Preparation method of trench type catalyst layer membrane electrode of fuel cell
Through the preparation of the trench-type catalytic layer membrane electrode, a high-efficiency catalytic layer is formed using soft template technology and resin combination coating process, which solves the problem of low efficiency of the catalytic layer structure of traditional fuel cells and realizes gas-water transmission under high current density and Improved reaction efficiency.
Patent Information
- Application Number
- CN202410986519.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-12-06
AI Technical Summary
The complex disordered structure of the catalytic layer of traditional fuel cell limits the gas-water transmission efficiency of the electrode and the utilization rate of the catalyst, making it difficult to meet the needs of high power density and rapid reaction kinetics, especially at high current density water accumulation and low gas transmission efficiency.
The trench-type catalytic layer film electrode preparation method is adopted to prepare ridge-shaped and grooved structures through soft template technology, and a combination of short-chain and long-chain resin is used to form an efficient trench-type catalytic layer, and transfer it to On the proton exchange membrane, the PTFE protective layer is combined with the stability and drainage capacity of the catalytic layer.
The catalytic active area and reaction sites are significantly improved, the diffusion efficiency of protons and gas is enhanced, the gas-water transmission efficiency under high current density is ensured, and the overall performance of the membrane electrode is improved.
Smart Images

Figure CN119092721A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a method for preparing a grooved catalyst layer membrane electrode for a fuel cell. Background Art
[0002] As an efficient and clean energy conversion device, fuel cells have been widely used in energy fields such as automobiles, mobile power stations, portable power sources, and aerospace. The membrane electrode is a key component for electrochemical reactions, and its performance directly affects the overall efficiency and life of the battery. In terms of the structural design of the membrane electrode, the catalyst layer of the traditional proton exchange membrane fuel cell is composed of carbon-supported platinum and ionomers, which are mixed in a slurry and deposited on the membrane surface through spraying, coating and other processes to form a porous electrode. This complex and disordered catalytic layer structure of the pore network limits the gas-water transmission efficiency of the electrode and reduces the utilization rate of the catalyst, making it difficult to meet the requirements of high power density and fast reaction kinetics;
[0003] Patent publication number CN118016920A discloses a fuel cell membrane electrode with a grooved catalyst layer and a preparation method thereof, wherein the catalyst layer is directly coated on a polytetrafluoroethylene membrane with a certain groove structure, and then the orderly arranged grooved catalyst layer is transferred to the proton exchange membrane by hot pressing transfer;
[0004] The catalyst layer prepared by the above-mentioned fuel cell membrane electrode with a grooved catalyst layer and its preparation method has uniform ionomer content in the ridge structure and grooves, and the grooves with high ionomer content show higher hydrophilicity. Under actual operating conditions of high current density, a large amount of generated water at the cathode is easily accumulated in the grooves and cannot be discharged, thereby hindering the rapid transmission of the reaction gas in the grooves, and at the same time affecting the lateral diffusion of the reaction gas to the ridge structure reaction sites, thereby greatly reducing the catalytic and mass transfer efficiency under high current density. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a grooved catalyst layer membrane electrode for a fuel cell.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a grooved catalyst layer membrane electrode for a fuel cell comprises the following steps:
[0008] S1: coating and curing the prepared soft template, treating it to increase wettability, processing grooves using micro-nano technology, and then performing secondary curing;
[0009] S2: Use short-chain resin with high I / C to prepare coating slurry, apply it to the soft template through slit coating and dry it to form a ridge structure;
[0010] S3: Spray slurry was prepared using long-chain resin with low I / C and sprayed onto the soft template by ultrasonic spraying to cover the ridge structure as grooves;
[0011] S4: Laminating the proton exchange membrane and the catalyst layer, hot pressing under PTFE protection, and transferring the catalyst layer to the proton exchange membrane;
[0012] S5: Spraying of the catalyst layer on the anode side, bonding of the gas diffusion layer, and packaging into a membrane electrode.
[0013] Preferably, the soft film board in step S1 comprises the following steps during preparation:
[0014] S11: Weigh Sylgard 184 (PDMS) and curing agent, and mix them evenly in a ratio of 10:1;
[0015] S12: placing the mixed PDMS in a vacuum degassing machine and degassing at a speed of 15000 RPM for 30 min to remove bubbles generated during the mixing process;
[0016] S13: taking the silicon wafer substrate and using isopropyl alcohol and deionized water for ultrasonic cleaning respectively, and drying and setting aside for later use;
[0017] S14: The degassed PDMS is evenly coated on the silicon wafer substrate with a thickness of 1 mm, and the coated silicon wafer is placed in an oven at 60° C. for 4 hours;
[0018] S15: Use an oxygen plasma processor to treat the PDMS surface to increase the adhesion of the subsequent catalyst slurry. The treatment time is controlled at 3 minutes and the power is set to 50W;
[0019] S16: Fabrication of microscale grooves on the PDMS surface using a laser direct writing system;
[0020] S17: After processing, the PDMS surface is rinsed and cleaned with isopropyl alcohol to remove the residues that may be generated during the processing;
[0021] S18: The PDMS was post-cured in an oven at 80°C for 2 hours for secondary curing to ensure its mechanical stability.
[0022] Further: the method for preparing the ridge structure in step S2 comprises the following steps:
[0023] S21: Weigh 3.50 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 17.26 g of deionized water and stir thoroughly to wet;
[0024] S22: 14.92 g of perfluorosulfonic acid resin DFPSA-2179 (10 wt%) was slowly added dropwise during stirring, and 4.26 g of n-propanol was added after mixing, and magnetic stirring was performed for 30 min;
[0025] S23: High-speed shearing at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, the pre-dispersed slurry is put into a homogenizer, homogenized at 800 Bar pressure for 3 times, and then transferred to a vacuum degassing machine for degassing;
[0026] S24: A platform-type slot extrusion sheet coating machine is used, and the platform drying temperature is set at 60°C to coat the treated coating slurry on the soft template.
[0027] Further: the ridge structure in step S3 is covered with a low hydrophilic groove, comprising the following steps:
[0028] S31: Weigh 0.60 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 5.31 g of deionized water and stir thoroughly to wet, and slowly drop 3.84 g of perfluorosulfonic acid resin D520CS (5 wt%) while stirring;
[0029] S32: After mixing, add 26.24 g of ethanol, stir with a magnetic stirrer for 30 min, high-speed shear at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, and ultrasonicate the pre-dispersed slurry in a water bath at 10°C for 1 h;
[0030] S33: Using platform ultrasonic spraying equipment, the platform drying temperature is set at 90°C, and the treated spray slurry is coated on the above catalyst layer to complete the construction of the entire grooved catalyst layer. The Pt loading is controlled at 0.30 mg / cm 2 .
[0031] As a preferred solution of the present invention: the transfer of the grooved catalytic layer in step S4 comprises the following steps:
[0032] S41: The proton exchange membrane uses a 12-micron membrane, cuts the proton exchange membrane and PTFE protective layer of appropriate size, covers the proton exchange membrane on the catalyst layer side of the soft template, fits and discharges the air, and fits the PTFE protective layer on both sides of the composite membrane material;
[0033] S42: Set the temperature and pressure of the hot press, the platform temperature is controlled at 140℃, and the pressure is controlled at 5kN / m 2 , put the sample into the hot press and keep the pressure for 3 minutes;
[0034] S43: After the hot pressing is completed, the sample is taken out, and after the sample is cooled, the soft template is peeled off from the composite membrane material, and the catalytic layer is transferred from the soft template to the proton exchange membrane.
[0035] As a further solution of the present invention: the membrane electrode preparation comprises the following steps:
[0036] 1: Use the above-mentioned spray slurry as the anode slurry and use a platform ultrasonic spraying device to spray 0.08 mg / cm on the cathode grooved catalyst layer half CCM. 2 A platinum-loaded anode catalyst layer;
[0037] 2: The gas diffusion layers are attached to both sides and packaged into membrane electrodes.
[0038] As a further solution of the present invention: the width of the micro-scale grooves in step S16 is 10 microns, the spacing is 20 microns, and the depth is 15 microns.
[0039] Based on the above scheme: the dry film thickness in step S24 is controlled at 13 microns.
[0040] Based on the above scheme: the dry film thickness in step S33 is controlled at 4 microns.
[0041] Based on the above scheme: the thickness of the PTFE protective layer in step S41 is 40 microns.
[0042] The beneficial effects of the present invention are:
[0043] 1. A method for preparing a grooved catalyst layer membrane electrode for a fuel cell, which adopts a grooved catalyst layer structure design, significantly increases the effective catalytic activity area of the membrane electrode, provides more reaction sites, separates proton flow and oxygen flow, and improves diffusion efficiency;
[0044] 2. A method for preparing a grooved catalyst layer membrane electrode for a fuel cell, wherein the grooved ridge structure is mixed with a short-chain resin with a high I / C value to enhance the proton transfer capacity.
[0045] 3. A method for preparing a grooved catalyst layer membrane electrode for a fuel cell, wherein the I / C value is reduced at the bottom of the groove, a long-chain resin is used, the drainage capacity of the catalyst layer is optimized, and good gas-water transmission efficiency is ensured under high current density conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic flow chart of a method for preparing a grooved catalyst layer membrane electrode for a fuel cell proposed by the present invention;
[0047] Figure 2 It is a structural schematic diagram of the preparation process of a grooved catalytic layer of a fuel cell grooved catalytic layer membrane electrode preparation method proposed by the present invention;
[0048] Figure 3It is a comparison diagram of polarization curves of an embodiment and a comparative example of a method for preparing a grooved catalyst layer membrane electrode for a fuel cell proposed by the present invention;
[0049] Figure 4 It is a comparison diagram of EIS impedance spectra of an embodiment of a method for preparing a grooved catalyst layer membrane electrode for a fuel cell proposed by the present invention and a comparative example. DETAILED DESCRIPTION
[0050] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.
[0051] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0052] Embodiment 1:
[0053] A method for preparing a grooved catalyst layer membrane electrode for a fuel cell, such as Figure 1 to Figure 2 As shown, the following steps are included:
[0054] S1: coating and curing the prepared soft template, treating it to increase wettability, processing grooves using micro-nano technology, and then performing secondary curing;
[0055] S2: Use short-chain resin with high I / C to prepare coating slurry, apply it to the soft template through slit coating and dry it to form a ridge structure;
[0056] S3: Spray slurry was prepared using long-chain resin with low I / C and sprayed onto the soft template by ultrasonic spraying to cover the ridge structure as grooves;
[0057] S4: Laminating the proton exchange membrane and the catalyst layer, hot pressing under PTFE protection, and transferring the catalyst layer to the proton exchange membrane;
[0058] S5: Spraying of the catalyst layer on the anode side, bonding of the gas diffusion layer, and packaging into a membrane electrode.
[0059] The soft film board in step S1 includes the following steps during the preparation process:
[0060] S11: Weigh Sylgard 184 (PDMS) and curing agent, and mix them evenly in a ratio of 10:1;
[0061] S12: placing the mixed PDMS in a vacuum degassing machine and degassing at a speed of 15000 RPM for 30 min to remove bubbles generated during the mixing process;
[0062] S13: taking the silicon wafer substrate and using isopropyl alcohol and deionized water for ultrasonic cleaning respectively, and drying and setting aside for later use;
[0063] S14: The degassed PDMS is evenly coated on the silicon wafer substrate with a thickness of 1 mm, and the coated silicon wafer is placed in an oven at 60° C. for 4 hours;
[0064] S15: Use an oxygen plasma processor to treat the PDMS surface to increase the adhesion of the subsequent catalyst slurry. The treatment time is controlled at 3 minutes and the power is set to 50W;
[0065] S16: Microscale grooves were prepared on the PDMS surface using a laser direct writing system, with a groove width of 10 μm, a spacing of 20 μm, and a depth of 15 μm;
[0066] S17: After processing, the PDMS surface is rinsed and cleaned with isopropyl alcohol to remove the residues that may be generated during the processing;
[0067] S18: The PDMS was post-cured in an oven at 80°C for 2 hours for secondary curing to ensure its mechanical stability.
[0068] The method for preparing the ridge structure in step S2 comprises the following steps:
[0069] S21: Weigh 3.50 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 17.26 g of deionized water and stir thoroughly to wet;
[0070] S22: 14.92 g of perfluorosulfonic acid resin DFPSA-2179 (10 wt%) was slowly added dropwise during stirring, and 4.26 g of n-propanol was added after mixing, and magnetic stirring was performed for 30 min;
[0071] S23: High-speed shearing at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, the pre-dispersed slurry is put into a homogenizer, homogenized at 800 Bar pressure for 3 times, and then transferred to a vacuum degassing machine for degassing;
[0072] S24: A platform-type slot extrusion sheet coating machine is used, and the platform drying temperature is set at 60°C. The treated coating slurry is coated on the soft template, and the dry film thickness is controlled at 13 microns.
[0073] The ridge structure in step S3 is covered with a low hydrophilic groove, comprising the following steps:
[0074] S31: Weigh 0.60 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 5.31 g of deionized water and stir thoroughly to wet, and slowly drop 3.84 g of perfluorosulfonic acid resin D520CS (5 wt%) while stirring;
[0075] S32: After mixing, add 26.24 g of ethanol, stir with a magnetic stirrer for 30 min, high-speed shear at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, and ultrasonicate the pre-dispersed slurry in a water bath at 10°C for 1 h;
[0076] S33: Using platform ultrasonic spraying equipment, the platform drying temperature is set at 90℃, the treated spray slurry is coated on the above catalyst layer, the dry film thickness is controlled at 4 microns, the construction of the entire grooved catalyst layer is completed, and the Pt loading is controlled at 0.30mg / cm 2 .
[0077] The transfer of the grooved catalytic layer in step S4 comprises the following steps:
[0078] S41: The proton exchange membrane uses a 12-micron membrane, cuts the proton exchange membrane and PTFE protective layer of appropriate size, covers the proton exchange membrane on the catalyst layer side of the soft template, fits and discharges the air, and fits the two sides of the composite membrane material with a 40-micron thick PTFE protective layer respectively;
[0079] S42: Set the temperature and pressure of the hot press, the platform temperature is controlled at 140℃, and the pressure is controlled at 5kN / m 2 , put the sample into the hot press and keep the pressure for 3 minutes;
[0080] S43: After the hot pressing is completed, the sample is taken out, and after the sample is cooled, the soft template is peeled off from the composite membrane material, and the catalytic layer is transferred from the soft template to the proton exchange membrane.
[0081] The membrane electrode preparation comprises the following steps:
[0082] 1: Use the above-mentioned spray slurry as the anode slurry and use a platform ultrasonic spraying device to spray 0.08 mg / cm on the cathode grooved catalyst layer half CCM. 2 A platinum-loaded anode catalyst layer;
[0083] 2: The gas diffusion layers are attached to both sides and packaged into membrane electrodes.
[0084] Embodiment 2:
[0085] In this embodiment, the preparation of the soft film board in step S1 is different from that in embodiment 1 in that the groove width is 12 microns, the spacing is 25 microns, and the depth is 18 microns;
[0086] The method for preparing the ridge structure in step S2 is different from that in Example 1 in that the dry film thickness is controlled at 16 micrometers.
[0087] Embodiment 3:
[0088] (1) In this embodiment, comparative example 1 is introduced. Compared with embodiment 1, a planar catalytic layer structure is adopted. The preparation method of comparative example 1 comprises: weighing 3.50 g of platinum carbon catalyst TEC10E50E (Pt content 46.70 wt%), adding 17.26 g of deionized water to fully stir and wet, slowly dripping 14.92 g of perfluorosulfonic acid resin DFPSA-2179 (10 wt%) while stirring, adding 4.26 g of n-propanol after mixing, stirring with a magnetic stirrer for 30 min, high-speed shearing at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10° C., putting the pre-dispersed slurry into a homogenizer, homogenizing at a pressure of 800 Bar for 3 times, and transferring to a vacuum degassing machine for degassing;
[0089] A platform-type slot extrusion sheet coating machine was used. The platform drying temperature was set at 60°C. The treated coating slurry was coated on the soft template. The dry film thickness was controlled at 9 microns and the cathode Pt loading was controlled at 0.30 mg / cm 2 , i.e. as a cathode catalyst layer;
[0090] Weigh 0.60g of platinum carbon catalyst TEC10E50E (Pt content 46.70wt%), add 5.31g of deionized water to fully stir and wet, slowly drip 3.84g of perfluorosulfonic acid resin D520CS (5wt%) while stirring, add 26.24g of ethanol after mixing, stir with a magnetic stirrer for 30min, high-speed shear at a linear speed of 20m / s for 10min in a constant temperature water bath at 10℃, ultrasonicate the pre-dispersed slurry in a 10℃ water bath for 1h, use a platform ultrasonic spraying equipment, the platform drying temperature is set at 90℃, and the treated spray slurry is coated on the anode side of the above-mentioned cathode half CCM, and the anode Pt loading is controlled at 0.08mg / cm 2 ;
[0091] The gas diffusion layers are attached to both sides of the CCM to form a membrane electrode.
[0092] (2) Comparative Example 2, compared with Example 1, does not distinguish between the ionic polymer components of the groove structure and the ridge structure, and the catalytic slurry uses a short-chain resin and a high I / C value ratio. The preparation method of Comparative Example 2 includes:
[0093] Weigh Sylgard184 (PDMS) and curing agent, mix them evenly in a ratio of 10:1, place the mixed PDMS in a vacuum degassing machine, degas at a speed of 15000RPM for 30 minutes to remove bubbles generated during the mixing process, clean the silicon wafer substrate, use isopropanol and deionized water for ultrasonic cleaning respectively, and set aside after drying. The degassed PDMS is evenly coated on the silicon wafer substrate with a thickness of 1mm. The coated silicon wafer is placed in an oven and allowed to stand at 60°C for 4 hours. The PDMS surface is treated with an oxygen plasma processor to increase the adhesion of the subsequent catalyst slurry. The treatment time is controlled at 3 minutes and the power is set to 50W. A laser direct writing system is used to prepare micro-scale grooves on the PDMS surface. The groove width is 10 microns, the spacing is 20 microns, and the depth is 15 microns. After the processing is completed, the PDMS surface is rinsed and cleaned with isopropanol to remove the residues that may be generated during the processing. The PDMS is post-cured in an oven and allowed to stand at 80°C for 2 hours.
[0094] Weigh 3.50g of platinum carbon catalyst TEC10E50E (Pt content 46.70wt%), add 17.26g of deionized water to fully stir and wet, slowly drip 14.92g of perfluorosulfonic acid resin DFPSA-2179 (10wt%) while stirring, add 4.26g of n-propanol after mixing, stir with a magnetic stirrer for 30min, high-speed shear at a linear speed of 20m / s for 10min in a constant temperature water bath at 10°C, put the pre-dispersed slurry into a homogenizer, homogenize at 800Bar pressure for 3 times, transfer to a vacuum degassing machine for degassing, use a platform-type slit extrusion sheet coater, the platform drying temperature is set at 60°C, and the treated coating slurry is coated on a soft template, the dry film thickness is controlled at 17 microns, and the Pt loading is controlled at 0.30mg / cm 2 ;
[0095] The proton exchange membrane uses a commercially available 12-micron membrane. Cut the proton exchange membrane and PTFE protective layer of appropriate size, cover the proton exchange membrane on the catalyst layer side of the soft template, fit and exhaust the air, and fit the two sides of the composite membrane material with a 40-micron thick PTFE protective layer. Set the temperature and pressure of the hot press, control the platform temperature at 140°C, and the pressure at 5kN / m 2 The sample is placed in a hot press and kept under pressure for 3 minutes. After the sample is cooled, the soft template is peeled off from the composite membrane material, and the catalytic layer is transferred from the soft template to the proton exchange membrane.
[0096] Weigh 0.60g of platinum carbon catalyst TEC10E50E (Pt content 46.70wt%), add 5.31g of deionized water to fully stir and wet, slowly drip 3.84g of perfluorosulfonic acid resin D520CS (5wt%) while stirring, add 26.24g of ethanol after mixing, stir with a magnetic stirrer for 30min, high-speed shear at a linear speed of 20m / s for 10min in a constant temperature water bath at 10℃, ultrasonicate the pre-dispersed slurry in a 10℃ water bath for 1h, use a platform ultrasonic spraying equipment, the platform drying temperature is set at 90℃, and the treated spray slurry is coated on the anode side of the above-mentioned cathode half CCM, and the anode Pt loading is controlled at 0.08mg / cm 2 The prepared CCM samples were bonded with Toray 0020 gas diffusion layers on both sides and packaged into membrane electrodes.
[0097] The polarization curves of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 are as follows: Figure 3 As shown, compared with the planar catalyst layer form of comparative example 1, examples 1 and 2 show higher polarization performance advantages at 2 A / cm 2 The voltage at the current density reached above 0.65V; at the same time, Example 1 had an advantage of 10-20mV over Example 2, because the reduction of the groove arrangement period and the refinement of the grooves further exerted the advantages of rapid lateral diffusion of O2 in the grooves and efficient transmission of H+ in the ridge structure; while the performance of Comparative Example 2 dropped sharply at high current density, which was attributed to the poor hydrophobicity caused by the high ion polymer content of the grooves as a whole, and the generated water accumulated in the grooves of the catalyst layer hindered gas transmission and lateral diffusion.
[0098] The impedance spectrum EIS curves of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 are as follows: Figure 4 As shown, the mass transfer impedance of Comparative Example 2 is more obvious in the high frequency band, indicating that at 2A / cm 2 Under working conditions, the impedance effect caused by membrane electrode gas transmission has occupied a dominant position, and drainage gas shortage problems begin to appear at the reaction sites of the catalyst layer; whereas in Example 1, a groove structure is formed by using low I / C and long-chain ionomer components, which significantly improves the drainage problem under high current density, so that the mass transfer advantages brought by the grooved catalyst layer can be fully utilized.
[0099] The above is a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any modification, equivalent substitution and improvement made by any technician familiar with the field within the technical scope disclosed by the present invention in combination with the prior art or public common sense, within the spirit and principle of the present invention, shall be covered by the protection scope of the present invention.
Claims
1. A method for preparing a grooved catalyst layer membrane electrode for a fuel cell, characterized in that: The following steps are involved: S1: coating and curing the prepared soft template, treating it to increase wettability, processing grooves using micro-nano technology, and then performing secondary curing; S2: Use short-chain resin with high I / C to prepare coating slurry, apply it to the soft template through slit coating and dry it to form a ridge structure; S3: Spray slurry was prepared using long-chain resin with low I / C and sprayed onto the soft template by ultrasonic spraying to cover the ridge structure as grooves; S4: Laminating the proton exchange membrane and the catalyst layer, hot pressing under PTFE protection, and transferring the catalyst layer to the proton exchange membrane; S5: Spraying the catalyst layer on the anode side, attaching the gas diffusion layer, and packaging into a membrane electrode.
2. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 1, characterized in that: The soft film board in step S1 includes the following steps during the preparation process: S11: Weigh Sylgard 184 (PDMS) and curing agent, and mix them evenly in a ratio of 10:1; S12: placing the mixed PDMS in a vacuum degassing machine and degassing at a speed of 15000 RPM for 30 min to remove bubbles generated during the mixing process; S13: taking the silicon wafer substrate and using isopropyl alcohol and deionized water for ultrasonic cleaning respectively, and drying and setting aside for later use; S14: evenly coating the degassed PDMS on the silicon wafer substrate with a thickness of 1 mm, placing the coated silicon wafer in an oven at 60° C. for 4 hours; S15: Use an oxygen plasma processor to treat the PDMS surface to increase the adhesion of the subsequent catalyst slurry. The treatment time is controlled at 3 minutes and the power is set to 50W; S16: Microscale grooves were prepared on the PDMS surface using a laser direct writing system; S17: After processing, the PDMS surface is rinsed and cleaned with isopropyl alcohol to remove the residues that may be generated during the processing; S18: The PDMS was post-cured in an oven at 80°C for 2 hours for secondary curing to ensure its mechanical stability.
3. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 2, characterized in that: The method for preparing the ridge structure in step S2 comprises the following steps: S21: Weigh 3.50 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 17.26 g of deionized water and stir thoroughly to wet; S22: 14.92 g of perfluorosulfonic acid resin DFPSA-2179 (10 wt%) was slowly added dropwise during stirring, and 4.26 g of n-propanol was added after mixing, and magnetic stirring was performed for 30 min; S23: High-speed shearing at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, the pre-dispersed slurry is put into a homogenizer, homogenized at 800 Bar pressure for 3 times, and then transferred to a vacuum degassing machine for degassing; S24: A platform-type slot extrusion sheet coating machine is used, and the platform drying temperature is set at 60°C to coat the treated coating slurry on the soft template.
4. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 3, characterized in that: The ridge structure in step S3 is covered with a low hydrophilic groove, comprising the following steps: S31: Weigh 0.60 g of platinum-carbon catalyst TEC10E50E (Pt content 46.70 wt%), add 5.31 g of deionized water and stir thoroughly to wet, and slowly drop 3.84 g of perfluorosulfonic acid resin D520CS (5 wt%) while stirring; S32: After mixing, add 26.24 g of ethanol, stir with a magnetic stirrer for 30 min, high-speed shear at a linear speed of 20 m / s for 10 min in a constant temperature water bath at 10°C, and ultrasonicate the pre-dispersed slurry in a water bath at 10°C for 1 h; S33: Using platform ultrasonic spraying equipment, the platform drying temperature is set at 90°C, and the treated spray slurry is coated on the above catalyst layer to complete the construction of the entire grooved catalyst layer. The Pt loading is controlled at 0.30 mg / cm 2 .
5. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 4, characterized in that: The transfer of the grooved catalytic layer in step S4 comprises the following steps: S41: The proton exchange membrane uses a 12-micron membrane, cuts the proton exchange membrane and PTFE protective layer of appropriate size, covers the proton exchange membrane on the catalyst layer side of the soft template, fits and discharges the air, and fits the PTFE protective layer on both sides of the composite membrane material; S42: Set the temperature and pressure of the hot press, the platform temperature is controlled at 140℃, and the pressure is controlled at 5kN / m 2 , put the sample into the hot press and keep the pressure for 3 minutes; S43: After the hot pressing is completed, the sample is taken out, and after the sample is cooled, the soft template is peeled off from the composite membrane material, and the catalytic layer is transferred from the soft template to the proton exchange membrane.
6. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 5, characterized in that: The membrane electrode preparation comprises the following steps: 1: Use the above-mentioned spray slurry as the anode slurry and use a platform ultrasonic spraying device to spray 0.08 mg / cm on the cathode grooved catalyst layer half CCM. 2 A platinum-loaded anode catalyst layer; 2: The gas diffusion layers are attached to both sides and packaged into membrane electrodes.
7. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 6, characterized in that: The micro-scale grooves in step S16 have a width of 10 microns, a pitch of 20 microns, and a depth of 15 microns.
8. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 7, characterized in that: The dry film thickness in step S24 is controlled at 13 μm.
9. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 8, characterized in that: The dry film thickness in step S33 is controlled at 4 μm.
10. A method for preparing a fuel cell grooved catalyst layer membrane electrode according to claim 9, characterized in that: The thickness of the PTFE protective layer in step S41 is 40 microns.