preparation of batteries:

[0156] A composite material is used as the positive electrode material of the all-solid-state battery, without adding carbon conductive material and solid electrolyte. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. A Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0157] Comparative Example 3

[0158] Comparative Example 3 comprises the following steps:

[0159] (1) Preparation of positive electrode composite material:

[0160] Li2S is directly used as the positive electrode material.

[0161] (2) Preparation of batteries:

[0162] Li2S is used as the positive electrode material of the all-solid-state battery. No carbon conductive material and solid electrolyte are added. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0163] Comparative Example 4

[0164] Comparative Example 4 comprises the following steps:

[0165] (1) Preparation of positive electrode composite material:

[0166] 2.7565 g of Li2S, 2.2052 g of Li3PS4 and 0.5513 g of vapor grown carbon fiber (VGCF) were weighed and manually mixed in a mortar for 30 minutes to obtain a mixture; the above steps were all carried out in a dry argon-filled glove box.

[0167] (2) Preparation of batteries:

[0168] The above-mentioned composite positive electrode material is used as the positive electrode material of the all-solid-state battery. The positive electrode material and the solid electrolyte are placed in a PTFE tube with a diameter of 10 mm and pressed together under a pressure of 360 MPa. Li-In alloy is used as the negative electrode material and placed on the surface of the solid electrolyte Li3PS4. Two stainless steel rods are used as conductors and pressed to both sides of the positive and negative electrodes by applying a pressure of 120 MPa. The above steps are all carried out in a dry glove box filled with argon.

[0169] Electrochemical testing:

[0170] At 25°C, the above examples and comparative examples 1-3 were heated at 0.13 mA cm -2 The electrochemical test was carried out at a current density of , and the discharge and charge cut-off voltages were 0 and 3.0 V respectively. The test results are shown in Table 1: [Table 1]

[0171]

[0172] It can be seen that, by comparing Example 1 with Comparative Example 1, the addition of LiI significantly improves the ionic conductivity, thereby improving the capacity utilization; by comparing Example 1 with Comparative Example 2, the addition of transition metal sulfide FeS significantly improves the electronic conductivity, thereby improving the capacity utilization; by comparing Example 1 with Comparative Examples 3 and 4, it can be seen that Li2S has poor capacity utilization due to its poor ionic and electronic conductivity. After compounding a large amount of ionic conductor Li3PS4 and electronic conductor VGCF, the ionic conductivity and electronic conductivity are improved, thereby improving the discharge capacity. However, the discharge specific capacity of the overall positive electrode material of Comparative Example 4 is lower than the specific capacity of the positive electrode material synthesized in Example 1 without compounding ionic and electronic conductive agents.

[0173] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present disclosure, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present disclosure.

Claims

1. A positive electrode material, It is characterized in that The positive electrode material comprises: First sulfide, and solid solution; The first sulfide includes at least one lithium-containing transition metal sulfide, wherein the lithium-containing transition metal sulfide has Li x M y S z A chemical formula wherein M is selected from metal elements of the first subgroup, the fourth subgroup, the fifth subgroup, the sixth subgroup or the eighth subgroup, and x, y, and z are selected from numbers greater than 0; The solid solution contains Li 2 S and a lithium halide; the lithium halide is selected from at least one of LiCl, LiBr and LiI.

2. The positive electrode material according to claim 1, in, The Li x M y S z Selected from Li 2 FeS 2 、LiMoS 2 , Li 2 TiS 3 , Li 3 Nb 4 , Li 3 QUR 2 or LiVS 2 .

3. The positive electrode material according to claim 1, in, The molar ratio of the first sulfide to the solid solution is selected from 10-0.

1.

4. The positive electrode material according to claim 1, in, In the solid solution, the lithium halide and Li 2 The molar ratio of S is selected from 0-1.

5. The positive electrode material according to claim 1, in, The ionic conductivity of the positive electrode material is 2.0×10 -4 ~8.5×10 -4 S cm -1 .

6. A method for preparing the positive electrode material according to any one of claims 1 to 5, It is characterized in that The method comprises In an inert atmosphere, Li 2 At least one of S and S, M b S c and a lithium halide to obtain the positive electrode material; Among them, the M b S c At least one selected from molybdenum sulfide, iron sulfide, vanadium sulfide, niobium sulfide, copper sulfide and titanium sulfide, and b and c are selected from positive integers.

7. The method according to claim 6, in, The Li 2 At least one of S and S, M b S c The molar ratio of niobium to lithium halide is selected from (5-13):(1-3):(1-3).

8. The method according to claim 6, in, The mixing includes a ball milling process; the ball milling process satisfies at least one of the following conditions: (1) The time of the ball milling process is selected from 40 to 100 hours; (2) The rotation speed of the ball milling process is selected from 300-700 rpm; (3) During the ball milling process, the ball milling medium is selected from ZrO 2 .

9. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises the positive electrode material according to any one of claims 1 to 5 or the positive electrode material prepared by the method according to any one of claims 6 to 8.

10. A secondary battery, It is characterized in that The secondary battery comprises the positive electrode sheet according to claim 9.

Citation Information

Cited By

  • Positive electrode sheet, secondary battery, method for preparing secondary battery, and electrical apparatus