Method for preparing silicon-carbon nano composite material based on clay mineral-graphite compound and application of silicon-carbon nano composite material

Through self-assembly and chemical reduction technology of clay mineral-graphite composites, uniformly distributed silicon-carbon nanocomposites are formed, which solves the problem of insufficient interface bonding between nanosilicon and graphite composites, and improves the cycle stability of lithium-ion batteries and Electrochemical performance, suitable for the negative electrode of high-energy density lithium-ion batteries.

CN119092676APending Publication Date: 2024-12-06GUANGZHOU INSTITUTE OF GEOCHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411207652.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The specific capacity of traditional graphite anode is limited. The structure of silicon anode in lithium-ion batteries is unstable due to volume changes, and the cycle life is short. The interface bonding force between nano-silicon and graphite composite materials is weak, making it difficult to suppress volume expansion, limiting lithium-ion batteries. high energy density and long life applications.

Method used

The clay mineral-graphite composite is used to form silicon-carbon nanocomposites through peeling and self-assembly. The silicon oxide in the clay mineral is reduced to nanosilicon through chemical reduction method. The nanosilicon is evenly distributed in the graphite sheet layer to form a uniform composite , and further improve the stability of the electrode through carbon coating.

Benefits of technology

The uniform composite and structural stability of silicon-carbon nanocomposites are achieved, the preparation cost is reduced, the cycle stability and electrochemical performance of lithium-ion batteries are improved, and it is suitable for high energy density and long-life lithium-ion batteries negative electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092676A_ABST
    Figure CN119092676A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a silicon-carbon nano composite material based on a clay mineral-graphite compound and application of the silicon-carbon nano composite material. The preparation method comprises the following steps: delaminating graphite and layered clay minerals, self-assembling the delaminated layers to form a clay mineral-graphite compound, and reducing the clay mineral-graphite compound to obtain the silicon-carbon nano composite material. Natural layered mineral graphite and clay mineral which are rich in reserves and low in price are used as raw materials, the layered structures of the graphite and the clay mineral and the silicon-containing property of the clay mineral are fully utilized, the silicon element in the clay mineral is reduced into nano silicon through the steps of delamination, self-assembly, reduction and the like, and the silicon-containing property of the clay mineral is improved. According to the invention, the problem of non-uniform compounding of graphite and nano silicon in the silicon-carbon composite material is solved, the preparation process of the traditional silicon-carbon nano composite material is simplified, the cost for preparing the silicon-carbon composite material is reduced, and the prepared silicon-carbon nano composite material has relatively good structural stability and conductivity and can be widely applied to lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of efficient utilization of mineral resources and lithium ion batteries, and specifically relates to a method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite and an application thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high specific energy, high battery voltage, wide operating temperature range, and long storage life, and have been widely used in various portable electronic devices. In order to meet the needs of new fields such as electric vehicles and large-scale energy storage devices, higher requirements are placed on the energy density of lithium-ion batteries. However, the specific capacity of traditional graphite anodes (372mAh g -1 ) is limited, and the development of large-capacity, long-life, and safe lithium-ion battery negative electrode materials has become an urgent problem to be solved in related research. Silicon materials have high lithium storage capacity (3580mAh g -1 ), low working voltage, abundant reserves, and environmental friendliness, and are considered to be the most promising lithium battery negative electrode materials. However, the silicon negative electrode undergoes a huge volume change during the process of lithium extraction / insertion, resulting in the rupture and pulverization of the active material, the separation of the active material from the current collector, and the continuous generation of the solid electrolyte membrane. This causes the capacity of the silicon negative electrode to decay rapidly and the cycle stability to be poor, hindering its practical application. In order to improve the cycle life of the silicon negative electrode, researchers have proposed a series of solutions, such as designing unique nanostructures (nanowires, nanotubes, nanoporous materials, core-shell, etc.) and composite second-phase functional materials (carbon materials, metals, conductive polymers, etc.). In recent years, the silicon-carbon negative electrode composited with nano-silicon and graphite is considered to be the most promising high-performance lithium-ion battery negative electrode. Graphite has the advantages of low cost, high Coulomb efficiency, excellent cycle life, good mechanical flexibility, small volume change, and high conductivity. Combining it with nano-silicon can not only reduce the volume expansion rate of the silicon negative electrode and improve the conductivity, but also improve the specific capacity, surface capacity, and volume capacity of the negative electrode. However, the following problems still exist in the composite of nano-silicon and graphite: (1) Nano-silicon has high surface activity and is easy to agglomerate, making it difficult to achieve uniform composite with graphite, resulting in anisotropy of the silicon / graphite composite material. The difference in volume change leads to poor electrode structure stability and short cycle life; (2) Compared with silicon, the volume expansion rate of graphite during lithiation is about 10%, which can be used as a good mechanical stabilizer to inhibit the volume expansion of nano-silicon. However, the interface bonding force of directly composited nano-silicon and graphite is weak, making it difficult to inhibit the volume change of nano-silicon. Therefore, it is urgent to develop a new method for low-cost, easy-to-scale preparation of high-performance silicon-graphite nano-composite materials. Summary of the invention

[0003] In view of this, in order to solve the above-mentioned technical problems, the purpose of the present invention is to provide a method for preparing a silicon-carbon nanocomposite material, which can solve the problems of uneven composite and loose contact between silicon and graphite, simplify the preparation process of the silicon-carbon composite material and reduce the preparation cost of the silicon-carbon composite material.

[0004] Another object of the present invention is to provide a silicon-carbon nanocomposite material with excellent electrical conductivity and stable structure to improve application performance.

[0005] Another object of the present invention is to provide a silicon-carbon nanocomposite material for use in lithium-ion batteries.

[0006] In the first aspect, the present invention provides a method for preparing a silicon-carbon nanocomposite material using a clay mineral-graphite composite, which is achieved by the following scheme: first, graphite and layered clay minerals are peeled, and then the peeled sheets are self-assembled to form a clay mineral-graphite composite, followed by reduction of the clay mineral-graphite composite and acid washing to obtain a silicon-carbon nanocomposite material. Natural graphite and layered clay minerals are selected as raw materials, and the layered materials are peeled from top to bottom to obtain a single-layer or few-layer two-dimensional nanomaterial. The target clay mineral-graphite composite precursor can be constructed through self-assembly to achieve uniform composite of clay minerals and graphite. The composite is then chemically reduced, and the silicon oxide in the clay mineral is reduced to nano-silicon during the reduction process. The nano-silicon is evenly distributed in the graphite flakes, and other by-products in the reduction reaction are removed by hydrochloric acid to obtain a uniformly composited silicon-carbon nanocomposite material.

[0007] In order to achieve the above technical objectives, the technical solutions adopted are as follows:

[0008] Step 1: Composite of graphite and clay mineral sheets: First, graphite is used as a precursor and a graphite nanosheet solution is obtained by exfoliation; natural layered clay minerals are used as precursors and a single-layer or few-layer clay mineral nanosheet solution is obtained by exfoliation. The above two solutions are then mixed evenly in a certain proportion and vacuum filtered to obtain a clay mineral-graphite sheet self-assembled composite.

[0009] In an optional embodiment, a surfactant is added to the graphite nanosheet solution and the single-layer or few-layer clay mineral nanosheet solution, or the clay mineral nanosheets can be organically modified to make the surface of the clay mineral nanosheets positively charged, so that the graphite nanosheets with negative charges on the surface and the clay mineral nanosheets with positive charges on the surface are self-assembled through electrostatic effects, thereby achieving uniform recombination of the clay mineral-graphite complex.

[0010] In an optional embodiment, the graphite exfoliation in step one includes at least one of mechanical exfoliation, organic solvent ultrasonic method, surfactant ultrasonic method, ionic liquid ultrasonic method, and oxidation-exfoliation.

[0011] Preferably, the oxidation step of the oxidation-exfoliation of graphite includes at least one of Brodie method, Hummers method, improved Hummers method, and Staudenmaier method. The exfoliation step of the oxidation-exfoliation of graphite includes at least one of ultrasonic dispersion method and electrostatic repulsion dispersion method.

[0012] It should be noted that the thickness of the graphite flakes can be controlled by controlling the amount of oxidant used in the oxidation step, the amount of concentrated sulfuric acid used, the oxidation time, and the dispersion time in the dispersion process.

[0013] In an optional embodiment, the layered clay mineral in step 1 includes at least one of montmorillonite, kaolinite, vermiculite, talc, black talc, pyrophyllite, saponite, and mica.

[0014] In an optional embodiment, the stripping of the clay mineral in step one includes at least one of a high-pressure homogenization stripping method, a chemical immersion method, a grinding stripping method, a chemical immersion-grinding stripping method, an intercalation-ultrasonic method, a gas flow milling stripping method, and a molten salt stripping method.

[0015] In an optional embodiment, the graphite nanosheet solution and the clay mineral nanosheet solution in step 1 are mixed in a mass ratio of graphite to clay mineral of 1:0.5-10.

[0016] In an optional embodiment, the surfactant in step one is a cationic surfactant such as a polyalkyl quaternary ammonium salt, an alkyl pyridinium salt, or an alkyl amine salt.

[0017] Step 2: Reduction of graphite and clay mineral composites: Using clay mineral-graphite composites as precursors, silicon-carbon nanocomposites can be obtained through both metal thermal reduction and electrochemical reduction methods.

[0018] (1) Metal thermal reduction method: The above-mentioned clay mineral-graphite composite, metal reducing agent, and inorganic salt are mixed uniformly in a certain proportion, then placed in a high-temperature furnace, introduced with inert gas, and reacted at high temperature for a period of time. After natural cooling, acid washing is performed to remove reaction by-products, then ultrapure water is washed to neutral pH, and dried under vacuum conditions to obtain a silicon-carbon nanocomposite.

[0019] In an optional embodiment, preferably, the metal reducing agent is at least one of magnesium, sodium, zinc, aluminum and iron.

[0020] In an optional embodiment, the inorganic salt is at least one of an alkali metal or alkaline earth metal salt. Preferably, the inorganic salt is at least one of sodium chloride, magnesium chloride, calcium chloride, aluminum chloride, sodium nitrate, and potassium nitrate.

[0021] In an optional embodiment, the clay mineral-graphite composite, the metal reducing agent, and the inorganic salt are mixed in a mass ratio of 1:0.5-5:1-10.

[0022] In an optional embodiment, preferably, the reaction temperature of the mixture is 250-900° C., and the reaction time is 1-10 h.

[0023] In an optional embodiment, the pickling includes at least one of hydrochloric acid, nitric acid, sulfuric acid, and hydrofluoric acid.

[0024] In this reaction step, the role of the metal reducing agent is to reduce the silicon oxide in the clay mineral to elemental silicon to form a silicon-carbon nanocomposite. Under high-temperature reduction, silicon carbide may form in the area where the graphite is in close contact with the clay mineral. The silicon carbide formed in situ makes the silicon and graphite tightly connected to form a mechanically stable three-phase structure. It should be noted that the inventors found that when the thickness of the graphite flakes and the clay mineral flakes are both less than 10nm, the silicon carbide content in the product is high, and the lithium storage activity of silicon carbide is low, which is not conducive to being used as a high-capacity negative electrode material.

[0025] The role of inorganic salts is to absorb the large amount of heat released during the thermal reduction of metals, inhibit the production of high-temperature phases (such as spinel), prevent the local temperature of the reaction from being too high, and make the reaction controllable; in addition, the molten inorganic salts can also act as a partition to prevent the melting and growth of silicon particles.

[0026] (2) Electrochemical reduction method: All electrolytic reactions are carried out in a stainless steel container and an inert protective gas is introduced. Electrochemical reduction is carried out using a dual-electrode device, which is placed in a corundum crucible filled with molten salt. Before high-temperature heating, the molten salt is first dried at low temperature to remove moisture. The molten salt is then heated to the melting point, melted into a liquid and used as an electrolyte in the electrolytic reaction. The compacted pellets of the clay mineral-graphite composite are fixed on a molybdenum wire with nickel foam as the cathode, and a graphite rod is used as the anode. The dual electrodes are inserted into the molten salt and constant-voltage electrolysis is performed for a period of time. After the electrolysis is completed, the electrolysis product is removed from the molten salt and naturally cooled to room temperature. Finally, the electrolysis product is acid-washed, washed with ultrapure water to neutrality, and vacuum-dried to obtain a silicon-carbon nanocomposite.

[0027] In an optional embodiment, the inert gas is at least one of nitrogen, argon, and helium.

[0028] In an optional embodiment, the molten salt is at least one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, lithium chloride, and cesium chloride. Preferably, the melting point of the mixed molten salt is lower than 700°C.

[0029] In an optional embodiment, the temperature for heating the stainless steel container should be higher than the melting point of the molten salt, preferably, the temperature is 300-700°C.

[0030] In an optional embodiment, the electrolysis voltage range of the clay mineral-graphite composite is 2 to 4 V, and the electrolysis time is 1 to 20 h.

[0031] In an optional embodiment, the acid solution in the pickling process is at least one of hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid.

[0032] During the electrochemical reduction of clay mineral-graphite composites, the oxygen of silicon oxide in clay minerals is ionized to form elemental silicon. Graphite does not participate in the electrochemical reaction, and elemental silicon grows in situ between graphite sheets to form a uniformly composite silicon / graphite nanocomposite. In addition, due to the poor conductivity of clay mineral crystal sheets, the addition of graphite sheets can effectively improve the conductivity of the composite, thereby improving the electrolysis rate of silicon oxide.

[0033] In addition, it should be noted that the electrolysis products are closely related to the electrolysis voltage, electrolyte type, and configuration parameters of the clay mineral-graphite composite. Similar to the carbon thermal reduction method and the metal thermal reduction method, due to the spontaneous reactivity of silicon and carbon, the electrochemical reduction of silicon-carbon composites may also produce silicon carbide. However, the formation of silicon carbide can be avoided by regulating factors such as the molten salt type, electrolysis voltage, and electrolysis temperature.

[0034] The inventors have found that for clay mineral-graphite composites (the thickness of the flakes is less than 10nm, and the mass ratio is 1:1), when magnesium chloride molten salt is added to the molten salt, when the voltage range is controlled at 2.2-2.4V, the product is a silicon / graphite composite; when the voltage is 2.5V, a silicon / silicon carbide / graphite composite is generated; when the voltage is 2.6V, the product is a silicon carbide / graphite composite.

[0035] In a second aspect, the present invention provides a silicon-carbon nanocomposite material, which is prepared by the method for preparing the silicon-carbon nanocomposite material described in any one of the above embodiments.

[0036] In addition, in an embodiment, the silicon-carbon nanocomposite prepared by any of the above-mentioned embodiments is coated with a carbon layer to reduce the side reaction between the electrolyte and nano-silicon, so as to further improve the cycle stability of the electrode. Specifically, the following steps are included:

[0037] The silicon-carbon nanocomposite material obtained above is fully mixed with a coating agent to form secondary particles, wherein the coating agent is added in an amount of 1 to 50 wt % of the mixture, the mixture is heated to 400 to 1200° C., reacted for 1 to 10 hours, and then naturally cooled to room temperature to obtain a carbon-coated silicon-carbon nanocomposite material.

[0038] In an optional embodiment, preferably, the coating agent is at least one of asphalt, phenolic resin, furfural resin, coumarone resin, and dopamine hydrochloride.

[0039] In a third aspect, the present invention provides use of the silicon-carbon nanocomposite material as described in the aforementioned embodiment in a lithium ion battery.

[0040] Beneficial effects:

[0041] The beneficial effects of the present invention are embodied in:

[0042] (1) The present invention uses natural layered mineral graphite and clay minerals as raw materials, peels the layered materials from top to bottom, obtains a single layer or a few layers of two-dimensional nanomaterials, constructs a uniform composite clay mineral-graphite composite precursor through self-assembly, and then reduces the silicon oxide in the clay mineral to nano-silicon through chemical reduction (metal thermal reduction and electrochemical reduction), and the nano-silicon grows in situ in the graphite sheet interlayer to form a uniform composite silicon / graphite nano-composite material. This method uses abundant and low-priced natural minerals of graphite and clay minerals as raw materials, fully utilizes the lamellar structure of clay minerals and the properties of silicon elements, solves the problem of uneven composite formation of graphite and nano-silicon, simplifies the preparation process of silicon-graphite nano-composite materials, effectively avoids the use of high-cost nano-silicon as the raw material of silicon-carbon composites, and greatly reduces the cost of preparing silicon-carbon nano-composite materials.

[0043] (2) The structure and composition of the clay mineral-graphite composite can be regulated by self-assembly, and the product components can be precisely regulated. Compared with the traditional mechanical mixing method, the self-assembled composite is more uniform and the batch stability of the product is higher.

[0044] (3) The silicon dioxide-containing precursor is preferentially compounded with graphite. Graphite also has the following advantages in the chemical reduction process: ① Graphite can be used as a carbon source. Silicon carbide is generated at the position where graphite is in close contact with clay mineral sheets. The in-situ generated silicon carbide can be used as a rivet to tightly connect silicon and graphite sheets to form a mechanically stable ternary complex. ② In the electrochemical reduction process, since graphite has excellent electrical conductivity, the introduction of graphite sheets can improve the conductivity of the composite and further improve the electroreduction efficiency.

[0045] (4) The prepared silicon-carbon nanocomposite material has the following advantages when used as a lithium-ion negative electrode material: ① The graphite sheet and the nano-silicon composite are uniformly composited, and the graphite sheet can not only alleviate the volume expansion of the silicon negative electrode, but also form a conductive network to improve the conductivity; ② The outer carbon coating layer can further alleviate the volume expansion of the material and hinder the side reaction between silicon and the electrolyte, further improving the electrochemical stability; ③ The carbon-coated silicon / graphite composite material has a high tap density (~1g cm -3 ), with a high volumetric capacity. Batteries assembled based on silicon-carbon nanocomposites have the characteristics of fast ion / electron transmission and stable mechanical strength, showing good electrochemical lithium storage performance and can be widely used in the field of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0047] Figure 1 is the X-ray diffraction pattern of the product prepared in Example 1 of the present invention;

[0048] Figure 2 It is a cycle curve diagram of the product prepared in Example 8 of the present invention. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0050] Example 1

[0051] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0052] 1) Add 2g of natural fine flake graphite to a reagent bottle containing 200mL of a mixture of benzyl benzoate solvent and phenyl salicylate (the molar ratio of phenyl salicylate to graphite is 1:1), and ultrasonicate for 10 hours to obtain a uniform and stable dispersion. Then use a low-speed centrifuge to centrifuge at 4000rpm for 10 minutes to obtain an upper suspension. Collect the suspension, vacuum filter, and dry at 150°C for 10 hours under vacuum conditions to obtain graphite nanosheets with a thickness of about 50nm. Then disperse the dried graphite nanosheets in deionized water to prepare a graphite nanosheet solution with a concentration of 1g / L.

[0053] 2) 1 g of montmorillonite was added to 500 mL of deionized water, and stirred at 300 r / min for 12 h at room temperature to prepare a montmorillonite suspension with a mass concentration of 2 g / L. The montmorillonite suspension was transferred to a 1 L beaker, placed in an ultrasonic cell disruptor, and ultrasonically peeled at 300 W ultrasonic power for 1 min to obtain a montmorillonite nanosheet solution with a thickness of about 10 to 50 nm.

[0054] 3) 5 L of 2 g / L montmorillonite solution and 0.1 g of dodecyltrimethylammonium bromide were stirred for 2 h, and then 1 L of 1 g / L graphite nanosheet solution was added and stirred for 2 h, vacuum filtered, and dried to obtain a self-assembled complex of graphite nanosheets and montmorillonite sheets, wherein the mass ratio of graphite to clay minerals was 1:10.

[0055] 4) The montmorillonite-graphite composite, aluminum powder and aluminum chloride were mixed uniformly in a mass ratio of 1:0.5:10, and placed in a sealed reactor. Then, the reactor was placed in an oven, slowly heated to 270°C, and kept warm for 10 hours. Naturally cooled to room temperature, washed with 200mL 1M hydrochloric acid for 5 hours, then immersed in 100mL 1wt% HF for 5 minutes, washed with ultrapure water until neutral, and vacuum dried at 80°C for 10 hours to obtain a silicon-carbon nanocomposite material.

[0056] like Figure 1 As shown, the obtained silicon-carbon composite was analyzed by X-ray diffraction spectrum (XRD). The results showed that the obtained material had characteristic diffraction peaks at 28.4, 47.3, 56.1, 69.1, and 76.3° (2θ), which belonged to the silicon phase; a diffraction peak belonging to graphite appeared at 26.6° (2θ), and the product was mainly composed of elemental silicon and graphite.

[0057] Example 2

[0058] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0059] 1) Add 2g of natural fine flake graphite to a reagent bottle containing 200mL of a mixture of benzyl benzoate solvent and phenyl salicylate (the molar ratio of phenyl salicylate to graphite is 1:1), and ultrasonicate for 10 hours to obtain a uniform and stable dispersion. Then use a low-speed centrifuge to centrifuge at 4000rpm for 10 minutes to obtain an upper suspension. Collect the suspension, vacuum filter, and dry at 150°C for 10 hours under vacuum conditions to obtain graphite nanosheets with a thickness of about 50nm. Then disperse the dried graphite nanosheets in deionized water to prepare a graphite nanosheet solution with a concentration of 1g / L.

[0060] 2) 1 g of kaolinite was added to 1 L of deionized water, and stirred at 300 r / min for 4 h at room temperature to prepare a kaolinite suspension with a mass concentration of 1 g / L. The kaolinite suspension was transferred to a 1 L beaker, placed in an ultrasonic cell disruptor, and ultrasonically peeled at 300 W ultrasonic power for 1 min to obtain a kaolinite nanosheet solution with a thickness of about 50 to 100 nm.

[0061] 3) 1L 1g / L kaolinite nanosheet solution and 0.05g polyquaternium-16 were stirred for 2h, and then 1L 1g / L graphite nanosheet was added and stirred for 2h, vacuum filtered, and dried to obtain a self-assembled complex of graphite and kaolinite sheets, wherein the mass ratio of graphite to kaolinite is 1.

[0062] 4) The kaolinite-graphite composite, magnesium powder and sodium chloride were mixed uniformly in a mass ratio of 1:0.7:5, placed in a sealed reactor, placed in a high-temperature furnace, introduced into an argon atmosphere, heated to 650°C at a rate of 5°C / min, and kept warm for 5 hours. Naturally cooled to room temperature, washed with 200mL 1M hydrochloric acid for 5 hours, then immersed in 100mL 1wt% HF for 5 minutes, washed with ultrapure water until neutral, and vacuum dried at 80°C for 10 hours to obtain a silicon-carbon nanocomposite material.

[0063] The product was analyzed by X-ray diffraction spectrum, and the obtained product was composed of graphite, nano-silicon and a small amount of silicon carbide.

[0064] Example 3

[0065] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0066] 1) Add 2g of natural fine flake graphite to a reagent bottle containing 200mL of a mixture of benzyl benzoate solvent and phenyl salicylate (the molar ratio of phenyl salicylate to graphite is 1:1), and ultrasonicate for 10 hours to obtain a uniform and stable dispersion. Then use a low-speed centrifuge to centrifuge at 4000rpm for 10 minutes to obtain an upper suspension. Collect the suspension, vacuum filter, and dry at 150°C for 10 hours under vacuum conditions to obtain graphite nanosheets with a thickness of about 50nm. Then disperse the dried graphite nanosheets in deionized water to prepare a graphite nanosheet solution with a concentration of 1g / L.

[0067] 2) 10g of kaolinite is soaked in 25mL of 15% potassium acetate solution and mixed for 2h. The stirred solution is placed in a 250mL agate ball mill with a ball-to-material ratio of 6:1 and a medium ball diameter of 1mm:2mm:3mm in a ratio of 3:2:1. The mixture is ground in a planetary ball mill at a speed of 350rpm for 2h, and then the ground slurry is poured out and filtered for separation. The composite is washed with water to remove potassium acetate, and then dried and ground to obtain kaolinite nanosheets with a thickness of 1 to 2nm. The kaolinite nanosheets are dispersed in deionized water and ultrasonically dispersed at a power of 200W for 1h to prepare a kaolinite nanosheet solution with a concentration of 1g / L.

[0068] 3) 1L 1g / L kaolinite nanosheets and 0.05g polyquaternium-16 were stirred for 2h, and then 1L 1g / L graphite nanosheets were added and stirred for 2h, vacuum filtered, and dried to obtain a self-assembled complex of graphite and kaolinite sheets, wherein the mass ratio of graphite to kaolinite is 1.

[0069] 4) The kaolinite-graphite composite, magnesium powder and sodium chloride were mixed uniformly in a mass ratio of 1:0.7:5, placed in a sealed reactor, placed in a high-temperature furnace, introduced into an argon atmosphere, heated to 650°C at a rate of 5°C / min, and kept warm for 5 hours. Naturally cooled to room temperature, washed with 200mL 1M hydrochloric acid for 5 hours, then immersed in 100mL 1wt% HF for 5 minutes, washed with ultrapure water until neutral, and vacuum dried at 80°C for 10 hours.

[0070] The product was analyzed by X-ray diffraction spectroscopy, and the obtained product consisted of silicon carbide and graphite. Compared with the product of Example 2, the results showed that the thickness of the kaolinite flakes was crucial to the product composition of the magnesia thermal reduction nanographite / kaolinite flake complex. When the kaolinite flakes were less than 10nm, during the magnesia thermal reduction process, the silicon element in the kaolinite was easily combined with the carbon element in the graphite to form silicon carbide.

[0071] Example 4

[0072] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0073] 1) Add 2g of natural fine flake graphite to a reagent bottle containing 200mL of a mixture of benzyl benzoate solvent and phenyl salicylate (the molar ratio of phenyl salicylate to graphite is 1:1), and ultrasonicate for 10 hours to obtain a uniform and stable dispersion. Then use a low-speed centrifuge to centrifuge at 4000rpm for 10 minutes to obtain an upper suspension. Collect the suspension, vacuum filter, and dry at 150°C for 10 hours under vacuum conditions to obtain graphite nanosheets with a thickness of about 50nm. Then disperse the dried graphite nanosheets in deionized water to prepare a graphite nanosheet solution with a concentration of 1g / L.

[0074] 2) Add 10g of muscovite to 100mL of NN dimethylformamide liquid, stir ultrasonically at 800r / min for 6h at room temperature, and then centrifuge at 3000rpm for 5min using a low-speed centrifuge to obtain an upper suspension. Collect the suspension, vacuum filter, and dry at 150°C for 10h under vacuum conditions to obtain mica nanosheets with a thickness of about 100nm. Disperse 1g of mica nanosheets in deionized water to prepare a mica nanosheet solution with a concentration of 1g / L.

[0075] 3) 1L of 1g / L mica nanosheet solution and 0.05g of polyquaternium-16 were stirred for 2h, and then 1L of 1g / L graphite nanosheet solution was added and stirred for 2h, vacuum filtered, and dried to obtain a self-assembled complex of graphite and mica sheets.

[0076] 4) The mica-graphite composite, magnesium powder and sodium chloride were mixed uniformly in a mass ratio of 1:0.7:5, placed in a sealed reactor, placed in a high-temperature furnace, introduced into an argon atmosphere, heated to 650°C at a rate of 5°C / min, and kept warm for 8 hours. Naturally cooled to room temperature, washed with 200mL 1M hydrochloric acid for 5 hours, then soaked in 100mL 1wt% HF for 5 minutes, washed with ultrapure water until neutral, and vacuum dried at 80°C for 10 hours to obtain a silicon-carbon nanocomposite material.

[0077] The self-assembled composite formed by mica nanosheets and graphite nanosheets can obtain silicon, graphite and a small amount of silicon carbide nanocomposite materials after magnesium thermal reduction, and the nano silicon and graphite are uniformly compounded.

[0078] Example 5

[0079] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0080] 1) Add 1g of natural fine flake graphite to a beaker containing 23mL of 98% concentrated sulfuric acid, stir magnetically in an ice water bath below 15°C, and add 3g of potassium permanganate slowly while stirring, and keep the reaction in the ice water bath for 2h. Then, during the stirring process, raise the system temperature to 35°C and maintain it for 30min. During the stirring process, add a certain amount of deionized water at a uniform rate to control the reaction temperature below 98°C until the temperature of the reaction system no longer rises. Continue stirring for 30min, then add an appropriate amount of 5% H2O2 until no bubbles are generated in the system, and filter while hot. Wash the sample with appropriate amounts of 5% HCl and ultrapure water in turn until it is neutral, and there is no The filter cake was placed in a vacuum drying oven at 60°C and vacuum dried to obtain graphite oxide. The dried graphite oxide was then dispersed in deionized water and ultrasonically dispersed at 200W for 1 hour to prepare a graphene oxide solution with a concentration of 1g / L. The average thickness of the graphene oxide sheet was about 1.3nm.

[0081] 2) Soak 5g of expanded vermiculite particles in 100mL of saturated sodium chloride solution, seal the sample in a glass bottle, place the glass bottle in a 110℃ oil bath, and stir for 24h. After the sample is cooled to room temperature, centrifuge and wash the sample with distilled water and anhydrous ethanol until no chloride ions are detected in the centrifugal supernatant. Then soak the cleaned sample in 2M lithium chloride solution, seal the glass bottle, and stir at 110℃ for 24h. After the sample is cooled to room temperature, centrifuge and wash the sample with distilled water and anhydrous ethanol until no chloride ions are detected in the centrifugal supernatant. Mix the gel-like substance at the bottom with 1L of 30wt% hydrogen peroxide solution, stir and react at 110℃ for 24h, and the entire reaction process is carried out under reflux conditions. The reaction solution was cooled to room temperature and dried to obtain vermiculite nanosheets with a thickness of 2 to 4 nm. The vermiculite was dispersed in deionized water and ultrasonically dispersed at a power of 200 W for 1 h to prepare a vermiculite nanosheet dispersion solution with a concentration of 1 g / L.

[0082] 3) 1.5 L of 1 g / L vermiculite nanosheet dispersion solution and 0.07 g of polyquaternium-16 were stirred for 2 h, and then 1 L of 1 g / L graphene oxide was added and stirred for 2 h, vacuum filtered, and dried to obtain a self-assembled complex of graphene oxide and vermiculite sheets.

[0083] 4) Take 1g of graphene oxide-vermiculite sheet self-assembled complex, press it into a round cake with a diameter of 2cm under a pressure of 10MPa for 1min, and then sinter it at 700℃ for 5h. Wrap the sintered sample with nickel foam and fix it on a 2mm metal molybdenum wire collector with a 0.3mm molybdenum wire as the cathode. A graphite rod with a diameter of 15mm is used as the anode.

[0084] 5) Before the electrochemical reaction begins, dry the mixed molten salt of MgCl2, NaCl and KCl (according to the molar mass ratio of Mg:Na:K=0.508:0.271:0.221) at 250°C for 24h to remove the moisture in the molten salt, then place the inorganic salt in a zirconia crucible, and then place the zirconia crucible in the reactor. The electrochemical reaction adopts a double electrode mode, suspends the cathode and anode above the chloride salt, closes the reactor, and continuously introduces argon into the reactor through the air inlet on the reactor and discharges it through the air outlet to form an argon atmosphere in the reactor. Heat the reactor to 660°C, melt the inorganic salt, and form a molten salt as an electrolyte. Then insert the cathode and anode into the molten salt to form a double electrode system, apply a voltage of 2.4V between the two electrodes, and electrolyze at constant voltage for 6h to obtain the cathode after electrolysis, which is then taken out and cooled. The cooled cathode was placed in deionized water to remove the molten salt, then pickled with 100 mL 2M hydrochloric acid for 5 h and 100 mL 2 wt % hydrofluoric acid for 10 min, then washed with ultrapure water until neutral, and vacuum dried to obtain a silicon / graphene nanocomposite material.

[0085] The self-assembled complex formed by graphene oxide and vermiculite flakes, after electrochemical reduction, X-ray diffraction spectrum (XRD) shows that the product is composed of graphite and nano-silicon. Under transmission electron microscopy, it can be observed that the graphene and nano-silicon particles are uniformly composited.

[0086] Example 6

[0087] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0088] 1) Add 1g of natural fine flake graphite to a beaker containing 23mL of 98% concentrated sulfuric acid, stir magnetically in an ice water bath below 15°C, and add 3g of potassium permanganate slowly while stirring, and keep the reaction in the ice water bath for 2h. Then, during the stirring process, raise the system temperature to 35°C and maintain it for 30min. During the stirring process, add a certain amount of deionized water at a uniform rate to control the reaction temperature below 98°C until the temperature of the reaction system no longer rises. Continue stirring for 30min, then add an appropriate amount of 5% H2O2 until no bubbles are generated in the system, and filter while hot. Wash the sample with appropriate amounts of 5% HCl and ultrapure water in turn until it is neutral, and there is no The filter cake was placed in a vacuum drying oven at 60°C and vacuum dried to obtain graphite oxide. The dried graphite oxide was then dispersed in deionized water and ultrasonically dispersed at 200W for 1 hour to prepare a graphene oxide solution with a concentration of 1g / L. The average thickness of the graphene oxide sheet was about 1.3nm.

[0089] 2) Soak 5g of expanded vermiculite particles in 100mL of saturated sodium chloride solution, seal all samples in a glass bottle, place the glass bottle in a 110℃ oil bath, and stir for 24h. After the sample cools to room temperature, centrifuge and wash the sample with distilled water and anhydrous ethanol until no chloride ions are detected in the centrifugal supernatant. Then soak the cleaned sample in 2M lithium chloride solution, seal the glass bottle, and stir at 110℃ for 24h. After the sample cools to room temperature, centrifuge and wash the sample with distilled water and anhydrous ethanol until no chloride ions are detected in the centrifugal supernatant. Mix the gel-like substance at the bottom with 1L of 30wt% hydrogen peroxide solution, stir and react at 110℃ for 24h, and the entire reaction process is carried out under reflux conditions. The reaction solution was cooled to room temperature and dried to obtain vermiculite nanosheets with a thickness of 2 to 4 nm. The vermiculite nanosheets were dispersed in deionized water and ultrasonically dispersed at a power of 200 W for 1 h to prepare a vermiculite nanosheet dispersion solution with a concentration of 1 g / L.

[0090] 3) 1.5 L of 1 g / L vermiculite nanosheet solution and 0.07 g of polyquaternium-16 were ultrasonically stirred for 2 h, and then 1 L of 1 g / L graphene oxide was added and stirred for 2 h, vacuum filtered, and dried to obtain a self-assembled complex of graphene oxide and vermiculite sheets.

[0091] 4) Take 1g of the vermiculite-graphene oxide self-assembled complex, press it into a round cake with a diameter of 2cm under a pressure of 10MPa for 1min, and then sinter it at 700℃ for 5h. Wrap the sintered sample with nickel foam and fix it on a 2mm metal molybdenum wire collector with a 0.3mm molybdenum wire as the cathode. A graphite rod with a diameter of 15mm is used as the anode.

[0092] 5) Before the electrochemical reaction begins, dry the mixed molten salt of MgCl2, NaCl and KCl (according to the molar mass ratio of Mg:Na:K=0.508:0.271:0.221) at 250°C for 24h to remove the moisture in the molten salt, then place the inorganic salt in a zirconia crucible, and then place the zirconia crucible in the reactor. The electrochemical reaction adopts a double electrode mode, suspends the cathode and anode above the chloride salt, closes the reactor, and continuously introduces argon into the reactor through the air inlet on the reactor and discharges it through the air outlet to form an argon atmosphere in the reactor. Heat the reactor to 660°C, melt the inorganic salt, and form a molten salt as an electrolyte. Then insert the cathode and anode into the molten salt to form a double electrode system, apply a voltage of 2.6V between the two electrodes, and electrolyze at constant voltage for 6h to obtain the cathode after electrolysis, which is then taken out and cooled. The cooled cathode was placed in deionized water to remove the molten salt, then pickled with 100 mL 2M hydrochloric acid for 5 h, 100 mL 2 wt % hydrofluoric acid for 10 min, then washed with ultrapure water until neutral, and vacuum dried to obtain a silicon / graphene nanocomposite material.

[0093] The self-assembled composite formed by graphene oxide and vermiculite flakes was electrolyzed at a constant voltage of 2.6 V, and the X-ray diffraction spectrum (XRD) showed that the product consisted of graphite, nano-silicon and silicon carbide. Compared with Example 5, the results show that the electrolysis voltage is crucial to the composition of the product.

[0094] Example 7

[0095] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0096] 1) Add 1g of natural fine flake graphite to a beaker containing 23mL of 98% concentrated sulfuric acid, perform magnetic stirring in an ice water bath below 15°C, and slowly add 3g of potassium permanganate during the stirring process, and keep the reaction in the ice water bath for 2h. Then, raise the temperature of the reaction system to 35°C under stirring conditions and maintain it for 30min. During the stirring process, add a certain amount of deionized water at a uniform rate to control the reaction temperature below 98°C until the temperature of the reaction system no longer rises. Continue stirring for 30min, then add an appropriate amount of 5% H2O2 until no bubbles are generated in the system, and filter while hot. Wash the sample with appropriate amounts of 5% HCl and ultrapure water in turn until it is neutral, and there is no The filter cake was placed in a vacuum drying oven at 60°C and vacuum dried to obtain graphite oxide. The dried graphite oxide was then dispersed in deionized water and ultrasonically dispersed at 200W for 1 hour to prepare a graphene oxide solution with a concentration of 1g / L. The average thickness of the graphene oxide sheet was about 1.3nm.

[0097] 2) 10g of kaolinite is soaked in 25mL of 15% potassium acetate solution and mixed and stirred for 2h. The stirred solution is placed in a 250mL agate ball mill with a ball-to-material ratio of 6:1. The grinding ball diameter is 1mm:2mm:3mm (3:2:1) and ground in a planetary ball mill at a speed of 350rpm for 2h. The ground slurry is then poured out and filtered for separation. The composite is washed with water to remove potassium acetate, and then dried and ground to obtain kaolinite nanosheets with a thickness of 1 to 2nm. The kaolinite flakes are dispersed in deionized water and ultrasonically dispersed at a power of 200W for 1h to prepare a kaolinite nanosheet solution with a concentration of 1g / L.

[0098] 3) 1.5 L of 1 g / L kaolinite solution and 0.07 g of polyquaternium-16 were stirred for 2 h, and then 1 L of 1 g / L graphene oxide was added and stirred for 2 h, vacuum filtered, and dried to obtain a self-assembled complex of graphene oxide and kaolinite sheets.

[0099] 4) Take 1g of the self-assembled composite of graphene oxide and kaolinite sheets, press it into a round cake with a diameter of 2cm under a pressure of 10MPa for 1min, and then sinter it at 700℃ for 5h. Wrap the sintered sample with nickel foam and fix it on a 2mm metal molybdenum wire collector with a 0.3mm molybdenum wire as the cathode. A graphite rod with a diameter of 15mm is used as the anode.

[0100] 5) Before the electrochemical reaction begins, dry the mixed molten salt of MgCl2, NaCl and KCl (according to the molar mass ratio of Mg:Na:K=0.508:0.271:0.221) at 250°C for 24h to remove the moisture in the molten salt, then place the inorganic salt in a zirconia crucible, and then place the zirconia crucible in the reactor. The electrochemical reaction adopts a double electrode mode, suspends the cathode and anode above the chloride salt, closes the reactor, and continuously introduces argon into the reactor through the air inlet on the reactor and discharges it through the air outlet to form an argon atmosphere in the reactor. Heat the reactor to 660°C, melt the inorganic salt, and form a molten salt as an electrolyte. Then insert the cathode and anode into the molten salt to form a double electrode system, apply a voltage of 2.4V between the two electrodes, and electrolyze at constant voltage for 6h to obtain the cathode after electrolysis, which is then taken out and cooled. The cooled cathode was placed in deionized water to remove the molten salt, and then acid-washed with 100 mL of 2M hydrochloric acid for 5 h, and then washed with ultrapure water until neutral, and vacuum-dried to obtain a silicon / graphene nanocomposite material.

[0101] The products of the electrochemical reduction of the kaolinite-graphene oxide self-assembled complex are silicon and graphite. Under a transmission electron microscope, it can be observed that the graphite and nano-silicon are uniformly composited.

[0102] Example 8

[0103] The silicon-carbon nanocomposite material of the present invention was prepared in the same manner as in Example 1, and then 0.5 g of the silicon / graphite composite material, 0.4 g of artificial graphite and 0.2 g of coated asphalt were mixed evenly in a high shear granulator to form secondary particles, and then transferred to a high-temperature reaction furnace, heated to 900° C. and kept warm for 2 h under nitrogen conditions. After naturally cooling to room temperature, a carbon-coated silicon-carbon nanocomposite material was obtained.

[0104] The tap density of the prepared silicon / carbon nanocomposite material is 1 g cm -3 .

[0105] Comparative Example 9

[0106] Compared with Example 7, Example 9 uses kaolinite nanosheets as raw materials for direct electrochemical reduction without being compounded with graphene oxide. The specific preparation process is as follows:

[0107] 1) 10 g of kaolinite is soaked in 25 mL of a 15% potassium acetate solution and mixed and stirred for 2 h. The stirred solution is placed in a 250 mL agate ball mill with a ball-to-material ratio of 6:1. The grinding balls are mixed in a ratio of 1 mm:2 mm:3 mm in diameter (3:2:1). The mixture is ground in a planetary ball mill at a speed of 350 rpm for 2 h. The ground slurry is then poured out and filtered for separation. The composite is washed with water to remove potassium acetate, and then dried and ground to obtain kaolinite nanosheets with a thickness of 1 to 2 nm.

[0108] 2) Take 0.6g of kaolinite nanosheets, press them into a round cake with a diameter of 2cm under a pressure of 10MPa for 1min, and then sinter them at 700℃ for 5h. Wrap the sintered sample with nickel foam and fix it on a 2mm metal molybdenum wire collector with a 0.3mm molybdenum wire as the cathode. A graphite rod with a diameter of 15mm is used as the anode.

[0109] 5) Before the electrochemical reaction begins, dry the mixed molten salt of MgCl2, NaCl and KCl (according to the molar mass ratio of Mg:Na:K=0.508:0.271:0.221) at 250°C for 24h to remove the moisture in the molten salt, then place the inorganic salt in a zirconia crucible, and then place the zirconia crucible in the reactor. The electrochemical reaction adopts a double electrode mode, suspends the cathode and anode above the chloride salt, closes the reactor, and continuously introduces argon into the reactor through the air inlet on the reactor and discharges it through the air outlet to form an argon atmosphere in the reactor. Heat the reactor to 660°C, melt the inorganic salt, and form a molten salt as an electrolyte. Then insert the cathode and anode into the molten salt to form a double electrode system, apply a voltage of 2.4V between the two electrodes, and electrolyze at constant voltage for 6h to obtain the cathode after electrolysis, which is then taken out and cooled. The cooled cathode was placed in deionized water to remove the molten salt, and then acid-washed with 100 mL of 2M hydrochloric acid for 5 h, and then washed with ultrapure water until neutral, and vacuum-dried to obtain the final product.

[0110] The final products of the kaolinite nanosheets after electrochemical reduction are mainly silicon, amorphous silicon oxide and aluminum silicate. Compared with Example 7, the reduction degree of this example is lower, indicating that the composite of graphite is beneficial to improving the efficiency of electrochemical reduction of kaolinite.

[0111] Application Example 1

[0112] A method for preparing a silicon-carbon nanocomposite material using clay minerals comprises the following steps:

[0113] The silicon-carbon nanocomposites obtained in Examples 1 to 8 were used as negative electrode materials for lithium-ion batteries, and CR2032 button cells were assembled to evaluate their lithium storage performance. The obtained active material, acetylene black, and sodium alginate were mixed evenly in a mass ratio of 8:1:1, coated on copper foil, vacuum dried at 80°C for 10 hours, and cut into discs with a diameter of 12 mm as working electrodes. Metal lithium sheets were used as counter electrodes, and the electrolyte consisted of 1 mol / L LiPF6+

[0114] 89wt%EC / DEC (1:1, Vol)+10wt%FEC+1wt%VC additive composition. The battery assembly process was carried out in an argon glove box, and the water and oxygen contents were both less than 0.1ppm.

[0115] Figure 2 The carbon-coated silicon / graphite nanocomposite prepared in Example 8 was heated to 0.5 Ag. -1 Cyclic performance diagram under current density (the first three cycles are at 0.1A -1 The results showed that the obtained material has excellent lithium storage performance and cycle stability at 0.5A g -1 After 500 cycles, the specific capacity is 498 mAh g -1 , the capacity retention rate is 77%. This shows that it has broad application prospects in the field of lithium-ion batteries.

[0116] In summary, the present invention provides a new method for preparing high-performance silicon-carbon nanocomposites at low cost. Using natural layered mineral graphite and clay minerals as raw materials, the layered materials are peeled off from top to bottom to obtain a single-layer or few-layer two-dimensional nanomaterial, and a uniformly composite graphite / clay mineral composite precursor is constructed by self-assembly, and then the silicon element in the clay mineral is reduced to nano-silicon by chemical reduction (metal thermal reduction and electrochemical reduction), and the nano-silicon is in situ grown in the graphite sheet to form a uniformly composite nano-silicon and graphite composite material. This method uses abundant and low-priced natural minerals of graphite and clay minerals as raw materials, fully utilizes the layered structure and elemental properties (rich in silicon) of clay minerals, solves the problem of uneven composite of graphite and nano-silicon, simplifies the nano-silicon / graphite composite preparation process, effectively avoids the use of high-cost nano-silicon as a raw material for silicon-carbon composites, and greatly reduces the cost of preparing silicon / graphite composites. Compared with the traditional mechanical mixing method, the self-assembly method can achieve the structural and composition regulation of the clay mineral and graphite sheet complex, the complex is more uniform, and the batch stability of the product is higher. In addition, the silica-containing precursor is preferentially compounded with graphite. During the chemical reduction process, graphite also has the following advantages: ① Graphite can be used as a carbon source, and silicon carbide is generated at the position where the graphite is in close contact with the clay mineral sheet. The in-situ generated silicon carbide can be used as a rivet to tightly connect the silicon and graphite sheets to form a mechanically stable ternary complex; ② During the electrochemical reduction process, since graphite has excellent conductivity, the introduction of graphite sheets can improve the conductivity of the complex and further improve the electroreduction efficiency. The obtained silicon-carbon nanocomposite material has good structural stability and conductivity and can be widely used in lithium-ion batteries.

[0117] The above description is not intended to impose any form of limitation on the present invention. Although the present invention has been disclosed through the above embodiments, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite, characterized in that: The method comprises the following steps: Using graphite and layered clay minerals as precursors, graphite nanosheet solution and clay mineral nanosheet solution are obtained by exfoliating graphite and layered clay minerals, respectively; Then, the graphite nanosheet solution and the clay mineral nanosheet solution obtained above are mixed evenly in a certain ratio, vacuum filtered, dried and self-assembled to form a clay mineral-graphite composite; Then, the clay mineral-graphite composite is used as raw material to obtain silicon-carbon nanocomposite material through chemical reduction method.

2. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 1, characterized in that: The graphite exfoliation method includes at least one of a mechanical exfoliation method, an organic solvent ultrasonic method, a surfactant ultrasonic method, an ionic liquid ultrasonic method, and an oxidation-exfoliation method; the oxidation in the oxidation-exfoliation method step includes at least one of a Brodie method, a Hummers method, an improved Hummers method, and a Staudenmaier method; the exfoliation in the oxidation-exfoliation method step includes at least one of an ultrasonic dispersion method and an electrostatic repulsion dispersion method.

3. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 1, characterized in that: The layered clay mineral includes at least one of montmorillonite, kaolinite, vermiculite, talc, black talc, pyrophyllite, saponite, and mica; the stripping method of the clay mineral includes at least one of high-pressure homogenization stripping method, chemical immersion method, grinding stripping method, chemical immersion-grinding stripping method, intercalation-ultrasound method, air flow crushing stripping method, and molten salt stripping method.

4. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 1, characterized in that: The graphite nanosheet solution and the clay mineral nanosheet solution are mixed in a mass ratio of graphite to clay mineral of 1:0.5-10; the clay mineral nanosheet is organically modified to make the surface of the clay mineral nanosheet positively charged, so that the graphite nanosheet with negative charge on the surface and the clay mineral nanosheet with positive charge on the surface are self-assembled through electrostatic action to achieve uniform composite of clay mineral and graphite; the clay mineral nanosheet organic modifier is an organic cation, including one or more of polyalkyl quaternary ammonium salt, alkyl pyridinium salt and alkyl amine salt.

5. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 1, characterized in that: The chemical reduction method includes a metal thermal reduction method or an electrochemical reduction method; the metal thermal reduction method is: a clay mineral-graphite composite, a metal reducing agent, and an inorganic salt are uniformly mixed in a certain proportion, the mixture is heated to a certain temperature, and reacted for a period of time under inert gas conditions; after natural cooling, the reaction by-products are removed by acid washing, and then washed with ultrapure water until the pH is neutral, and dried under vacuum conditions to obtain a silicon-carbon nanocomposite material.

6. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 5, characterized in that: In the metal thermal reduction method, the metal reducing agent is at least one of magnesium, sodium, zinc, aluminum, and iron; the inorganic salt is at least one of alkali metal or alkaline earth metal salts; the inorganic salt is at least one of sodium chloride, magnesium chloride, calcium chloride, aluminum chloride, sodium nitrate, and potassium nitrate; the clay mineral-graphite composite, the metal reducing agent, and the inorganic salt are mixed in a quantitative ratio of 1:0.5 to 5:1 to 10; the reaction temperature of the mixture is 250 to 900° C., and the reaction time is 1 to 10 hours; the pickling includes at least one of hydrochloric acid, nitric acid, sulfuric acid, and hydrofluoric acid.

7. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 5, characterized in that: The electrochemical reduction method comprises: compacting the clay mineral-graphite composite into pellets and fixing them on a molybdenum wire as a cathode, using a graphite rod as an anode, and using a double-electrode device for electrolysis; the electrode device is first placed above a corundum crucible containing an inorganic salt, and after the inorganic salt is heated to a certain temperature, the electrode is inserted, and constant voltage electrolysis is performed for a period of time; The entire electrolysis process is carried out in a stainless steel container and an inert protective gas is introduced; after the electrolysis is completed, the electrolysis product is taken out from the molten salt and naturally cooled to room temperature; finally, the electrolysis product is acid-washed, washed with ultrapure water to neutrality, and vacuum-dried to obtain a silicon-carbon nanocomposite material.

8. A method for preparing a silicon-carbon nanocomposite material based on a clay mineral-graphite composite as claimed in claim 7, characterized in that: The inorganic salt in the electrochemical reduction method is at least one of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, lithium chloride, and cesium chloride; the melting point of the mixed inorganic salt is lower than 700°C; the temperature at which the inorganic salt is heated should be higher than the melting point of the molten salt, and the temperature at which the inorganic salt is heated is 300-700°C; the constant electrolysis voltage range of the clay mineral-graphite composite is 2-4V, and the electrolysis time is 1-20h; the inert gas is at least one of nitrogen, argon, and helium; the acid solution in the pickling process is at least one of hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid.

9. A silicon-carbon nanocomposite material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8; In order to further improve the structural stability of the silicon-carbon nanocomposite material, the prepared silicon-carbon nanocomposite material is coated with a carbon layer to reduce the side reaction between the electrolyte and nano-silicon, so as to further improve the cycle stability of the electrode, specifically: The silicon-carbon nanocomposite material prepared according to the above method and the coating agent are fully mixed to form secondary particles, the coating agent is added in an amount of 1 to 50 wt% of the mixture of the silicon-carbon nanocomposite material and the coating agent, and then heated to 400 to 1200° C., reacted for 1 to 10 hours, and naturally cooled to room temperature to obtain a carbon-coated silicon-carbon nanocomposite material; The coating agent includes one or more of asphalt, phenolic resin, furfural resin, coumarone resin, and dopamine hydrochloride.

10. A silicon-carbon nanocomposite material as claimed in claim 9, characterized in that: The silicon-carbon nanocomposite material is applied in lithium-ion batteries.

Citation Information

Patent Citations

  • Carbon coated core shell structure nano-silicon / graphene composite anode material and preparation method thereof

    CN107611394A

  • Core-shell graphene-silicon composite material, preparation method thereof, electrode material and battery

    CN110112380A

  • Method for preparing silicon carbide nano material and silicon carbide-containing nano composite material by using clay minerals and application

    CN110844907A

  • Preparation method of high-specific-capacity multi-sheet stacked silicon-carbon composite material

    CN111370665A

  • Method for preparing silicon-carbon nano composite material by using black talc, product and application

    CN113809306A