Composite positive electrode material and preparation method thereof
Through the unique ratio and preparation process of NaYMnxFe(1-x)PO4/C composite positive electrode material, the problems of insufficient electrical performance and process complexity of the positive electrode material of lithium-ion battery are solved, and high energy density and good cycle stability are achieved. The industrial production process is simplified and suitable for large-scale mass production.
Patent Information
- Application Number
- CN202411206339.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing lithium-ion battery cathode materials have insufficient electrical performance and complex manufacturing process in industrial production, making it difficult to achieve low-cost and large-scale mass production.
Using NaYMnxFe(1-x)PO4/C composite positive electrode material, the standard spherical nanoparticles are prepared through unique iron-manganese raw material ratio, grinding, spray drying and multiple sintering processes, which improve capacity and rate performance and simplify the process flow to suit the Industrialized production.
It achieves high energy density, good cycle stability and rate performance, simplifies the process flow, facilitates large-scale mass production, and reduces production costs.
Smart Images

Figure CN119092673A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite positive electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion battery is an energy storage device that is widely used in the field of energy storage, power batteries and portable electronic devices. It has the advantages of high open circuit voltage, high energy density, long service life, no memory effect, no pollution and low self-discharge. It is currently the battery product with the best comprehensive performance and the battery product with the widest range of applications. Lithium-ion batteries are composed of positive electrodes, negative electrodes, electrolytes, isolation membranes and other parts. Among them, the positive electrode material is the source of lithium ions, which determines the performance of lithium-ion batteries, and directly determines the energy density and safety of the battery, thereby affecting the overall performance of the battery. Moreover, the positive electrode material accounts for more than 40% of the overall material cost of lithium batteries, so its cost also directly determines the overall cost of the battery.
[0003] Lithium manganese iron phosphate (LMFP) is considered in the industry to be an upgraded version of lithium iron phosphate and is currently a relatively feasible upgrade solution for lithium iron phosphate. This solution is to add a certain amount of manganese to lithium iron phosphate and adjust the ratio of its atomic number to iron (manganese to iron ratio) to increase the voltage platform of the material. (1-x) Fe x PO4) is an upgraded product of lithium iron phosphate, where X is the manganese-iron ratio. It has similar properties to lithium iron phosphate and lithium manganese phosphate. It has better thermal stability, chemical stability and economy than ternary materials, and has a higher energy density than lithium iron phosphate.
[0004] The invention application with publication number CN117673330A discloses a method for preparing sodium manganese iron pyrophosphate positive electrode material. This invention application uses lower-cost bulk oxides for reduction pretreatment and matches the continuous production process to efficiently synthesize sodium manganese iron pyrophosphate positive electrode material with uniform particles, high phase purity, obvious charge and discharge voltage platform, and good performance. However, the specific capacity of this product is low, and the 0.1C discharge specific capacity is only 107.55mAh / g, which is not competitive compared to existing products on the market. The invention application with publication number CN109659525A discloses a method for preparing sodium manganese iron fluorophosphate composite positive electrode material. This invention application converts Na2Fe (1-x) Mn xPO4F is compounded with conductive polymers to produce synergistic effects, and a composite material with excellent electrochemical performance is obtained. It has high specific capacity, good rate performance, long cycle life, and good safety performance. It is a new type of high energy density battery composite positive electrode material with broad application prospects. However, its production process is complicated, and it is difficult to control the quality of the manufacturing process, so it is not possible to implement low-cost large-scale mass production.
[0005] Fan Hao from Wuhan University of Technology published a paper titled "Na4Fe 1.5 Mn 1.5 (PO4)2(P2O7):A Low-Cost and Earth-Abundant Cathode for RobustSodium Storage, Materials Today Energy, 2024, 101552, ISSN 2468-6069. This paper designs an iron-manganese-based mixed phosphate cathode material Na4Fe with high average operating voltage and excellent cycle stability. 1.5 Mn 1.5 (PO4)2(P2O7) / C-rGO (NFMPP / C-rGO), this material has a high specific capacity of up to 121mAh / g (0.1C), an energy density of 392Wh / kg, and excellent cycle stability. However, this material has poor rate performance, and the manufacturing process is not suitable for mass production, and it is not feasible to implement low-cost large-scale mass production.
[0006] In summary, there is an urgent need to design a positive electrode material and a preparation method that are suitable for industrial production and have good electrical properties to solve the problems existing in the prior art. Summary of the invention
[0007] The object of the present invention is to provide a composite positive electrode material suitable for industrial production and having good electrical properties and a preparation method thereof. The specific technical scheme is as follows:
[0008] A composite positive electrode material, the chemical formula of the composite positive electrode material is NaYMn x Fe (1-x) PO4 / C, x value is 0.45-0.5, the typical value is 0.48;
[0009] Y is one or more of Mg, Co, Ni, Cr, V, Ti, Zr and Nb elements.
[0010] Preferably, Y accounts for 0.3%-0.5% of the total mass of the composite positive electrode material; C accounts for 2%-5% of the total mass of the composite positive electrode material; the composite positive electrode material is a regular spherical nanoparticle with a particle size D50 of 0.4-1 μm, and a typical value of 500-950 nm.
[0011] In LiMn (1-x) Fe x In PO4 material, x represents the manganese doping ratio, which can be any value between 0-1. Since Mn has a higher voltage platform and Fe has better conductivity, different manganese-iron ratios make the performance of lithium manganese iron phosphate different. When the manganese-iron ratio is relatively high, Mn drives the battery voltage and energy density to increase significantly. In the prior art, in order to pursue the improvement of capacity density, the Mn content in the material is often not less than 50%. However, excessive manganese content will destroy the solid solution structure due to the Jahn-Teller effect, resulting in the dissolution of active materials and rapid decay of cycle performance. The present invention further improves the electrical properties such as capacity and rate performance while ensuring the cycle performance through particle nano-sizing, and has broad application prospects.
[0012] The present invention also discloses a method for preparing a composite positive electrode material, which is used to prepare the composite positive electrode material;
[0013] The preparation method comprises the following steps:
[0014] The material is added and mixed, specifically: an iron source, a manganese source, a phosphorus source and a sodium source are added according to a mass ratio and stirred to obtain a first mixed solution; a carbon source is added to the first mixed solution according to a mass ratio and stirred to obtain a second mixed solution; an additive containing Y is added to the second mixed solution according to a mass ratio and stirred to obtain an original slurry;
[0015] The first grinding is to grind the original slurry by crushing with abrasives of different diameters to obtain a first slurry, wherein the particle size of the first slurry is as follows: D50 < 1.2 μm, D90 < 10 μm;
[0016] The second grinding is to grind the first slurry by crushing with a grinding agent to obtain a second slurry, wherein the particle size of the second slurry is as follows: D50 < 0.35 μm, D90 < 0.8 μm;
[0017] Spray drying, specifically: spray drying the second slurry to obtain dry powder;
[0018] The first sintering is specifically: sintering the dry powder at a typical temperature of 460° C. to 480° C. to obtain a first sintering material;
[0019] The first crushing and demagnetization is specifically: the first sintered material is subjected to airflow crushing to remove magnetic substances, thereby obtaining the first material;
[0020] The second sintering is specifically: sintering the first material at a typical temperature of 830° C. to 870° C. to obtain a second sintered material;
[0021] The second pulverization and demagnetization is specifically: the second sintered material is subjected to air flow pulverization to remove the magnetic material to obtain a composite positive electrode material.
[0022] Preferably, the iron source is ferric phosphate and / or ferromanganese phosphate; the manganese source is manganese tetraoxide and / or manganese dioxide; the phosphorus source is sodium dihydrogen phosphate; the sodium source is sodium carbonate and / or sodium hydroxide; the carbon source is glucose and / or sucrose; the additive is polyethylene glycol and Y oxide, Y is one or more of Mg, Co, Ni, Cr, V, Ti, Zr and Nb elements; the mass ratio of the iron source, manganese source, phosphorus source and sodium source is 4:4:3:1; the input amount of the iron source, manganese source, phosphorus source and sodium source is the fed amount, the mass ratio of the carbon source to the fed amount is 2-5:100 and the typical value is 5%, the mass ratio of the additive to the fed amount is 3-5:1000 and the typical value is 0.3%; the polyethylene glycol comprises at least one of PEG200, PEG1000, PEG1500 and PEG2000.
[0023] Preferably, the first grinding includes one grinding unit or at least two grinding units performed sequentially; the grinding unit includes a first grinding, a second grinding and a third grinding performed sequentially;
[0024] In the first grinding, the grinding agent comprises zirconium oxide beads with diameters of 0.5-0.6 mm and 0.3-0.4 mm, respectively, and the number ratio of the two diameters of zirconium oxide beads is 6:4; the grinding time is 0.5-1h; the particle size of the slurry satisfies: D90<25μm;
[0025] In the second grinding, the abrasive comprises zirconium oxide beads with diameters of 0.8-1.2 mm, 0.5-0.6 mm and 0.3-0.4 mm, respectively, and the number ratio of the three diameters of zirconium oxide beads is 7:2:1; the grinding time is 0.5-1 h; the particle size of the slurry satisfies: D50<3 μm, D90<15 μm;
[0026] In the third grinding, the grinding agent is zirconia beads with a diameter of 0.2-0.3 mm; the grinding time is 0.5-1h; the particle size of the first slurry satisfies: D50<1.2μm, D90<10μm.
[0027] Preferably, 0.1-0.2 mm zirconium oxide beads are used for grinding in the second grinding, and the blowing pressure during grinding is 0.2-0.6 MPa; the grinding time is 1-2 h.
[0028] Preferably, the spray drying is carried out in a spray drying tower, and the specific parameters are: the inlet air temperature is 200°C-260°C; the exhaust air temperature is 90°C-120°C; the negative pressure in the spray drying tower is less than or equal to 2kpa; and the particle size of the dry powder is D50<10μm.
[0029] Preferably, the first sintering includes three processes: a heating section, a constant temperature section and a cooling section, specifically: heating for 3.5-6.5 hours to a typical temperature of 460°C-480°C, maintaining a constant temperature for 4-7 hours, and cooling for 5.5-8.5 hours to room temperature; a positive pressure of 10-50pa is ensured in the furnace body of the sintering furnace; the difference between the actual temperature and the set temperature in the constant temperature section does not exceed ±2°C; the difference between the actual temperature and the set temperature in the heating section does not exceed ±5°C; the particle size of the first sintering material is D50<25um; the temperature of the first sintering material is less than 80°C; the moisture content of the first sintering material is less than 250ppm.
[0030] Preferably, the second sintering includes three processes: a heating section, a constant temperature section and a cooling section, specifically: heating for 3.5-6.5 hours to a typical temperature of 830°C-870°C, maintaining a constant temperature for 9-11 hours, and cooling for 5.5-8.5 hours to room temperature; ensuring a positive pressure of 10-50pa in the furnace body of the sintering furnace; the difference between the actual temperature and the set temperature in the constant temperature section does not exceed ±2°C; the difference between the actual temperature and the set temperature in the heating section does not exceed ±5°C; the particle size of the second sintering material is D50<15μm; the temperature of the second sintering material is less than 80°C; the moisture content of the second sintering material is less than 250ppm.
[0031] Preferably, the first crushing and demagnetization and the second crushing and demagnetization are both crushed by airflow crushing equipment, and demagnetization is carried out by a demagnetizer; the particle size of the first material is D50=0.3-1.3μm; the particle size of the composite positive electrode material is D50=0.4-1.0μm, and the moisture content is less than 250ppm.
[0032] Application of the preparation method of the present invention has the following beneficial effects: the present invention adopts a unique iron-manganese raw material ratio to obtain a unique original slurry, and then the original slurry is subjected to a unique grinding + spray drying + primary sintering + primary crushing + secondary sintering + secondary crushing process to obtain regular spherical nanoparticles with a particle size D50 of 0.4-1μm, that is, the present invention prepares nano-level spherical particles through a high-temperature solid phase method, and achieves a significant improvement in electrical properties such as capacity and rate performance by improving grain distribution and particle nano-sizing. At the same time, due to the reasonable ratio of manganese iron, the cycle performance is guaranteed. The method is mature in technology and can use existing factory batch large-scale equipment, which is convenient for large-scale batch production of products and has a wide range of applications. The specific principle is: the molar ratio of manganese source to iron source is x:(1-x) and x is 0.45-0.5, which is a reasonable ratio; the first grinding and the second grinding are combined to obtain the second slurry with particle size specifications of D50<0.35μm and D90<0.8μm; the process of "feeding and mixing + primary sintering + primary crushing + secondary sintering + secondary crushing" only needs to be fed once compared with the traditional process, the process steps are simple and easy to implement in industry; the preliminary carbonization of the primary sintering can carbonize the thin carbon layer coated on the surface of the particles, and at the same time, due to the control of the sintering temperature and time, the excessive carbon coating on the surface of the particles will not be completely carbonized, so as to achieve the desired effect. During the first pulverization process, the particles will fall off and be remixed, so that the carbon source adhering to the particles during the secondary sintering process will be carbonized and coated for the second time to obtain a uniform carbon coating. The uniform carbon coating can effectively improve the conductivity of the particles. The overall uniform particle size distribution can effectively shorten the lithium ion diffusion path, and the efficiency of lithium ion migration is improved, thereby improving the rate performance of the material. While reducing the crystal particle size, the carbon coating is broken up and reassembled due to multiple pulverization processes, and the coating is looser. The specific surface area of the material is increased, thereby increasing the contact interface with the electrolyte, reducing the electrode interface impedance, and thus the electrochemical performance can be improved accordingly.
[0033] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0035] Figure 1 is a flow chart of the method for preparing the composite positive electrode material in Example 1 of the present invention;
[0036] Figure 2are typical morphological images of composite positive electrode materials, wherein: (a1) is a typical morphological image of the composite positive electrode material in Example 1 under the condition of 10,000 times magnification; (a2) is a typical morphological image of the composite positive electrode material in Example 1 under the condition of 30,000 times magnification; (b1) is a typical morphological image of the composite positive electrode material in Comparative Example 1 under the condition of 10,000 times magnification; (b2) is a typical morphological image of the composite positive electrode material in Comparative Example 1 under the condition of 30,000 times magnification; (c1) is a typical morphological image of the composite positive electrode material in Comparative Example 2 under the condition of 10,000 times magnification. (c2) is a typical morphology image of the composite positive electrode material in comparative example 2 under the condition of 30,000 times magnification; (d1) is a typical morphology image of the composite positive electrode material in comparative example 3 under the condition of 10,000 times magnification; (d2) is a typical morphology image of the composite positive electrode material in comparative example 3 under the condition of 30,000 times magnification; (e1) is a typical morphology image of the composite positive electrode material in comparative example 4 under the condition of 10,000 times magnification; (e2) is a typical morphology image of the composite positive electrode material in comparative example 4 under the condition of 30,000 times magnification. DETAILED DESCRIPTION
[0037] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0038] Embodiment 1:
[0039] A composite positive electrode material, the chemical formula of the composite positive electrode material is NaYMn x Fe (1-x) PO4 / C, x is 0.45; Y is the V element.
[0040] Y accounts for 0.3%-0.5% of the total mass of the composite positive electrode material; C accounts for 2%-5% of the total mass of the composite positive electrode material; the composite positive electrode material is a regular spherical nanoparticle with a particle size D50 of 0.75um and a typical value of 500-950nm.
[0041] A method for preparing a composite positive electrode material, for preparing the above-mentioned composite positive electrode material, see Figure 1 , specifically including the following steps:
[0042] The materials are added and mixed, specifically: an iron source, a manganese source, a phosphorus source and a sodium source are added in proportion and stirred to obtain a first mixed solution; a carbon source is added to the first mixed solution in proportion and stirred to obtain a second mixed solution; an additive containing Y is added to the second mixed solution in proportion and stirred to obtain an original slurry.
[0043] In this embodiment, the iron source is preferably ferrous phosphate; the manganese source is manganese tetraoxide; the phosphorus source is sodium dihydrogen phosphate; the sodium source is sodium carbonate; the carbon source is glucose; the additive is polyethylene glycol (preferably PEG1500) and Y oxide in a molar ratio of 1:1, and the Y oxide is vanadium oxide (chemical formula VO2). That is: according to the mass ratio of 4:4:3:1, ferrous phosphate, manganese tetraoxide, sodium dihydrogen phosphate and sodium carbonate are added to the stirring kettle for slow stirring to obtain a first mixed solution, and the sum of the masses of ferrous phosphate, manganese tetraoxide, sodium dihydrogen phosphate and sodium carbonate is the amount of feed; the carbon source is added to the first mixed solution according to 5% of the amount of feed, and the carbon source is dissolved into a suspension by adding deionized water and stirring to obtain a second mixed solution, the stirring speed is 20rpm, and the time is 10min; according to 0.3% of the amount of feed, the additive is added to the second mixed solution to obtain the original slurry, and the stirring speed is 15rpm. The original slurry was transported to the stirring tank by a pump, and then deionized water was introduced into the stirring tank to adjust the solid content of the solution to 42%, followed by rapid dispersion stirring at a dispersion stirring speed of 60 rpm and a dispersion stirring time of 1 h. The viscosity after dispersion was 1500 cP.
[0044] This embodiment uses an additive containing vanadium to change the conductivity and ion diffusion properties of the material from within the lattice. Doping ions can cause defects in the lattice and inhibit the John-Teller effect, thereby improving material performance.
[0045] The first grinding (i.e., coarse grinding) is to grind the original slurry in a crushing manner using abrasives of different diameters to obtain a first slurry, wherein: the particle size of the first slurry is as follows: D50<1.2μm, D90<10μm.
[0046] In this embodiment, the dispersed original slurry is preferably transported to a circulation tank through a pipeline, the original slurry is coarsely ground by a nano-mill, and the coarsely ground slurry is returned to the circulation tank through a pipeline. The first grinding includes one grinding unit or at least two grinding units carried out in sequence (this embodiment includes three grinding units carried out in sequence); the grinding units include a first grinding, a second grinding and a third grinding carried out in sequence; in the first grinding: the abrasive contains zirconia beads with diameters of 0.5-0.6mm and 0.3-0.4mm, respectively, and the quantity ratio of the two diameters of zirconia beads is 6:4; the grinding time is 0.5-1h; the particle size of the slurry satisfies: D90<25μm; the first grinding can increase the local stress of extrusion by grinding with zirconia beads of different particle sizes, thereby achieving rapid crushing of the powder; in the second grinding: the abrasive contains zirconia beads with diameters of 0.8-1.2mm, 0.5-0.6mm and 0.3-0.4mm, respectively, and the quantity ratio of the three diameters of zirconia beads is 7:2:1; the grinding time is 0.5-1h; the particle size of the slurry satisfies: D50<3μm, D90<15μm. In the third grinding, the grinding agent is zirconia beads with a diameter of 0.2-0.3 mm; the grinding time is 0.5-1h; the particle size of the first slurry satisfies: D50 = 1.0 μm, D90 = 5 μm. The third grinding is mainly for further breaking up the particles and shrinking the particle size range.
[0047] The second grinding (i.e., fine grinding) is specifically to grind the first slurry in a crushing manner using an abrasive to obtain a second slurry, wherein: the particle size of the second slurry is ground to the following specifications: D50 < 0.35 μm, D90 < 0.8 μm;
[0048] In this embodiment, preferably, the second grinding is performed with zirconium oxide beads, and gas is blown in during grinding; the grinding time is 1-2 hours; the particle size of the second slurry satisfies: D50=0.30μm, D90=0.75μm. The slurry that has passed the rough grinding is transported to the AB circulation tank through a pipeline, and the slurry is finely ground through a nano-mill, and the fine grinding is performed with 0.1-0.2mm zirconium oxide beads. During the grinding, a gas with a pressure of 0.2-0.6MPa is blown into the grinding machine cavity through an air pipe. The gas is compressed air or nitrogen. The gas mainly plays a role in separating particles and intensifying stirring, which can further improve the grinding efficiency. The finely ground slurry is exchanged through the AB circulation tank, and a small amount of slurry is extracted after fine grinding for particle size detection. The next step is performed after meeting the requirements.
[0049] Spray drying specifically involves spray drying the second slurry to obtain dry powder.
[0050] In this embodiment, the spray drying is carried out in a spray drying tower, and the specific parameters are: the air inlet temperature is 200℃-260℃; the exhaust air temperature is 90℃-120℃; the negative pressure in the spray drying tower does not exceed 2kpa; the particle size of the dry powder is D50<10μm. The wet-ground slurry (i.e., the second slurry) is pumped into the spray tank through the material pump, and the slurry is transported from the spray irrigation to the top of the spray drying for atomization and drying through the hose pump of the spray drying. The slurry is atomized into nano-droplets after passing through the atomizing disk. The water in the droplets contacts with hot air (natural gas heating) in the drying tower, and is instantly evaporated into water vapor at 260℃. The material bag receiver recovers the material to separate the material from the water vapor. The air inlet temperature of the spray drying is 260℃; the exhaust air temperature of the spray drying is 90℃; the particle size D50 of the atomizer granulation in the spray drying tower is 5μm.
[0051] The first sintering is specifically: sintering the dry powder at a typical temperature of 460° C.-480° C. to obtain a first sintered material.
[0052] In this embodiment, the first sintering includes three processes: a heating section, a constant temperature section and a cooling section, specifically: heating for 3.5-6.5 hours to a typical temperature of 460°C-480°C, maintaining a constant temperature for 4-7 hours, and cooling for 5.5-8.5 hours to room temperature; a positive pressure of 10-50pa is ensured in the furnace body of the sintering furnace; the difference between the actual temperature and the set temperature in the constant temperature section is ≤±2°C; the difference between the actual temperature and the set temperature in the heating section does not exceed ±5°C; the particle size of the first sintering material is D50<25μm; the temperature of the first sintering material is less than 80°C; the moisture content of the first sintering material is less than 250ppm. That is, the dry powder is fed by an automatic bowl loading machine, and a dust collector is installed above the bowl loading machine. The automatic line transports the graphite sagger to the bowl loading machine for feeding, enters the automatic line in turn, and queues up in turn to enter the furnace mouth of each kiln, and performs automatic temperature control sintering at a uniform speed. The material continuously passes through the electric heating process of heating-insulating-cooling, and completes the sintering process of reducing and synthesizing sodium manganese iron phosphate at 780°C. In order to prevent the material from being oxidized at high temperature during the sintering process, nitrogen is introduced for protection, and the kiln heating adopts an automatic temperature control electric heating system to ensure the stability of the temperature; after the material is sintered, the graphite box and the product are transported out of the kiln by rail, and then sent to the crushing workshop silo through the automatic bowl unloading machine and the conveying system to enter the next step of crushing. The sintering process is a sintering time of about 22h (heating 3.5h, constant temperature 11h, cooling 7.5h). The particle size D50 of the sintered powder is 20μm; the temperature of the material after sintering is 80℃; the moisture content of the material after sintering is 215ppm.
[0053] In this embodiment, the first sintering adopts low-temperature sintering to preliminarily carbonize the carbon source. At the same time, a crushing after sintering can improve the unevenness of the particle surface coating. The carbon source with too thick coating on the particle surface will fall off during the crushing process due to incomplete carbonization during low-temperature calcination, thereby effectively performing a second coating in the uncoated area, thereby improving the uniformity and consistency of the powder coating.
[0054] The first crushing and demagnetization is specifically: the first sintered material is subjected to air flow crushing to remove magnetic substances to obtain the first material.
[0055] In this embodiment, the first crushing and demagnetization is carried out by air flow crushing equipment, and the demagnetization treatment is carried out by a demagnetizer. That is, the sintered material is sent to the crushing bin via a closed pneumatic conveyor, and the bin is fed to the crusher for air flow crushing. The crushing pressure, feed amount, and induced draft fan frequency of the crusher are adjusted to make the product reach a qualified particle size. The qualified crushed material is separated by gas and solid through the collector at the tail end of the crusher, and the solid material enters the screening process after separation. The screened material is sent to the secondary sintering furnace through a closed pneumatic conveyor after the magnetic material is removed by the demagnetizer. The particle size D50 of the material after the crushing and demagnetization is 0.8μm.
[0056] The second sintering is specifically: sintering the first material at a typical temperature of 830° C.-870° C. to obtain a second sintered material.
[0057] In this embodiment: the second sintering includes three processes: heating section, constant temperature section and cooling section, specifically: heating for 3.5-6.5h to a typical temperature of 830℃-870℃, constant temperature for 9-11h, cooling for 5.5-8.5h to room temperature; the positive pressure in the furnace body of the sintering furnace is ensured to be 10-50pa; the difference between the actual temperature and the set temperature in the constant temperature section is ≤±2℃; the difference between the actual temperature and the set temperature in the heating section is ≤±5℃; the particle size of the second sintering material is D50<15μm; the temperature of the second sintering material is<80℃; the moisture content of the second sintering material is<250ppm. That is, the dry powder (i.e., the second sintering material) is fed by an automatic bowl loading machine. A dust collector is installed above the bowl loading machine. The automatic line transports the graphite sagger to be fed through the bowl loading machine, enters the automatic line in turn, and queues up in turn to enter the furnace mouth of each kiln. Automatic temperature-controlled sintering is carried out at a uniform speed. The material continuously passes through the electric heating process of heating-keeping-cooling, and the sintering process of reducing and synthesizing sodium ferromanganese phosphate is completed at 860°C. After the material is sintered, the graphite box and the product are transported out of the kiln via the track, and are transported to the silo of the crushing workshop through the automatic bowl unloading machine and the conveying system to enter the next step of crushing, demagnetization and packaging. The sintering process is a sintering time of 22h (heating 3.5h, constant temperature 11h, cooling 7.5h). The particle size D50 of the sintered powder is 10μm.
[0058] The second pulverization and demagnetization is specifically: the second sintered material is subjected to air flow pulverization to remove the magnetic material to obtain a composite positive electrode material.
[0059] In this embodiment: the second crushing and demagnetization is carried out by airflow crushing equipment, and the demagnetization treatment is carried out by a demagnetizer. That is, the sintered powder is further broken up by the airflow mill, and the product reaches a qualified particle size by adjusting the crushing pressure, feeding amount, and induced draft fan frequency of the crusher. The qualified crushed materials are separated by gas and solid through the collector at the tail end of the crusher, and the solid materials enter the screening process after separation. The screened materials are sent to the packaging buffer silo through a closed pneumatic conveyor after the magnetic material is removed by the demagnetizer. The packaging machine packages the materials stored in the packaging buffer silo, and the packaged materials enter the temporary storage silo. The materials enter the finished product silo after passing the inspection. The particle size of the packaged powder meets the following requirements: D50=0.75μm, D90=2.1μm; the moisture content of the packaged powder is 200ppm.
[0060] Applying the technical solution of this embodiment has the following effects:
[0061] 1. Compared with the traditional process, the unique process (i.e., the process of primary sintering + crushing + secondary sintering + crushing) only requires the input of carbon source once, has simple steps, and is easy to implement in industry.
[0062] 2. The initial carbonization of the first sintering can carbonize the thin carbon layer on the surface of the particles. At the same time, due to the control of sintering temperature and time, the excessive carbon coating on the surface of the particles will not be completely carbonized, so it will fall off and remix during the first crushing process. Therefore, during the second sintering process, the carbon source adhering to the particles will be carbonized and coated for the second time. The uniform carbon coating layer can effectively improve the conductivity of the particles. The overall uniform particle size distribution can effectively shorten the lithium ion diffusion path, and the efficiency of lithium ion migration is improved, thereby improving the rate performance of the material. While reducing the crystal particle size, the carbon coating layer is broken up and reassembled due to multiple crushing processes, and the coating layer is looser, the specific surface area of the material is increased, thereby increasing the contact interface with the electrolyte, reducing the electrode interface impedance, and the electrochemical performance can also be improved accordingly.
[0063] Embodiment 2-3:
[0064] The steps and parameters of Example 2-3 and Example 1 are compared in Table 1:
[0065] Table 1 Comparison of steps and parameters of Examples 1-3
[0066]
[0067] The typical morphology of the positive electrode material obtained in Example 2-3 is similar to the typical morphology of the composite positive electrode material in Example 1.
[0068] Comparative Example 1
[0069] A composite positive electrode material is prepared by the following method:
[0070] (1) Mixing of materials, specifically:
[0071] Add ferric phosphate, manganese tetraoxide, sodium dihydrogen phosphate and sodium carbonate into the stirring kettle in a molar ratio of 2:1:3:1 and stir slowly. The stirring speed of the powder is 5rpm. Add the carbon source to the sugar dissolving tank according to 5% of the total mass of the powder, and dissolve the carbon source into a suspension by adding deionized water and stirring. The stirring speed is 20rpm and the time is 10min. After the stirring of the sugar dissolving tank is completed, the corresponding solution is transported to the stirring kettle by a pump, and then deionized water is introduced into the stirring kettle to adjust the solid content of the solution to 40%, followed by rapid dispersion stirring. The dispersion stirring speed is 60rpm, the dispersion stirring time is 1h, and the viscosity after dispersion is 1500cP.
[0072] (2) Rough grinding, specifically:
[0073] The dispersed slurry is transported to the circulation tank through a pipeline, the slurry is coarsely ground by a nano-mill, and the coarsely ground slurry returns to the circulation tank through a pipeline, and so on and so forth, the particle size of the slurry is ground to the following particle size: D50 = 2 μm, D90 = 15 μm.
[0074] (3) Fine grinding, specifically:
[0075] The qualified slurry after rough grinding is transported to the AB circulation tank through the pipeline, and the slurry is finely ground by the nano mill. The finely ground slurry is exchanged through the AB circulation tank. A small amount of slurry is extracted after fine grinding for particle size detection. If it meets the requirements, the next step will be carried out. If the particle size exceeds this range, the process equipment parameters will be adjusted. The particle size of this process is ground to the following particle size: D50 = 0.8μm, D90 = 1.8μm. The slurry with composite particle size requirements after fine grinding is pumped into the finished product tank after pipeline demagnetization and electromagnetic iron removal.
[0076] (4) Spray drying, specifically:
[0077] The wet-ground slurry is pumped into the spray tank through the material pump, and the slurry is transported from the spray tank to the top of the spray dryer for atomization and drying through the hose pump of the spray dryer. The slurry is atomized into nano-droplets after passing through the atomizing disk. The water in the droplets contacts the hot air (heated by natural gas) in the drying tower and is instantly evaporated into water vapor at 260°C. The material bag receiver collects the material to separate the material from the water vapor. The inlet temperature of the spray dryer is 260°C; the exhaust temperature of the spray dryer is 90°C; the particle size of the atomizer granulation in the spray dryer is D50=25um.
[0078] (5) Primary sintering, specifically:
[0079] The dry powder is fed by an automatic bowl loading machine. A dust collector is installed above the bowl loading machine. The automatic line transports the graphite sagger to the bowl loading machine for feeding, enters the automatic line in turn, and queues up to enter the furnace mouth of each kiln in turn. The material is sintered at a uniform speed with automatic temperature control. The material continuously passes through the electric heating process of heating-keeping-cooling, and the sintering process of reducing and synthesizing sodium manganese iron phosphate is completed at 780°C. In order to prevent the material from being oxidized at high temperature during the sintering process, nitrogen is introduced for protection. The kiln heating adopts an automatic temperature control electric heating system to ensure the stability of the temperature; the graphite box and the product after the material sintering are transported out of the kiln through the track, and are transported to the silo of the crushing workshop through the automatic bowl unloading machine and the conveying system to enter the next step of crushing. The sintering process is a sintering time of about 22 hours (heating 3.5 hours, constant temperature 11 hours, cooling 7.5 hours). The particle size of the sintered powder is D50 = 35μm; the temperature of the material after sintering = 80°C; the moisture content of the material after sintering = 210ppm.
[0080] (6) Crushing and demagnetizing packaging, specifically:
[0081] The sintered powder is further broken up by the air flow mill, and the product reaches the qualified particle size by adjusting the crushing pressure, feed amount, and induced draft fan frequency of the crusher. The qualified crushed materials are separated by gas and solid through the collector at the tail end of the crusher, and the solid materials enter the screening process after separation. The screened materials are sent to the packaging buffer silo through a closed pneumatic conveyor after the magnetic material is removed by the demagnetizer. The packaging machine packages the materials stored in the packaging buffer silo, and the packaged materials enter the temporary storage warehouse. After the materials are inspected and qualified, they enter the finished product warehouse. The particle size of the packaged powder is: D50 = 8.84μm, D90 = 12.65μm; the moisture content of the packaged powder is 200ppm.
[0082] Comparative Examples 2-4:
[0083] The differences between Comparative Examples 2-4 and Comparative Example 1 are shown in Table 2:
[0084] Table 2 Process and parameter statistics of Example 1 and Comparative Examples 1-4
[0085]
[0086] The positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to physical and chemical analysis and electrical performance tests, and the results were shown in Tables 3-4. The materials obtained in Examples 1-3 of the present invention have higher gram capacity, rate performance and cycle performance, and have broad application prospects.
[0087] Table 3 Typical values of physical and chemical indicators
[0088]
[0089] Table 4 Electrical performance test data table
[0090]
[0091] The positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-4 were tested. The typical morphology is shown in Figure 2 , Figure 2 In: (a1) is a typical morphology of the composite positive electrode material in Example 1 under the condition of 10000 times magnification; (a2) is a typical morphology of the composite positive electrode material in Example 1 under the condition of 30000 times magnification; (b1) is a typical morphology of the composite positive electrode material in Comparative Example 1 under the condition of 10000 times magnification; (b2) is a typical morphology of the composite positive electrode material in Comparative Example 1 under the condition of 30000 times magnification; (c1) is a typical morphology of the composite positive electrode material in Comparative Example 2 under the condition of 10000 times magnification ; (c2) is a typical morphology picture of the composite positive electrode material in Comparative Example 2 when it is magnified 30,000 times; (d1) is a typical morphology picture of the composite positive electrode material in Comparative Example 3 when it is magnified 10,000 times; (d2) is a typical morphology picture of the composite positive electrode material in Comparative Example 3 when it is magnified 30,000 times; (e1) is a typical morphology picture of the composite positive electrode material in Comparative Example 4 when it is magnified 10,000 times; (e2) is a typical morphology picture of the composite positive electrode material in Comparative Example 4 when it is magnified 30,000 times.
[0092] Combining Table 3 and Table 4, we can see that:
[0093] Compared with Comparative Examples 1-4, if the proportions of Examples 1-3 of the present invention are not within the proportion range of the present invention, the cycle performance or capacity of the finished battery cell will be greatly reduced; if the preparation method does not adopt "one sintering + one crushing + two sintering + two crushing", the particle size of the powder of the finished product will be too large, and the coating effect will be poor, which will affect the conductivity of the powder and thus affect the electrical properties of the finished battery cell. The details are as follows:
[0094] Combining Examples 1-3, it can be seen that the material obtained by the material ratio and preparation method adopted by the present invention has a narrow overall particle size distribution and a uniform overall particle size (see Figure 2 (a1) and (a2)), the physical and chemical properties are roughly equal, which is convenient for mass production and subsequent battery processing; due to its stable physical and chemical properties and high consistency, its capacity, rate performance and cycle performance are stable, and compared with the industry, it is at the leading level and has broad application prospects.
[0095] Combining Example 1 and Comparative Example 1, it can be seen that: only one sintering and one pulverization are performed, and although the initial particle size of the powder reaches the nanometer level, the particles are not evenly dispersed and coated during the incineration and pulverization, resulting in poor granulation and coating effects, poor overall conductivity of the powder, large agglomeration of the powder as a whole, large particles and wide particle size distribution (see Figure 2 (b1) and (b2)); insufficient internal voids and a small overall specific surface area make it easy for the powder to have insufficient wetting during the reaction with the electrolyte, which leads to an increase in side reactions during subsequent cycles and rate discharge, and ultimately leads to poor initial coulombic efficiency, rate and cycle performance of the finished battery cell.
[0096] Combining Example 1 and Comparative Examples 2-3, it can be seen that the adjustment of the ratio of iron and manganese has an impact on the performance of the composite positive electrode material. When manganese is reduced, as shown in Comparative Example 3, the capacity will be greatly reduced; when iron is greatly reduced, as shown in Comparative Example 2, the cycle performance will be greatly reduced. The powder as a whole shows large agglomeration, large particles and wide particle size distribution (see Figure 2 (c1) and (c2) and Figure 2 (d1) and (d2)).
[0097] Combining Example 1 and Comparative Example 4, it can be seen that if only grinding is performed and then simply dried, the powder will agglomerate on a large scale (see Figure 2 (e1) and (e2)), and the particle size distribution is uncontrollable, the coating effect is extremely poor, resulting in extremely poor powder conductivity, and poor electrolyte infiltration effect, many side reactions and insufficient occurrence, resulting in a sharp deterioration in the electrical performance of the finished battery cell.
[0098] Based on the above, it can be seen that compared with the prior art, the embodiments of the present invention have the following advantages:
[0099] 1. Product ratio optimization: The present invention refers to the iron phosphate solid phase method widely used in lithium iron phosphate to prepare sodium iron manganese phosphate / carbon composite materials, and optimizes the ratio of different substances to achieve the effect of optimizing and improving performance. It can be mass-produced using existing equipment and has broad prospects for use. The existing technology is mostly prepared by various laboratory special methods, and the process technology is complicated and has strict environmental requirements. It is impossible to use the existing equipment on the market, which is not conducive to the implementation of large-scale mass production.
[0100] 2. Particle nano-crystalization: The present invention optimizes the grinding and powder sintering processes, and finally prepares a finished powder with a diameter of D50≤1μm and D90≤2.3μm, with a typical value of 500-900nm, and a uniform particle size distribution, which has good electrical properties and is a significant improvement over existing products; currently, the powder materials in the existing technology are all micron-level particles, and particle nano-crystalization improves the rate performance and other electrochemical properties by reducing the crystal particle size of the material. Nano-crystalization reduces the crystal particle size of the material through mechanical ball milling, controlling the calcination temperature, air flow crushing and other methods, thereby shortening the lithium ion diffusion path, improving the efficiency of lithium ion migration, and thus improving the rate performance of the material. While reducing the crystal particle size, the specific surface area of the material is increased, thereby increasing the contact interface with the electrolyte, reducing the electrode interface impedance, and thus the electrochemical performance can also be improved accordingly.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite positive electrode material, characterized in that: The chemical formula of the composite cathode material is NaYMn x Fe (1-x) PO4 / C, x value is 0.45-0.5; Y is one or more of Mg, Co, Ni, Cr, V, Ti, Zr and Nb elements.
2. The composite positive electrode material according to claim 1, characterized in that Y accounts for 0.3%-0.5% of the total mass of the composite positive electrode material; C accounts for 2%-5% of the total mass of the composite positive electrode material; the composite positive electrode material is a regular spherical nanoparticle with a particle size D50 of 0.4-1μm, and a typical value of 500-950nm.
3. A method for preparing a composite positive electrode material, characterized in that: Used to prepare the composite positive electrode material as claimed in claim 1 or 2; The preparation method comprises the following steps: The material is added and mixed, specifically: an iron source, a manganese source, a phosphorus source and a sodium source are added according to a mass ratio and stirred to obtain a first mixed solution; a carbon source is added to the first mixed solution according to a mass ratio and stirred to obtain a second mixed solution; an additive containing Y is added to the second mixed solution according to a mass ratio and stirred to obtain an original slurry; The first grinding is to grind the original slurry by crushing with abrasives of different diameters to obtain a first slurry, wherein the particle size of the first slurry is as follows: D50 < 1.2 μm, D90 < 10 μm; The second grinding is to grind the first slurry by crushing with a grinding agent to obtain a second slurry, wherein the particle size of the second slurry is as follows: D50 < 0.35 μm, D90 < 0.8 μm; Spray drying, specifically: spray drying the second slurry to obtain dry powder; The first sintering is specifically: sintering the dry powder at a typical temperature of 460° C. to 480° C. to obtain a first sintering material; The first crushing and demagnetization is specifically: the first sintered material is subjected to airflow crushing to remove magnetic substances, thereby obtaining a first material; The second sintering is specifically: sintering the first material at a typical temperature of 830° C. to 870° C. to obtain a second sintered material; The second pulverization and demagnetization is specifically: the second sintered material is subjected to air flow pulverization to remove the magnetic material to obtain a composite positive electrode material.
4. The preparation method according to claim 3, characterized in that: The iron source is ferric phosphate and / or ferromanganese phosphate; the manganese source is manganese tetraoxide and / or manganese dioxide; the phosphorus source is sodium dihydrogen phosphate; the sodium source is sodium carbonate and / or sodium hydroxide; the carbon source is glucose and / or sucrose; the additive is polyethylene glycol and Y oxide, and Y is one or more of Mg, Co, Ni, Cr, V, Ti, Zr and Nb elements; The mass ratio of the iron source, manganese source, phosphorus source and sodium source is 4:4:3:1; the input amount of the iron source, manganese source, phosphorus source and sodium source is the charged amount, the mass ratio of the carbon source to the charged amount is 2-5:100 and the typical value is 5%, the mass ratio of the additive to the charged amount is 3-5:1000 and the typical value is 0.3%.
5. The preparation method according to claim 3, characterized in that: The first grinding includes one grinding unit or at least two grinding units performed sequentially; the grinding unit includes a first grinding, a second grinding and a third grinding performed sequentially; In the first grinding, the grinding agent comprises zirconium oxide beads with diameters of 0.5-0.6 mm and 0.3-0.4 mm, respectively, and the number ratio of the two diameters of zirconium oxide beads is 6:4; the grinding time is 0.5-1h; the particle size of the slurry satisfies: D90<25μm; In the second grinding, the abrasive comprises zirconium oxide beads with diameters of 0.8-1.2 mm, 0.5-0.6 mm and 0.3-0.4 mm, respectively, and the number ratio of the three diameters of zirconium oxide beads is 7:2:1; the grinding time is 0.5-1 h; the particle size of the slurry satisfies: D50<3 μm, D90<15 μm; In the third grinding, the grinding agent is zirconia beads with a diameter of 0.2-0.3 mm; the grinding time is 0.5-1h; the particle size of the first slurry satisfies: D50<1.2μm, D90<10μm.
6. The preparation method according to claim 3, characterized in that: The second grinding is performed using 0.1-0.2 mm zirconium oxide beads, and the blowing pressure during grinding is 0.2-0.6 MPa; The grinding time is 1-2h.
7. The preparation method according to claim 3, characterized in that: The spray drying adopts a spray drying tower for spray drying, and the specific parameters are: the inlet air temperature is 200°C-260°C; the exhaust air temperature is 90°C-120°C; the negative pressure in the spray drying tower is less than or equal to 2kpa; and the particle size of the dry powder is D50<10μm.
8. The preparation method according to claim 3, characterized in that: The first sintering includes three processes: a heating section, a constant temperature section and a cooling section, specifically: heating for 3.5-6.5 hours to a typical temperature of 460°C-480°C, maintaining the temperature for 4-7 hours, and cooling for 5.5-8.5 hours to room temperature; ensuring a positive pressure of 10-50pa in the furnace body of the sintering furnace; the difference between the actual temperature and the set temperature in the constant temperature section does not exceed ±2°C; the difference between the actual temperature and the set temperature in the heating section does not exceed ±5°C; the particle size of the first sintering material is D50<25um; the temperature of the first sintering material is less than 80°C; the moisture content of the first sintering material is less than 250ppm.
9. The preparation method according to claim 3, characterized in that: The second sintering includes three processes: a heating section, a constant temperature section and a cooling section, specifically: heating for 3.5-6.5 hours to a typical temperature of 830°C-870°C, maintaining the temperature for 9-11 hours, and cooling for 5.5-8.5 hours to room temperature; ensuring a positive pressure of 10-50pa in the furnace body of the sintering furnace; the difference between the actual temperature and the set temperature in the constant temperature section does not exceed ±2°C; the difference between the actual temperature and the set temperature in the heating section does not exceed ±5°C; the particle size of the second sintering material is D50<15μm; the temperature of the second sintering material is less than 80°C; the moisture content of the second sintering material is less than 250ppm.
10. The preparation method according to claim 3, characterized in that: The first crushing and demagnetization and the second crushing and demagnetization are both crushed by air flow crushing equipment, and demagnetization is carried out by a demagnetizer; the particle size of the first material is D50=0.3-1.3μm; the particle size of the composite positive electrode material is D50=0.4-1.0μm, and the moisture content is less than 250ppm.