Preparation method and application of supported low-Pt core-shell fuel cell catalyst

By using trace surfactants and low-concentration salt solutions and reducing agents in proton exchange membrane fuel cells, the problem of high catalyst cost and difficult to take into account is solved, and efficient Oxygen reduction reaction performance and simple production process.

CN119092729AActive Publication Date: 2024-12-06DALIAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411137267.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-06
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The high cost of catalysts in existing proton exchange membrane fuel cells (PEMFCs) and the limited reserves of precious metal platinum, resulting in limited commercial development of fuel cells and difficult to take into account the activity and stability of the catalyst.

Method used

Use trace surfactant, low-concentration salt solution and reducing agent to prepare a supported low-Pt core-shell fuel cell catalyst. The metal salt and reducing agent are dispersed through a carbon support to form a uniform core-shell structure catalyst, suitable for a variety of platinum-based Preparation of alloy components.

Benefits of technology

The high activity and stability of the catalyst are achieved, and the production cost is reduced. The catalyst shows excellent oxygen reduction reaction performance in acidic media, the half-wave potential is higher than that of commercial Pt/C, and the synthesis process is simple and efficient, suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092729A_ABST
    Figure CN119092729A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrocatalysts, and particularly relates to a preparation method and application of a supported low-Pt core-shell fuel cell catalyst. The preparation method comprises the following steps: by adopting a water phase method, under the condition of adding a trace amount of a surfactant, putting a material subjected to two-step reducing agent reduction, filtering, washing and drying into a tubular furnace, heating to a specific temperature, annealing, and cooling to obtain a finished product of the carbon-supported low-Pt core-shell electrocatalyst. The catalyst is small in size and uniform in dispersion; the process is simple and efficient, and the high-stability core-shell catalyst can be prepared in batches.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysts, and in particular relates to a preparation method and application of a supported low-Pt core-shell fuel cell catalyst. Background Art

[0002] Hydrogen energy is a secondary energy source with abundant sources, green and low carbon, and wide application. It is gradually becoming one of the important carriers of global energy transformation and development. Proton exchange membrane fuel cells (PEMFC) are one of the current research and development focuses in the field of hydrogen energy applications, but they still face challenges in commercialization, including waste heat generation, sensitivity to fuel impurities, expensive catalysts, and slow oxygen reduction reaction (ORR) rates. The catalyst accounts for more than 30% of the total cost because PEMFC relies heavily on the use of precious metal Pt, but Pt is expensive and has limited reserves, resulting in high manufacturing costs for PEMFC, which seriously restricts its commercial development. The development of new high-performance and low-cost catalysts is of great significance to promote the development of fuel cells. In order to reduce the cost of catalysts while ensuring the requirements of high catalyst activity, the solution strategy is to design low Pt catalysts, including several forms, design the shape of catalytic particles to control the arrangement of surface atoms; single atoms to improve utilization; alloying the cheaper transition metal M with Pt, changing the electronic structure of Pt through the ligand effect, and constructing a core-shell structure to improve its utilization efficiency. However, the synthesis process of electrocatalysts with controlled morphology is cumbersome and difficult to mass produce. The single atom has poor durability and is easily deactivated. Dispersing Pt on the surface of non-platinum nanoparticles to form a core-shell structure catalyst can effectively improve the utilization efficiency of precious metal platinum. At the same time, due to the special surface electronic structure and the special interaction between the core and the shell, the Pt-based core-shell structure catalyst exhibits higher catalytic activity and stability.

[0003] Therefore, it is of great value and significance to develop a small-sized, supported low-Pt core-shell fuel cell catalyst with simple and efficient preparation process and mass production. Summary of the invention

[0004] The purpose of the present invention is to solve the above-mentioned problems in the prior art and provide a method for preparing a supported low-Pt core-shell fuel cell catalyst for oxygen reduction reaction and its application. The preparation method uses trace surfactants, low-concentration salt solutions and reducing agents to make the catalyst particles uniform in size, with a clear core-shell structure, good activity and stability, and can be adapted to the preparation of a variety of platinum-based alloy components.

[0005] To achieve the above object, the present invention adopts the following technical scheme:

[0006] A method for preparing a supported low-Pt core-shell fuel cell catalyst comprises the following steps:

[0007] (1) dispersing the carbon support in a surfactant aqueous solution, adding a Cu metal salt aqueous solution and an Au metal salt aqueous solution under vigorous stirring at a temperature of 0 to 25° C., and adjusting the solution pH to ≥ 7 with an alkaline solution; then adding a reducing agent aqueous solution, and reacting for 0.1 to 1.5 hours; then adjusting the solution pH to ≥ 7 with an alkaline solution, adding a Pt metal salt aqueous solution, and then adding a reducing agent aqueous solution, and reacting for 0.1 to 5 hours, preferably 0.1 to 1.5 hours;

[0008] (2) filtering, washing and drying the obtained mixed solution, placing the obtained material after drying in a porcelain boat, placing it in a tube furnace, introducing a certain gas, and keeping the temperature at a certain temperature, and finally obtaining a carbon-supported low Pt core-shell (AuCu@Pt / C) fuel cell catalyst material after cooling;

[0009] The catalyst is a carbon-supported platinum-copper-gold alloy material, in which the loading of the platinum-copper-gold alloy is 10-60wt% (preferably 10-50%), and the atomic ratio of Au, Cu and Pt is 1:1:1-1:3:7-1:4:9, preferably 1:1:1-1:3:7.

[0010] Furthermore, in step (1), the carbon carrier is dispersed in the surfactant aqueous solution at a concentration of 0.01 to 2 mg mL -1 , preferably 0.01 to 0.1 mg mL -1 ;

[0011] The concentration of the surfactant aqueous solution is 10 to 100 mmol L -1 , preferably 10 to 60 mmol L -1 , more preferably 10 to 50 mmol L -1 ;

[0012] The concentration of the metal salt aqueous solution is 0.1 to 60 mmol L -1 , preferably 1 to 40 mmol L -1 ;

[0013] The concentration of the reducing agent aqueous solution is 0.5 to 400 mmol L -1 , preferably 1 to 60 mmol L -1 , more preferably 50 to 100 mmol L -1 ;

[0014] The reducing agent added each time is in excess relative to the total amount of Cu metal salt, Au metal salt and Pt metal salt. The amount of the reducing agent added each time is 2 to 10 times, preferably 2 to 5 times, the total amount of Cu metal salt, Au metal salt and Pt metal salt.

[0015] Furthermore, the carbon carrier includes at least one of carbon black materials (such as Vulcan XC-72, BP2000, Ketjen Black EC-300J, ECP-600JD), fullerenes, carbon nanotubes, carbon nanotube aerogels, carbon aerogel materials, metal organic framework pyrolytic carbon materials, graphene, graphene aerogels, and carbon nanocages.

[0016] Further, the surfactant is at least one of a cationic surfactant, an anionic surfactant, an amphoteric surfactant, and a nonionic surfactant; preferably, the cationic surfactant is at least one of alkyltrimethylammonium chloride, alkyldimethylbenzylammonium chloride, and dialkyldimethylammonium chloride, the anionic surfactant is at least one of cyclopentaneate, alkylbenzenesulfonate, alkylsulfonate, and alkyl sulfate (such as sodium dodecyl sulfate (SDS)), the amphoteric surfactant is at least one of γ-(methacryloyloxy)propyltrimethoxysilane, bis-(3-triethoxysilylpropyl)amine and bis-(trimethoxysilylpropyl)amine, and the nonionic surfactant is at least one of Tween 20, Triton X-100, polyethylene glycol, and Surfynol 485.

[0017] Furthermore, the platinum metal salt may be one or a mixture of two or more of chloroplatinic acid, chloroplatinous acid, potassium chloroplatinate, potassium chloroplatinite, sodium chloroplatinate, sodium chloroplatinite, ammonium chloroplatinate, and ammonium chloroplatinite, but is not limited thereto.

[0018] Furthermore, the copper metal salt may be one or a mixture of two or more of cupric chloride, cuprous chloride, cupric nitrate, cupric sulfate, cuprous nitrate, cuprous sulfate, and cupric acetate, but is not limited thereto.

[0019] Furthermore, the gold metal salt may be one or a mixture of two or more of chloroauric acid, sodium chloroaurate, ammonium tetrachloroaurate, potassium chloroaurate, and potassium gold citrate, but is not limited thereto.

[0020] Furthermore, in step (1), the carbon support is dispersed in a 50-100 μL SDS aqueous solution and the solution is ultrasonically mixed to make it uniform.

[0021] Furthermore, in step (1), the rotation speed of the vigorous stirring is greater than 200 rpm.

[0022] Furthermore, in step (1), after the first addition of the reducing agent aqueous solution and the reaction for 0.1 to 1.5 hours, the solution pH is first adjusted to ≤ 7 with an acid to destroy the excess reducing agent, and then the solution pH is adjusted to ≥ 7 with an alkaline solution, and then the Pt metal salt aqueous solution is added, and then the reducing agent aqueous solution is added to react for 0.1 to 5 hours.

[0023] Furthermore, in step (1), before adding the reducing agent for the first time, the solution is aerated with an inert gas for 5-30 minutes to remove the oxidizing gas.

[0024] Furthermore, in step (1), the reaction atmosphere is an inert gas, and the inert gas can be helium, argon, or nitrogen, but is not limited thereto.

[0025] Furthermore, in step (2), the insulation temperature is 100-400° C., and the insulation time is 1-3 hours; the temperature is increased to the insulation temperature at a certain rate, and the heating rate is 1-10° C. / min.

[0026] Furthermore, in step (2), the reaction atmosphere can be one or more of helium, argon, nitrogen, hydrogen, a hydrogen-argon mixture (hydrogen accounts for 5-30% by volume, for example, 5, 10, 20, 30%), CO or low-carbon alkanes (C2-C3 chain alkanes), but is not limited thereto.

[0027] Furthermore, the reducing agent may be sodium borohydride, potassium borohydride, magnesium borohydride, formaldehyde, formic acid, citric acid, glucose, sucrose, ascorbic acid, but is not limited thereto.

[0028] Furthermore, the acid may be one or a mixture of two or more of hydrochloric acid, sulfuric acid, perchloric acid, nitric acid, oxalic acid, sulfurous acid, phosphoric acid, nitrous acid, carbonic acid, formic acid, lactic acid, benzoic acid, and acetic acid, but is not limited thereto.

[0029] Furthermore, the alkali may be one or a mixture of two or more of sodium hydroxide, potassium hydroxide, barium hydroxide, and ammonia water, but is not limited thereto.

[0030] Furthermore, in step (2), the drying time is 1 to 24 hours, the drying temperature is 60 to 90° C., and the drying environment is vacuum.

[0031] The present invention also relates to a supported low-Pt core-shell fuel cell catalyst obtained by protecting the above-mentioned preparation method, wherein the catalyst comprises low-Pt core-shell alloy particles and a catalyst carrier, wherein the low-Pt core-shell alloy particles are supported on the catalyst carrier, and the catalyst carrier is a carbon carrier; the low-Pt core-shell alloy particles in the supported low-Pt core-shell alloy material are uniformly dispersed on the surface of the carbon carrier, and the nanoparticles obtained by the present invention have good size uniformity and good electrocatalytic activity and durability.

[0032] Furthermore, the low Pt core-shell alloy particles include a shell layer and a core, the shell layer is Pt or PtCu alloy, and the core is AuCu alloy; the particle size of the catalyst is 2 to 5 nm; the shell layer half-encloses or covers the surface of the core; the Pt loading of the catalyst is 9-40%, preferably 20 to 30%; the copper-gold alloy loading of the core is 1 to 20%, preferably 10 to 20%.

[0033] The present invention also relates to the use of protecting the above-mentioned supported low-Pt core-shell fuel cell catalyst in an acidic cathode oxygen reduction reaction.

[0034] The present invention uses an aqueous phase method, under the condition of adding a trace amount of surfactant, the material after two-step reduction with a reducing agent and filtering, washing and drying is placed in a tubular furnace, raised to a specific temperature for annealing, and after cooling, it is a finished carbon-supported low-Pt core-shell electrocatalyst.

[0035] Compared with the prior art, the advantages of the technical solution of the present invention are:

[0036] The core-shell structure of the present invention exhibits good durability in acidic media, and its mass specific activity (MA) is several times that of commercial Pt / C, and its half-wave potential (0.906V) is much higher than that of Pt / C (0.860V), indicating that it has excellent ORR performance;

[0037] The present invention adopts a low-temperature reduction approach, and the catalyst size is small and evenly dispersed;

[0038] The catalyst synthesis process of the present invention is simple and efficient, easy to industrialize, low in cost, and has great application potential;

[0039] The method has a wide range of applicability and can be used to synthesize core-shell alloy catalysts with different shell thicknesses. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a transmission electron microscopy (TEM) image of the catalyst obtained in Example 1, and the inset is a particle size statistical histogram.

[0041] Figure 2 The X-ray diffraction (XRD) pattern of the catalyst in Example 1 is shown in FIG.

[0042] Figure 3 The acidic cyclic voltammetry (CV) curve of Example 1 is shown at 25°C N 2 Saturated 0.1M HClO 4 aq., 50mVs -1 The scan rate was scanned in the potential range of 0 to 1.2 V vs. RHE.

[0043] Figure 4The acidic linear sweep voltammetry (LSV) curve of Example 1 is shown at 25°C. 2 Saturated 0.1M HClO 4 The scan range was 0-1.2 V vs. RHE and the scan rate was 10 mVs -1 , the electrode speed is 1600rpm. Test and record at 25℃ N 2 Saturated 0.1M HClO 4 The LSV curve in aq. was used as background correction, with a scan range of 0 to 1.2 V vs. RHE and a scan rate of 10 mVs -1 By O 2 Saturated LSV curve minus N 2 The saturated LSV curve can be used to obtain the ORR polarization curve.

[0044] Figure 5 This is the thermogravimetric analysis (TGA) curve of Example 1.

[0045] Figure 6 The acidic cyclic voltammetry (CV) curve after accelerated aging (ADT) of Example 1 is shown at 25°C N 2 Saturated 0.1M HClO 4 aq., at 500mV s -1 The sample was subjected to CV scanning at a scanning rate of , with a potential range of 0.6-1.0 V vs. RHE and 10000 scanning cycles.

[0046] Figure 7 This is the acidic linear sweep voltammetry (LSV) curve after accelerated aging (ADT) of Example 1. DETAILED DESCRIPTION

[0047] The present invention will be further described in the following examples, but the present invention is not limited thereto.

[0048] Example 1

[0049] 30 mg ECP-600JD was diluted to 0.03 mg mL -1 The concentration of 100 μL SDS was dispersed in deionized water, ultrasonicated for 20 min, and then the mixture was placed in a water bath. Under the conditions of controlling the speed at 1000 rpm and the temperature at 0 °C, 10 mmol L -1 15 mL of copper nitrate aqueous solution and 5 mL of chloroauric acid aqueous solution were added to control the ratio of Cu atoms to Au atoms to Pt atoms to 3:1:3. Then 5 mL of sodium bicarbonate aqueous solution was added to control the pH to 7-8. Then 100 mL of 1 mmol L -1The sodium borohydride aqueous solution was used as a reducing agent and the reaction was continued for 1 h. 2 mL of 12 mol / L hydrochloric acid was added first, followed by sodium bicarbonate to adjust the pH to 7-8, and then 15 mL of chloroplatinic acid aqueous solution was added, followed by 50 mL of 1 mmol L -1 The sodium borohydride aqueous solution was used as a reducing agent and reacted for 1 hour. The final mixed solution was filtered and washed until the filtrate was neutral; dried at 70°C overnight and ground, and heat treated at 200°C for 1 hour in a 5% hydrogen and argon atmosphere to finally obtain a 32.4wt.% supported low Pt core-shell alloy material, namely AuCu@Pt / C.

[0050] like Figure 1 The figure shows the transmission electron microscope (TEM) image of the AuCu@Pt / C core-shell alloy sample prepared in Example 1. The inset is Figure 1 The particle size statistical distribution diagram of the AuCu@Pt / C core-shell alloy sample prepared in this embodiment is measured, and the average particle size is 3.89nm, and there is a Pt shell layer of about 2nm on the catalyst surface. The transmission electron microscope (TEM) image can prove that the core-shell catalyst particles prepared in this embodiment are uniform in size and small in size.

[0051] like Figure 2 As shown, the XRD results show that the product obtained in this example is AuCu@Pt / C alloy.

[0052] like Figure 3 As shown, TGA determined that the loading of AuCu@Pt in the product obtained in this example was 32.4 wt.%.

[0053] like Figure 4 As shown, the acidic linear sweep voltammetry (LSV) curve of Example 1 can be calculated to obtain a mass specific activity (MA) of 601.77 mA / mg Pt , far superior to commercial platinum carbon.

[0054] like Figure 5 As shown, the thermogravimetric analysis (TGA) curve of Example 1 shows that the metal loading is 32%.

[0055] like Figure 6 As shown in the acidic cyclic voltammetry (CV) curve after accelerated aging (ADT) of Example 1, the increase in the oxidation peak between 0.6-0.7 V may be due to atomic rearrangement during the potential cycling test.

[0056] like Figure 7 As shown, in the acidic linear sweep voltammetry (LSV) curve of Example 1 after accelerated aging (ADT), the half-wave potential only decays by 19 mV.

[0057] Example 2

[0058] 30mg Vulcan XC-72 in 0.3mgmL -1 The concentration was dispersed in deionized water containing 10 μL SDS, and ultrasonicated for 60 min. Then, the mixture was placed in a water bath, and the speed was controlled at 800 rpm and the temperature was 5 °C. First, 20 mmol L -1 5 mL of copper chloride aqueous solution and 5 mL of sodium chloroaurate aqueous solution were added to control the ratio of Cu atoms to Au atoms to Pt atoms to be 1:1:1. 10 mL of sodium bicarbonate aqueous solution was added to control the pH to 7-8. Then 100 mL of 10 mmol L -1 Ascorbic acid aqueous solution was used as a reducing agent and the reaction was continued for 4 hours. After adding 1.5 mL of 12 mol / L hydrochloric acid and sodium carbonate to adjust the pH to 7-8, potassium chloroplatinate aqueous solution (5 mL) was added, followed by 100 mL of 10 mmol L -1 Ascorbic acid aqueous solution was used as a reducing agent and reacted for 2 hours. The final mixed solution was cooled, filtered, and washed until the filtrate was neutral; vacuum dried at 70°C overnight and ground, and heat treated at 200°C for 2 hours in a 5% hydrogen and argon atmosphere to finally obtain a supported low-Pt core-shell alloy material.

[0059] Example 3

[0060] 20mg of Ketjen Black EC-300J was diluted to 0.2mgmL -1 The concentration of 20 mmol L was dispersed in deionized water containing 50 μL of Brij 35 aqueous solution, and ultrasonicated for 60 min. Then, the mixture was placed in a water bath, and the speed was controlled at 800 rpm and the temperature was 25 °C. First, 20 mmol L -1 A cupric chloride aqueous solution (5mL) and a sodium chloroaurate aqueous solution (5mL) were added to control the ratio of Cu atoms, Au atoms and Pt atoms to be 1:1:1, and then 5mL of sodium carbonate aqueous solution was added to adjust the pH to 7-8, and then 37wt.% of formaldehyde aqueous solution was added as a reducing agent, and the reaction was carried out for 4h. 2mL of 12mol / L hydrochloric acid was first added, and then sodium hydroxide was added to adjust the pH to 7-8, and then chloroplatinic acid aqueous solution (5mL) was added, and then 37wt.% of formaldehyde aqueous solution was added as a reducing agent, and the reaction was carried out for 2h. The final mixed solution was cooled, filtered, and washed until the filtrate was neutral; vacuum dried at 70℃ overnight and ground, and heat treated at 250℃ for 2h in a 5% hydrogen-argon atmosphere to finally obtain a supported low-Pt core-shell alloy material.

[0061] Example 4

[0062] 20 mg ECP-600JD was diluted to 0.2 mg mL -1The concentration of 100 μL PVP aqueous solution was dispersed in deionized water, ultrasonicated for 30 min, and then the mixture was placed in a water bath, and the speed was controlled at 800 rpm and the temperature was 25 ° C. First, a concentration of 10 mmol L -1 A cupric chloride aqueous solution (10 mL) and a sodium chloroaurate aqueous solution (3 mL) were added to control the ratio of Cu atoms, Au atoms and Pt atoms to 3:1:1, and then 10 mL of sodium hydroxide was added to adjust the pH to 7-8, and 80 microliters of 20 mM formic acid aqueous solution was added as a reducing agent to react for 4 hours. After adjusting the pH to 7-8 by adding sodium hydroxide, chloroplatinic acid aqueous solution (5 mL) was added, and then 80 microliters of 20 mM formic acid aqueous solution was added as a reducing agent to react for 2 hours. The final mixed solution was cooled, filtered, and washed until the filtrate was neutral; vacuum dried at 70 ° C overnight and ground, and heat treated at 350 ° C for 2 hours in a 5% hydrogen argon atmosphere to finally obtain a supported low Pt core-shell alloy material.

Claims

1. A method for preparing a supported low-Pt core-shell fuel cell catalyst, characterized in that: The steps include: (1) dispersing the carbon support in a surfactant aqueous solution, adding a Cu metal salt aqueous solution and an Au metal salt aqueous solution under stirring at a temperature of 0 to 25° C., and adjusting the solution pH to ≥ 7 with an alkaline solution; then adding a reducing agent aqueous solution, and reacting for 0.1 to 1.5 hours; then adjusting the solution pH to ≥ 7 with an alkaline solution, and then adding a Pt metal salt aqueous solution, and then adding a reducing agent aqueous solution, and reacting for 0.1 to 5 hours; (2) filtering, washing and drying the mixed solution obtained in step (1), placing the obtained material in a tubular furnace, introducing a certain gas and keeping the temperature at a certain temperature, and finally obtaining a supported low-Pt core-shell fuel cell catalyst after cooling; The supported low-Pt core-shell fuel cell catalyst is a carbon-supported platinum-copper-gold alloy material, in which the loading of the platinum-copper-gold alloy is 10-60wt%, and the atomic ratio of Au, Cu and Pt is 1:1:1-1:4:

9.

2. The preparation method according to claim 1, characterized in that: The carbon carrier is dispersed in the surfactant aqueous solution at a concentration of 0.01 to 2 mg mL -1 ; The concentration of the surfactant aqueous solution is 10 to 100 mmol L -1 ; The concentration of the metal salt aqueous solution is 0.1 to 60 mmol L; The concentration of the reducing agent aqueous solution is 0.5 to 400 mmol L -1 ; The amount of the reducing agent added each time is 2 to 10 times the total amount of the Cu metal salt, the Au metal salt and the Pt metal salt.

3. The preparation method according to claim 1, characterized in that: The carbon carrier includes at least one of carbon black material, fullerene, carbon nanotube, carbon nanotube aerogel, carbon aerogel material, metal organic framework pyrolytic carbon material, graphene, graphene aerogel, and carbon nanocage; preferably, the carbon black material includes at least one of Vulcan XC-72, BP2000, Ketjen Black EC-300J, and ECP-600JD; The surfactant is at least one of anionic surfactants, cationic surfactants, amphoteric surfactants and nonionic surfactants; preferably, the anionic surfactant is at least one of cycloalkaneate, alkylbenzene sulfonate, alkyl sulfonate and alkyl sulfate; the cationic surfactant is at least one of alkyltrimethylammonium chloride, alkyldimethylbenzylammonium chloride and dialkyldimethylammonium chloride; the amphoteric surfactant is at least one of γ-(methacryloyloxy)propyltrimethoxysilane, bis-(3-triethoxysilylpropyl)amine and bis-(trimethoxysilylpropyl)amine; the nonionic surfactant is at least one of Tween 20, Triton X-100, polyethylene glycol and Surfynol 485.

4. The preparation method according to claim 1, characterized in that: The platinum metal salt includes one or a mixture of two or more of chloroplatinic acid, chloroplatinous acid, potassium chloroplatinate, potassium chloroplatinite, sodium chloroplatinate, sodium chloroplatinite, ammonium chloroplatinate, and ammonium chloroplatinite; The copper metal salt includes one or a mixture of two or more of cupric chloride, cuprous chloride, cupric nitrate, cupric sulfate, cuprous nitrate, cuprous sulfate, and cupric acetate; The gold metal salt includes one or a mixture of two or more of chloroauric acid, sodium chloroaurate, ammonium tetrachloroaurate, potassium chloroaurate, and potassium gold citrate; The reducing agent is one or a mixture of two or more of sodium borohydride, potassium borohydride, magnesium borohydride, formaldehyde, formic acid, citric acid, glucose, sucrose and ascorbic acid.

5. The preparation method according to claim 1, characterized in that: In step (1), the reaction atmosphere is an inert gas, and the inert gas is one or more of helium, argon, and nitrogen; Before adding the reducing agent for the first time, the mixture is aerated with inert gas for 5-30 minutes; The stirring speed is greater than 200 rpm.

6. The preparation method according to claim 1, characterized in that: In step (2), the reaction atmosphere is one or more of helium, argon, nitrogen, hydrogen, CO or low carbon alkanes; The heating rate is 1-10°C / min, the insulation temperature is 100-400°C, and the insulation time is 1-3h.

7. The preparation method according to claim 1, characterized in that: The reducing agent is one or a mixture of two or more of sodium borohydride, potassium borohydride, magnesium borohydride, formaldehyde, formic acid, citric acid, glucose, sucrose, and ascorbic acid; The acid is one or a mixture of two or more of hydrochloric acid, sulfuric acid, perchloric acid, nitric acid, oxalic acid, sulfurous acid, phosphoric acid, nitrous acid, carbonic acid, formic acid, lactic acid, benzoic acid, and acetic acid; The alkali is one or a mixture of two or more of sodium hydroxide, potassium hydroxide, barium hydroxide and ammonia water.

8. The preparation method according to claim 1, characterized in that: In step (1), after adding the reducing agent aqueous solution and reacting for 0.1 to 1.5 hours, the pH of the solution is first adjusted to ≤ 7 with an acid, and then the pH of the solution is adjusted to ≥ 7 with an alkaline solution, and then the Pt metal salt aqueous solution is added, and then the reducing agent aqueous solution is added, and the reaction is continued for 0.1 to 5 hours; In step (2), the drying time is 1 to 24 hours, the drying temperature is 60 to 90° C., and the drying environment is vacuum.

9. The supported low-Pt core-shell fuel cell catalyst obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The catalyst comprises low-Pt core-shell alloy particles and a catalyst carrier, wherein the low-Pt core-shell alloy particles are loaded on the catalyst carrier, and the catalyst carrier is a carbon carrier.

10. Use of the catalyst according to claim 9, characterized in that: Used in oxygen reduction reactions.

Citation Information

Patent Citations

  • Preparation method of catalyst with core-shell structure for low-temperature fuel cell

    CN102500365A

  • Preparing method for supported core-shell-structure catalyst for low-temperature fuel cell

    CN103157519A

  • Green low-temperature preparation method and electro-catalysis application of supported high-entropy alloy material

    CN115101764A

  • Method for preparing carbon-supported platinum-copper-gold alloy material through one-step reduction and electro-catalysis application of carbon-supported platinum-copper-gold alloy material

    CN116742028A

  • Particle exhibiting catalytic activity

    US20150079499A1