Positive electrode slurry, positive electrode plate and preparation method thereof

By adding 2-methylaminoethanol and polyethyleneimine to the preparation of the positive electrode slurry, and using the synergistic effects of DMAE and PEI to inhibit NMP hydrolysis, the color of the positive electrode slurry is not pure white and the particle size is small. The problem of glue reaction has achieved the improvement of dispersion and fluidity, and has increased the production capacity of lithium batteries.

CN119092708APending Publication Date: 2024-12-06HUZHOU NANMU-NANO SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208004.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the preparation of existing positive electrode slurry, the N-methylpyrrolidone solution is prone to yellowing, resulting in impure white color, and the nano-scale LATP particle size is prone to gel reaction, affecting the coating efficiency and quality.

Method used

Add 2-methylaminoethanol and polyethyleneimine to the stirring device and mix it with LATP. By sanding to the target particle size, combined with the synergistic effect of DMAE and PEI, the hydrolysis of NMP molecules is inhibited and the premixed slurry will be avoided yellowing and agglomeration. , a positive electrode slurry with good dispersion and good fluidity is formed.

Benefits of technology

Significantly inhibit the hydrolysis of NMP molecules, avoid yellowing of premixed slurry, improve customer satisfaction, reduce gel reaction, obtain positive electrode slurry with no discoloration, non-aggregation and fluidity, and improve coating efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092708A_ABST
    Figure CN119092708A_ABST
Patent Text Reader

Abstract

The invention relates to the field of lithium ion batteries, in particular to positive electrode slurry, a positive electrode plate and a preparation method thereof. A preparation method of the positive electrode slurry comprises the following steps: S1, placing N-methyl pyrrolidone in a stirring device, adding LATP and stirring, then respectively adding 2-methylaminoethanol and polyethyleneimine, continuously stirring for a period of time, and sanding until LATP reaches a target particle size to obtain premixed slurry; and S2, mixing the premixed slurry with a positive electrode material, a conductive agent and an adhesive to prepare the positive electrode slurry. The positive pole piece is coated with the positive pole slurry. The 2-methylaminoethanol and the polyethyleneimine are added in the sanding process of the LATP, the two substances have a synergistic effect, so that hydrolysis of the N-methyl pyrrolidone is inhibited, gel reaction during homogenization is avoided, and the obtained positive electrode slurry is free of discoloration and agglomeration, good in dispersity, excellent in fluidity and good in coating property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a positive electrode slurry, a positive electrode sheet and a preparation method thereof. Background Art

[0002] Lithium Aluminum Titanium Phosphate (LATP) 1+x Al x Ti 2-x (PO4)3) is a NASICON type solid electrolyte material with excellent ionic conductivity and stable chemical properties. Therefore, it is widely used in positive electrode slurry in lithium-ion batteries. It can provide higher battery safety and cycle life, and also has higher electrochemical stability and cycle performance, which can effectively reduce the potential safety hazards of lithium batteries during charging and discharging, and improve the service life of the battery. In the prior art, generally, micron-sized LATP powder is first dispersed in an organic solution of N-methylpyrrolidone (NMP), and then the particle size of LATP is reduced to nanometer level by a sand mill, and then compounded with other ingredients to form a positive electrode slurry. In practice, the applicant found that the NMP solution of LATP is very easy to turn yellow during the sand milling process. The main reason for the yellowing is that NMP is hydrolyzed and the hydrolysis product undergoes polymerization to generate amide or ester polymers, and the longer the sand milling time, the more serious the yellowing phenomenon. Although it is not clear whether the yellowing phenomenon has an adverse effect on the positive electrode slurry and positive electrode sheet, customers generally require the color to be pure white, so it is necessary to improve the existing preparation method of the positive electrode slurry to avoid the yellowing phenomenon and improve customer satisfaction. In addition, when LATP is used in the preparation of high-nickel ternary positive electrode materials, the smaller the particle size, the easier it is for the slurry to undergo a gel reaction, resulting in poor slurry fluidity and affecting the efficiency and quality of coating.

[0003] To this end, this application is filed. Summary of the invention

[0004] In view of the problems mentioned in the background technology, the present invention discloses a positive electrode slurry, a positive electrode sheet and a preparation method thereof.

[0005] The present invention is achieved through the following technical solutions:

[0006] On the one hand, the present invention provides a method for preparing a positive electrode slurry, comprising the following steps:

[0007] S1. Place N-methylpyrrolidone in a stirring device, add LATP and stir, then add 2-methylaminoethanol and polyethyleneimine respectively, continue stirring for a period of time, and then sand grind until LATP reaches the target particle size to obtain a premixed slurry;

[0008] S2. Mix the premixed slurry with a positive electrode material, a conductive agent, and a binder to prepare a positive electrode slurry.

[0009] The addition of 2-methylaminoethanol (also known as 2-dimethylethanolamine, DMAE) and polyethyleneimine (PEI) can inhibit the hydrolysis of NMP molecules to a certain extent, but the inhibitory effect is limited, and a large amount of addition is required to obtain a significant inhibitory effect. Moreover, PEI has a strong flocculation effect, and a large amount of addition will cause LATP to agglomerate, especially when LATP is nanometer-sized, the agglomeration phenomenon is more serious. The applicant unexpectedly found that when the two substances are added at the same time, the liquid layer of the obtained premixed slurry is light milky white after sedimentation, and it will not turn yellow even if it is left for 10 days, and LATP has good dispersibility and no obvious agglomeration phenomenon. The reason for this is that the applicant speculates that: as the sand milling proceeds, the particle size of LATP becomes smaller, and the number of active sites exposed on the surface increases. These active sites promote the hydrolysis of NMP molecules, and DMAE and PEI are combined with the active sites after addition, reducing the contact between the active sites and the NMP molecules, thereby inhibiting the hydrolysis of NMP molecules. Due to the different molecular structures of DMAE and PEI, the amino groups contained in them have different binding forces with the active sites. The combined use of the two substances helps to maximize the combination with the active sites, thereby significantly inhibiting the hydrolysis of NMP molecules and avoiding the yellowing of the premixed slurry; moreover, the amount of DMAE and PEI can be significantly reduced. An appropriate amount of PEI can avoid the occurrence of gel reaction during homogenization and will not cause LATP agglomeration, and finally obtain a positive electrode slurry with good dispersion and good fluidity.

[0010] The operations and parameters of stirring and sand milling involved in the above preparation method are all conventional operations and parameters in the art, and the devices involved are all conventional devices in the art. In this embodiment, stirring uses a planetary mixer, specifically a MOFA-4000; in this embodiment, sand milling uses a dual-power centrifugal sand mill, specifically a NT-V2S.

[0011] Furthermore, in S1, the mass percentage of LATP in N-methylpyrrolidone is 19%-21%, the added amount of 2-methylaminoethanol is 0.05wt%-0.7wt% of LATP, and the added amount of polyethyleneimine is 0.05wt%-0.3wt% of LATP.

[0012] The applicant has found through creative work that the binding force between DMAE and the active sites on the surface of LATP is weak, and the binding force between PEI and the active sites on the surface of LATP is strong. When DMAE and PEI are added simultaneously at 0.05wt%-0.7wt% of LATP and 0.05wt%-0.3wt% of LATP respectively, the hydrolysis of NMP molecules can be significantly inhibited, and the obtained premixed slurry will not change color due to sand grinding, and the occurrence of gel reaction during homogenization can be effectively avoided. The obtained positive electrode slurry does not change color, does not agglomerate, has good fluidity, and has good coating properties without adding NMP to adjust the viscosity. Compared with the prior art that requires the use of a regulator (generally NMP) to adjust the viscosity or solid content before coating, the preparation operation process of the positive electrode sheet is reduced, which helps to improve the preparation efficiency of the positive electrode sheet.

[0013] Furthermore, the addition amount of 2-methylaminoethanol is 0.25wt%-0.5wt% of LATP, and the addition amount of polyethyleneimine is 0.15wt%-0.2wt% of LATP.

[0014] Furthermore, in S1, LATP was added at the micron level and then sand-ground to the nanometer level.

[0015] Furthermore, LATP was added to a D50 of 1-5 μm and sand-milled to a D50 of 200 nm.

[0016] Furthermore, in S2, the positive electrode material is NCM523, the conductive agent is Super P, and the binder is an N-methylpyrrolidone solution of polyvinylidene fluoride.

[0017] NCM523 ternary material (LiNi 0.5 Co 0.2 Mn 0.3 O2) has the advantages of high voltage platform, large specific capacity, good room temperature cycle performance, high energy density and low self-discharge. However, compared with lithium cobalt oxide, its main disadvantage is low conductivity and low compaction density. Therefore, the ion conductive material LATP is introduced to change the reaction kinetics of the slurry.

[0018] It should be noted that: the positive electrode material in the present invention can also be other high-nickel positive electrode materials, such as NCM622, NCM811, nickel cobalt aluminum lithium NCA, etc.; the conductive agent in the present invention can also be other conductive agents, such as acetylene black, Keqin black, graphene, carbon nanotubes, carbon nanowires, KS-6, etc.; the adhesive can also be other adhesives.

[0019] Furthermore, NCM523, Super P, and polyvinylidene fluoride are added in order according to the mass percentage of 94%, 3%, and 3%, the mass percentage of polyvinylidene fluoride in the adhesive is 7%, and the mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and polyvinylidene fluoride.

[0020] Furthermore, in S2, after the premixed slurry is mixed with the positive electrode material, the conductive agent and the adhesive, the solid content of the obtained mixture is first tested, and then N-methylpyrrolidone is added to make the solid content of the final product 60%-63%, with the best solid content being 62%.

[0021] Positive electrode slurry viscosity is too high or too low, which is not conducive to the coating of the pole piece. High viscosity has good dispersibility and is not easy to precipitate, but the leveling effect is not good, which is not conducive to coating; positive electrode slurry viscosity is low and has good fluidity, but poor dispersibility, easy precipitation, and difficult to dry. The drying efficiency of coating is low, and it is also easy to cause coating cracking, slurry particle agglomeration, and poor surface density consistency. Since it takes a long time to homogenize the positive electrode slurry, the slurry has a certain viscosity, so the temperature of the slurry will increase significantly during the homogenization process. Even if there is cooling water to control the temperature, the slurry temperature will still fluctuate. Under this condition, NMP will volatilize to a certain extent, resulting in an increase in the solid content of the slurry. For this reason, after each homogenization, it is necessary to first detect the solid content, and then add NMP to control the solid content to 60%-63%, preferably 62%. The positive electrode slurry within this solid content range has moderate viscosity, good dispersibility, good leveling, high coating and drying efficiency, which is helpful to improve the production capacity of lithium batteries. On the other hand, the present invention proposes a positive electrode slurry prepared according to the above preparation method.

[0022] In addition, the present invention also provides a positive electrode sheet, the surface of which is coated with the positive electrode slurry. The preparation method of the positive electrode sheet is specifically: the positive electrode slurry is stirred evenly, coated on the surface of the aluminum foil, and then dried, rolled, and processed.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. Add DMAE and PEI during LATP sand grinding. The synergistic effect of DMAE and PEI can significantly inhibit the hydrolysis of NMP molecules, avoid yellowing of premixed slurry, and improve customer satisfaction;

[0025] 2. Gel reaction is not easy to occur during homogenization. The obtained positive electrode slurry does not change color, does not agglomerate, has good fluidity, good dispersibility and good leveling, which helps to improve coating efficiency and coating quality and increase the production capacity of lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a comparison diagram of the premixed slurry of Example 2 of the present invention and Comparative Example 1: A is a photograph of the premixed slurry obtained in Example 2 after sedimentation and stratification, B is a photograph of the premixed slurry obtained in Example 2 after being placed for 10 days, C is a photograph of the premixed slurry obtained in Comparative Example 1 after sedimentation and stratification, D is a photograph of the premixed slurry obtained in Comparative Example 2 after sedimentation and stratification, and E is a photograph of the premixed slurry obtained in Comparative Example 3 after sedimentation and stratification.

[0028] Figure 2 It is a schematic diagram of the preparation process of the positive electrode slurry of the present invention. DETAILED DESCRIPTION

[0029] In order to facilitate the understanding of the present invention, the present invention will be described in more detail below, and embodiments of the present invention are given, but the scope of the present invention is not limited thereby.

[0030] All chemical substances involved in the raw materials in the following examples and comparative examples are commercially available. The experimental devices involved in the following examples and comparative examples are all conventional devices in the art. The technical details not described in detail in the following examples and comparative examples are all conventional technical means in the art. In the following examples and comparative examples, LATP D50 is 3 μm, and the adhesive is a 7% by mass PVDF NMP solution.

[0031] Example 1

[0032] A positive electrode slurry, the preparation method of which is as follows:

[0033] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 19%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0034] S2. The premixed slurry is mixed with the positive electrode material NCM523, the conductive agent Super P, and the adhesive PVDF to prepare a positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them in a planetary mixer in the mass percentage of 94%, 3%, and 3% respectively to mix evenly, and then weigh the premixed slurry and add it to the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 63%.

[0035] Example 2

[0036] A positive electrode slurry, the preparation method of which is as follows:

[0037] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0038] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0039] Example 3

[0040] A positive electrode slurry, the preparation method of which is as follows:

[0041] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 21%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0042] S2. The premixed slurry is mixed with the positive electrode material NCM523, the conductive agent Super P, and the adhesive PVDF to prepare a positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them in a planetary mixer in the mass percentage of 94%, 3%, and 3% respectively to mix evenly, and then weigh the premixed slurry and add it to the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 61%.

[0043] Example 4

[0044] A positive electrode slurry, the preparation method of which is as follows:

[0045] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.05%, and the mass percentage of PEI and LATP is 0.18%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0046] S2. The premixed slurry is mixed with the positive electrode material NCM523, the conductive agent Super P, and the adhesive PVDF to prepare a positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them in a planetary mixer in the mass percentage of 94%, 3%, and 3% respectively to mix evenly, and then weigh the premixed slurry and add it to the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 60%.

[0047] Example 5

[0048] A positive electrode slurry, the preparation method of which is as follows:

[0049] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.1%, and the mass percentage of PEI and LATP is 0.18%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0050] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0051] Example 6

[0052] A positive electrode slurry, the preparation method of which is as follows:

[0053] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.25%, and the mass percentage of PEI and LATP is 0.18%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes, and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0054] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0055] Example 7

[0056] A positive electrode slurry, the preparation method of which is as follows:

[0057] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.3%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0058] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0059] Example 8

[0060] A positive electrode slurry, the preparation method of which is as follows:

[0061] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.5%, and the mass percentage of PEI and LATP is 0.18%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes, and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0062] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0063] Example 9

[0064] A positive electrode slurry, the preparation method of which is as follows:

[0065] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.6%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0066] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0067] Example 10

[0068] A positive electrode slurry, the preparation method of which is as follows:

[0069] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.7%, and the mass percentage of PEI and LATP was 0.18%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0070] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0071] Embodiment 11

[0072] A positive electrode slurry, the preparation method of which is as follows:

[0073] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.4%, and the mass percentage of PEI and LATP is 0.05%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes, and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0074] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0075] Example 12

[0076] A positive electrode slurry, the preparation method of which is as follows:

[0077] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.1%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0078] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0079] Embodiment 13

[0080] A positive electrode slurry, the preparation method of which is as follows:

[0081] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.4%, and the mass percentage of PEI and LATP is 0.15%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes, and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0082] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0083] Embodiment 14

[0084] A positive electrode slurry, the preparation method of which is as follows:

[0085] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.2%. The stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0086] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0087] Embodiment 15

[0088] A positive electrode slurry, the preparation method of which is as follows:

[0089] S1. First, NMP is placed in a stirring tank, LATP is added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 minutes, the mass percentage of LATP in NMP is 20%, and then DMAE and PEI are weighed and added to the stirring tank, the mass percentage of DMAE and LATP is 0.4%, and the mass percentage of PEI and LATP is 0.25%. Stirring is continued at a stirring speed of 1500 rpm for 30 minutes, and then sand milling is performed until the D50 of LATP is 200±10 nm. The specific operation of sand milling is: N2 is used as a protective gas, the sand milling speed is 800 r / min, and a premixed slurry with uniform composition is obtained;

[0090] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0091] Example 16

[0092] A positive electrode slurry, the preparation method of which is as follows:

[0093] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.4%, and the mass percentage of PEI and LATP was 0.3%, and the stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0094] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0095] Embodiment 17

[0096] A positive electrode slurry, the preparation method of which is as follows:

[0097] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 19%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.05%, and the mass percentage of PEI and LATP was 0.3%. The stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0098] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0099] Embodiment 18

[0100] A positive electrode slurry, the preparation method of which is as follows:

[0101] S1. First, NMP was placed in a stirring tank, LATP was added to the stirring tank and stirred at a stirring speed of 1500 rpm for 30 min, the mass percentage of LATP in NMP was 20%, and then DMAE and PEI were weighed and added to the stirring tank, the mass percentage of DMAE and LATP was 0.7%, and the mass percentage of PEI and LATP was 0.05%. The stirring was continued at a stirring speed of 1500 rpm for 30 min, and then sand milled until the D50 of LATP was 200±10 nm. The specific operation of sand milling was: N2 was used as the protective gas, the sand milling speed was 800 r / min, and a premixed slurry with uniform composition was obtained;

[0102] S2. The premixed slurry is mixed with positive electrode material NCM523, conductive agent Super P, and adhesive PVDF to prepare positive electrode slurry. The homogenization order is: weigh NCM523, Super P, and PVDF and add them into a planetary mixer in the order of 94%, 3%, and 3% by mass, and then weigh the premixed slurry and add it into the planetary mixer to continue stirring evenly. The added mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and PVDF. After the homogenization is completed, NMP is added and stirred evenly, so that the solid content in the obtained positive electrode slurry is 62%.

[0103] Comparative Example 1

[0104] Compared with Example 2, DMAE and PEI were not added, and the rest were the same as Example 2.

[0105] Comparative Example 2

[0106] Compared with Example 2, DMAE was not added, and the rest was the same as Example 2.

[0107] Comparative Example 3

[0108] Compared with Example 2, PEI was not added, and the rest was the same as Example 2.

[0109] Comparative Example 4

[0110] Compared with Example 2, the addition percentage of DMAE was adjusted from 0.4% to 0.03%, and the rest was the same as Example 2.

[0111] Comparative Example 5

[0112] Compared with Example 2, the addition percentage of DMAE was adjusted from 0.4% to 0.8%, and the rest was the same as Example 2.

[0113] Comparative Example 6

[0114] Compared with Example 2, the addition percentage of PEI was adjusted from 0.18% to 0.04%, and the rest was the same as Example 2.

[0115] Comparative Example 7

[0116] Compared with Example 2, the addition percentage of PEI was adjusted from 0.18% to 0.6%, and the rest was the same as Example 2.

[0117] Comparative Example 8

[0118] Compared with Comparative Example 3, the addition percentage of DMAE was adjusted from 0.4% to 2%, and the rest was the same as Comparative Example 3.

[0119] Comparative Example 9

[0120] Compared with Comparative Example 2, the addition percentage of PEI was adjusted from 0.18% to 1.2%, and the rest was the same as Comparative Example 2.

[0121] The specific technical parameters of each embodiment and comparative example are shown in Table 1.

[0122]

[0123]

[0124] As shown in Table 1:

[0125] (1) By Figure 1 It can be seen that: when DMAE and PEI are not added (Comparative Example 1), the color of the premixed slurry is obviously yellow; when only PEI is added (Comparative Example 2, Comparative Example 9), when the PEI addition amount is 0.18%, the color of the premixed slurry is lighter than that of Comparative Example 1, but still has a light yellow color that can be discerned by the naked eye. This may be because the amount of PEI added is relatively small. Although the hydrolysis of NMP is restricted to a certain extent, it is not completely inhibited. When the PEI addition amount is 1.2%, the color of the premixed slurry is milky white, but it is found that LATP has agglomeration phenomenon in the subsequent process. Even if the sanding time or stirring time is extended, the target particle size distribution cannot be achieved. Only DMAE is added (Comparative Example 3, Comparative Example 8). When the addition amount of DMAE is 0.4%, the color of the premixed slurry is lighter than that of Comparative Example 1, but still has a light yellow color that can be discerned by the naked eye. This may be because the addition amount of DMAE is relatively small. Although the hydrolysis of NMP is limited to a certain extent, it is not completely inhibited. The present application found that when the addition amount of DMAE is increased to 2% (Comparative Example 8, the addition amount of DMAE is 5 times the addition amount of DMAE in Example 2), the color of the premixed slurry is basically close to that of Example 2, and the premixed slurry can achieve the target particle size distribution, and it is basically not yellow after being placed for 10 days. Obviously, in terms of the inhibitory effect on the hydrolysis of NMP, PEI is better than DMAE, but the addition of PEI will cause LATP to agglomerate. The present invention compounds DMAE with PEI, and DMAE and PEI work synergistically, which can significantly reduce the addition amount of PEI, avoid LATP agglomeration, and obtain a good NMP hydrolysis inhibition effect, and obtain a white, non-yellowing premixed slurry.

[0126] (2) As shown in the test results of Example 1 to Example 18: when the mass percentage of LATP in N-methylpyrrolidone is 19%-21%, the addition amount of 2-methylaminoethanol is 0.05wt%-0.7wt% of LATP, and the addition amount of polyethyleneimine is 0.05wt%-0.3wt% of LATP, the obtained premixed slurry is milky white in color, LATP does not agglomerate, and does not turn yellow after being placed for 10 days. Through further testing, the viscosity of the premixed slurries obtained in Example 1 to Example 18 is less than 10cps, which is helpful to prepare a positive electrode slurry with good viscosity and fluidity to obtain a positive electrode slurry with good coating properties.

[0127] (3) As shown in Examples 4 to 7, Example 2, Example 8 to 10, Comparative Example 4 and Comparative Example 5, when other conditions are the same, when the addition amount of DMAE is 0.05%, 0.1%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6% and 0.7%, the viscosity of the premixed slurry is basically unchanged. However, in the specific preparation operation, we found that the addition amount of DMAE will reduce the sand milling efficiency. The larger the addition amount of DMAE, the longer the sand milling time required to obtain the premixed slurry of the target particle size. However, if the addition amount of DMAE is too low, it cannot effectively inhibit the hydrolysis of NMP, and the premixed slurry is light yellow and cannot meet customer requirements. Taking into account the efficiency and effect of the preparation, the preferred addition amount of DMAE is 0.25%-0.5%. (4) As shown in Examples 11-13, 2, 14-16: Under the premise of other conditions being the same, when the addition amount of PEI is 0.05%, 0.1%, 0.15%, 0.18%, 0.2%, 0.25%, 0.3%, the viscosity of the premixed slurry is basically unchanged, but with the increase of the addition amount of PEI, the efficiency of sand milling decreases, and the sand milling time required to obtain the premixed slurry of the target particle size gradually increases, especially when the addition amount of PEI is 0.6%, we detected that the particle size of the premixed slurry during the sand milling process hardly decreased, and D50 remained in the range of 2-3 μm. Considering the efficiency and effect of the preparation, the preferred addition amount of PEI is 0.15%-0.2%.

[0128] Compared with the prior art, the present invention adds DMAE and PEI during LATP sand grinding. The synergistic effect of DMAE and PEI can not only significantly inhibit the hydrolysis of NMP molecules, avoid yellowing of premixed slurry, and improve customer satisfaction, but also make it difficult for gel reaction to occur during homogenization. The obtained positive electrode slurry does not change color, does not agglomerate, and has good fluidity, which helps to reduce the preparation operations of the positive electrode sheet and improve the coating efficiency and coating quality.

[0129] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a positive electrode slurry, characterized in that: The steps are as follows: S1. Place N-methylpyrrolidone in a stirring device, add LATP and stir, then add 2-methylaminoethanol and polyethyleneimine respectively, continue stirring for a period of time, and then sand grind until LATP reaches the target particle size to obtain a premixed slurry; S2. Mix the premixed slurry with a positive electrode material, a conductive agent, and a binder to prepare a positive electrode slurry.

2. The method for preparing the positive electrode slurry according to claim 1, characterized in that: In S1, the mass percentage of LATP in N-methylpyrrolidone is 19%-21%, the added amount of 2-methylaminoethanol is 0.05wt%-0.7wt% of LATP, and the added amount of polyethyleneimine is 0.05wt%-0.3wt% of LATP.

3. The method for preparing the positive electrode slurry according to claim 2, characterized in that: The added amount of 2-methylaminoethanol is 0.25wt%-0.5wt% of LATP, and the added amount of polyethyleneimine is 0.15wt%-0.2wt% of LATP.

4. The method for preparing the positive electrode slurry according to claim 1, characterized in that: In S1, LATP was added at the micron level and then sand-ground to the nanometer level.

5. The method for preparing the positive electrode slurry according to claim 4, characterized in that: When LATP was added, the D50 was 1-5 μm, and it was sand-milled to a D50 of 200 nm.

6. The method for preparing the positive electrode slurry according to claim 1, characterized in that: In S2, the positive electrode material is NCM523, the conductive agent is Super P, and the adhesive is an N-methylpyrrolidone solution of polyvinylidene fluoride.

7. The method for preparing the positive electrode slurry according to claim 6, characterized in that: NCM523, Super P, and polyvinylidene fluoride are added in order of 94%, 3%, and 3% by mass. The mass of the premixed slurry is 1% of the total mass of NCM523, Super P, and polyvinylidene fluoride. The mass percentage of polyvinylidene fluoride in the adhesive is 7%.

8. The method for preparing positive electrode slurry according to claim 1, characterized in that: In S2, after the premixed slurry is mixed with the positive electrode material, the conductive agent and the adhesive, the solid content of the obtained mixture is first tested, and then N-methylpyrrolidone is added to make the solid content of the final product be 60%-63%.

9. A positive electrode slurry prepared by the preparation method according to any one of claims 1 to 8.

10. A positive electrode plate, characterized in that: Coated with the positive electrode slurry as claimed in claim 8.