Sodium ion secondary battery

The energy density of sodium ion secondary batteries is solved by using carbon-sulfur system anode material and tunnel-like/layered metal oxide positive electrode material in sodium ion secondary batteries and coating MS-MTe2 heterostructured materials on the separator. The problem of electrochemical performance achieves high energy density and ideal cycle and rate performance.

CN119092796APending Publication Date: 2024-12-06SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411189493.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

While increasing the energy density of sodium ion secondary batteries, it is difficult to take into account capacity, circulation performance and rate performance, and the polysulfide shuttle effect of sulfur-based negative electrode materials affects the electrochemical performance.

Method used

Use carbon-sulfur system negative electrode material, combine tunnel metal oxides and/or layered metal oxides as positive electrode materials, and coat the separator with MS-MTe2 heterostructure material to enhance the energy density and structure of sodium ion secondary batteries. Stability, inhibiting the shuttle effect of polysulfides.

Benefits of technology

The high energy density, ideal cycle performance and rate performance of sodium ion secondary batteries are achieved, and the utilization rate and electrochemical performance of negative electrode materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015273180000131
    Figure BDA0005015273180000131
  • Figure BDA0005015273180000141
    Figure BDA0005015273180000141
  • Figure BDA0005015273180000151
    Figure BDA0005015273180000151
Patent Text Reader

Abstract

The invention discloses a sodium ion secondary battery, and belongs to the technical field of batteries. According to the sodium ion secondary battery, under the condition that a carbon-sulfur system negative electrode material is used, the diaphragm is coated with the MS-MTe2 heterostructure material, and the tunnel-shaped metal oxide and / or the layered metal oxide are / is used as the positive electrode material, so that the energy density of the whole sodium ion secondary battery can be effectively improved; meanwhile, the structural stability of the pole piece material is high, and the MS-MTe2 heterostructure material can inhibit the shuttle effect of polysulfide and reduce the influence of the MS-MTe2 heterostructure material on the deintercalation activity and quantity of sodium ions, so that the secondary battery synchronously has ideal cycle performance and rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a sodium ion secondary battery. Background Art

[0002] Using sulfur as the negative electrode material of sodium-ion secondary batteries can increase the sodium insertion capacity and efficiency of the negative electrode plate. The corresponding positive electrode material system can effectively improve the energy density of the secondary battery. However, due to the large size of sodium ions, the deintercalation process has high requirements on the structure of the plate material. Therefore, sodium-ion secondary batteries under high energy density systems often cannot take into account capacity, cycle performance and rate performance. On the other hand, sulfur-based negative electrode materials will introduce polysulfides, which have a shuttle effect and will significantly reduce the electrochemical performance of sodium-ion secondary batteries. Summary of the invention

[0003] The purpose of the present application is to overcome the shortcomings of the prior art and provide a sodium ion secondary battery. The secondary battery of the present application, when using a carbon-sulfur system negative electrode material, is coated with an MS-MTe2 heterostructure material on the diaphragm, and uses a tunnel-shaped metal oxide and / or a layered metal oxide as a positive electrode material, which can not only effectively improve the energy density of the overall sodium ion secondary battery, but also has high structural stability of the electrode material, and the MS-MTe2 heterostructure material can inhibit the shuttling effect of polysulfides, reduce its influence on the sodium ion deintercalation activity and quantity, so that the secondary battery simultaneously has ideal cycle performance and rate performance.

[0004] To achieve the above-mentioned object, in a first aspect of the present application, the present application provides a sodium ion secondary battery, including a positive electrode sheet, a negative electrode sheet, and a separator;

[0005] The positive electrode sheet includes a positive electrode material, and the positive electrode material includes at least one of a tunnel-shaped metal oxide and a layered metal oxide;

[0006] The negative electrode plate includes a negative electrode material, and the negative electrode material includes a sulfur-containing substance and a carbon-containing substance;

[0007] The diaphragm includes a coating, the coating includes a MS-MTe2 heterostructure material, and the M includes at least one of Fe, Ni, Co, and Cu.

[0008] As an embodiment of the present application, the tunnel-shaped metal oxide includes Na x XO2, X includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0<x<0.5.

[0009] As an embodiment of the present application, the layered metal oxide includes Na yYO2, Y includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0.5≤y<1.

[0010] As an embodiment of the present application, the mass ratio of the tunnel-shaped metal oxide to the layered metal oxide is (2:8) to (8:2).

[0011] As an embodiment of the present application, the particle size D of the tunnel-shaped metal oxide is v50 ≤30μm.

[0012] As an embodiment of the present application, the particle size D of the layered metal oxide is v50 ≤30μm.

[0013] As an embodiment of the present application, the negative electrode material includes elemental sulfur and elemental carbon, and the mass ratio of the elemental sulfur to the elemental carbon is (1:2) to (2:1).

[0014] As an embodiment of the present application, the particle size D of the negative electrode material v50 ≤5μm.

[0015] As an embodiment of the present application, the thickness of the coating layer is 2 to 5 μm.

[0016] As an embodiment of the present application, the particle dispersion degree of the tunnel-shaped structure metal oxide is 0.3-6.

[0017] As an implementation scheme of the present application, the air permeability of the diaphragm is 50 to 500 s / 100 mL; and the average pore size of the diaphragm is 1 to 3 μm.

[0018] As an embodiment of the present application, the sodium ion secondary battery satisfies:

[0019] 1<(β×b×d) / (θ×a×c)<1.1;

[0020] Among them, βg / m 2 is the mass per unit area of ​​the negative electrode material in the negative electrode sheet, θg / m 2 is the mass per unit area of ​​the positive electrode material in the positive electrode sheet, a wt% is the total mass percentage of tunnel-shaped metal oxides and layered metal oxides in the positive electrode material, b wt% is the total mass percentage of sulfur-containing substances and carbon-containing substances in the negative electrode material, c mAh / g is the reversible capacity of the positive electrode material at 25°C, and d mAh / g is the reversible capacity of the negative electrode material at 25°C.

[0021] More preferably,

[0022] a wt%=95-98.5wt%;

[0023] b wt% = 94-97.5 wt%;

[0024] c mAh / g = 108 to 170 mAh / g;

[0025] d mAh / g = 450 ~ 1000 mAh / g.

[0026] In a second aspect of the present application, the present application provides an electrical device, comprising the sodium ion secondary battery, wherein the sodium ion secondary battery serves as a power supply for the electrical device.

[0027] The beneficial effects of this application are:

[0028] The present application provides a sodium ion secondary battery. When a carbon-sulfur system negative electrode material is used, an MS-MTe2 heterostructure material is coated on a diaphragm, and a tunnel-shaped metal oxide and / or a layered metal oxide is used as a positive electrode material. This can not only effectively improve the energy density of the overall sodium ion secondary battery, but also the structural stability of the electrode material is high. The MS-MTe2 heterostructure material can inhibit the shuttling effect of polysulfides and reduce its influence on the activity and number of sodium ion deintercalation and extraction, so that the secondary battery simultaneously has ideal cycle performance and rate performance. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0030] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0031] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0032] The present application is further described below with specific embodiments:

[0033] The embodiment of the present application provides a sodium ion secondary battery, including a positive electrode sheet, a negative electrode sheet, and a separator;

[0034] The positive electrode sheet includes a positive electrode material, and the positive electrode material includes at least one of a tunnel-shaped metal oxide and a layered metal oxide;

[0035] The negative electrode plate includes a negative electrode material, and the negative electrode material includes a sulfur-containing substance and a carbon-containing substance;

[0036] The diaphragm includes a coating, the coating includes a MS-MTe2 heterostructure material, and the M includes at least one of Fe, Ni, Co, and Cu.

[0037] Sodium-ion secondary batteries have the advantages of a wide range of raw materials, high safety, and high temperature stability, but their relative energy density is low, and due to the large relative size of sodium ions, the structure of the pole material is easily damaged during the deintercalation process, so the cycle performance and rate performance need to be improved. Using sulfur-based materials as negative electrode materials for sodium-ion secondary batteries can effectively improve their energy density, but the utilization rate of sulfur-based materials at room temperature is not high, the redox kinetics are low, and the polysulfides produced have a shuttle effect, which in turn affects the electrochemical performance of secondary batteries. Therefore, in the scheme of the present application, when sulfur-containing substances and carbon-containing substances are compounded as negative electrode materials, at least one of tunnel-shaped metal oxides and layered metal oxides is introduced as positive electrode materials, wherein the former has a three-dimensional unique curved or angular tunnel structure, and the latter is formed by stacking of sheet oxides, both of which can provide sufficient sites for sodium ion deintercalation and have relatively ideal structural stability, and the rate performance will not decrease while the overall secondary battery energy density is improved, and the capacity and cycle performance are improved; on the other hand, the sodium ion secondary battery described in the present application is also provided with a coating containing MS-MTe2 heterostructure material on the diaphragm, and the MS-MTe2 heterostructure material can increase the chemical affinity of polysulfides, accelerate the catalytic conversion process of sulfur, and improve the redox kinetics of sulfur, and ultimately improve the utilization rate of sulfur in the negative electrode material and inhibit the shuttling effect of polysulfides, so that the sodium ion secondary battery ultimately has excellent comprehensive electrochemical properties.

[0038] In some embodiments, the tunnel-shaped metal oxide comprises Na x XO2, X includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0<x<0.5.

[0039] Further preferably, the tunnel-shaped metal oxide comprises Na 0.44 MnO2、Na 0.61 [Mn 0.27 Fe 0.34 Ti 0.39 ]O2、Na 0.66[Mn 0.66 Ti 0.34 ]At least one of O2.

[0040] In some embodiments, the layered metal oxide comprises Na y YO2, Y includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0.5≤y<1.

[0041] Further preferably, the layered metal oxide comprises Na 0.8 MnO2、Na 0.74 CoO2、Na 0.67 MnO2、Na 2 / 3 [Ni 1 / 3 Mn 2 / 3 ]At least one of O2.

[0042] In some embodiments, the positive electrode material includes tunnel-shaped metal oxides and layered metal oxides.

[0043] More preferably, the mass ratio of the tunnel-shaped metal oxide to the layered metal oxide is (2:8) to (8:2).

[0044] Further preferably, the mass ratio of the tunnel-shaped metal oxide to the layered metal oxide is in the range of one or any two of 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2.

[0045] Tunnel-shaped metal oxides and layered metal oxides differ greatly in morphology and interlayer spacing, so the diffusion rate and adsorption activity of sodium ions in the two positive electrode materials are also different, which in turn affects the total activity of sodium ion deintercalation and deintercalation stability. When the two metal oxides are used in combination, the advantages of both can be taken into account, thereby achieving high structural stability and high sodium storage activity. When the above-mentioned preferred compounding ratio is further selected, the product can achieve higher deintercalation capacity and better cycle performance and rate performance.

[0046] In some embodiments, the particle size D of the tunnel-shaped metal oxide is v50 ≤30μm.

[0047] Further preferably, the particle size D of the tunnel-shaped metal oxide is v50 =5~18μm.

[0048] Further preferably, the particle size D of the tunnel-shaped metal oxide is v50 =A range value of one or any two of 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 14μm, 16μm, and 18μm.

[0049] Further preferably, the particle size D of the tunnel-shaped metal oxide is v50 =7~13μm.

[0050] In some embodiments, the particle size D of the layered metal oxide is v50 ≤30μm.

[0051] More preferably, the particle size D of the layered metal oxide is v50 =5~30μm.

[0052] More preferably, the particle size D of the layered metal oxide is v50 =A range value of one or any two of 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 13μm, 16μm, 18μm, 20μm, 25μm, and 30μm.

[0053] The sizes of tunnel-structured metal oxides and layered metal oxides are related to the stacking density and bonding degree of the two when they are compounded. When the above-mentioned small-sized tunnel-structured metal oxides and layered metal oxides are preferably selected for combination, the particles of the two materials are arranged more tightly and concentrated, the density is higher and the force is more uniform when preparing the electrode, the bonding strength is high, and the sodium ions can maintain a higher diffusion, transmission and adsorption efficiency.

[0054] In some embodiments, the particle dispersion of the tunnel-shaped metal oxide is 0.3-6.

[0055] The calculation formula of the particle dispersion of the tunnel-shaped metal oxide is: (D v99 -D v10 ) / D v50 , the D v10 μm is the particle size corresponding to when the cumulative particle size distribution of the tunnel-shaped metal oxide reaches 10% based on the volume standard;

[0056] The D v50 μm is the particle size corresponding to when the cumulative particle size distribution of the tunnel-shaped metal oxide reaches 50% based on the volume standard;

[0057] The D v99 μm is the particle size corresponding to 99% of the cumulative particle size distribution of the tunnel-shaped metal oxide based on the volume standard.

[0058] Further preferably, the particle dispersion of the tunnel-shaped structured metal oxide is in the range of one or any two of 0.3, 0.5, 0.8, 1, 1.1, 1.2, 1.4, 1.5, 1.6, 1.8, 2, 3, 4, 5, 6.

[0059] Further preferably, the D of the tunnel-shaped metal oxide v10 It is 1 to 10 μm, and more preferably 4 to 6 μm.

[0060] Further preferably, the D of the tunnel-shaped metal oxide v10 The value is in the range of one or any two of 1 μm, 3 μm, 4 μm, 6 μm, 8 μm, and 10 μm.

[0061] Further preferably, the D of the tunnel-shaped metal oxide v99 It is 10 to 30 μm, and more preferably 15 to 27 μm.

[0062] Further preferably, the D of the tunnel-shaped metal oxide v99 The value is in the range of one or any two of 10 μm, 11 μm, 15 μm, 15 μm, 20 μm, 22 μm, 23 μm, 24 μm, 27 μm, 28 μm, and 30 μm.

[0063] The tunnel-structured metal oxide has a stable structure, and its particle dispersion directly affects the specific surface area and density of the positive electrode material when it is prepared into a positive electrode plate. It will also affect the bonding strength between the tunnel-structured metal oxide and the layered metal oxide in the positive electrode plate. When the tunnel-structured metal oxide within the above-mentioned preferred particle dispersion range is selected, the component can be more tightly combined with the layered metal oxide and will not damage the structure of the layered metal oxide due to its high density. At the same time, it can provide sufficient embedding and de-embedding sites for sodium ions, which is conducive to achieving better capacity and cycle stability.

[0064] The particle size D of the tunnel-shaped metal oxide v10 , D v50 and D v99 The testing method is as follows: the positive electrode material on the positive electrode sheet is scraped and placed in dimethyl carbonate for cleaning and drying, and then placed in ethanol for ultrasonic dispersion treatment. Then, the tunnel-shaped metal oxide particles are screened out and marked by EDS element content analysis under a scanning electron microscope. The number of marked particles is 200. Then, the marked particles are tested for particle size d using mapping software, and the software statistically calculates the single particle volume V and total volume of the particles. The volume V calculation formula is: V = (π / 6) × d 3 ; Record the particle size and corresponding volume of all measured particles; Sort the particles in ascending order according to particle size; Calculate the cumulative volume, starting from the first particle, to obtain the cumulative volume Vcum1, Vcum2, Vcum3, ..., Vcum200, then calculate the volume fraction, calculate the volume fraction corresponding to each cumulative volume Fi = 100% × Vcumi / total volume, and determine the Dv value:

[0065] When Fi reaches 10% for the first time, the corresponding particle size is the particle size D of the tunnel-shaped metal oxide. v10 .

[0066] When Fi reaches 50% for the first time, the corresponding particle size is the particle size D of the tunnel-shaped metal oxide. v50 .

[0067] When Fi reaches 99% for the first time, the corresponding particle size is the particle size D of the tunnel-shaped metal oxide. v99 The particle size test method of the layered structure metal oxide is the same as the particle size test method of the tunnel structure metal oxide.

[0068] In some embodiments, the particle size D of the positive electrode material is v50 =4~19μm

[0069] In some embodiments, the coating has a thickness of 2 to 5 μm.

[0070] More preferably, the thickness of the coating is in the range of one or any two of 2 μm, 2.5 μm, 3 μm, 4 μm, 4.5 μm, and 5 μm.

[0071] In some embodiments, the air permeability of the diaphragm is 50 to 500 s / 100 mL; and the average pore size of the diaphragm is 1 to 3 μm.

[0072] Further preferably, the air permeability of the diaphragm is 50s / 100mL, 80s / 100mL, 100s / 100mL, 120s / 100mL, 150s / 100mL, 180s / 100mL, 200s / 100mL, 250s / 100mL, 300s / 100mL, 350s / 100mL, 400s / 100mL, 500s / 100mL or any two of the range values; the average pore size of the diaphragm is 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm, 2.2μm, 2.5μm, 2.8μm, 3μm or any two of the range values.

[0073] Since the coating of the diaphragm contains MS-MTe2 heterostructure materials, the thickness of the coating is not only related to the physical properties of the diaphragm such as air permeability and pore size, but also to the relative content of the MS-MTe2 heterostructure materials. When the thickness within the above preferred range is selected to construct the diaphragm coating, the sodium-ion secondary battery can obtain better electrochemical performance.

[0074] In the present application, a Gurley 4110N air permeability tester is used to test the air permeability of the diaphragm. The steps are as follows: first, cut the diaphragm sample to a suitable size, then place the sample on the sample table, and tighten the sample table to fix the sample. Then rotate the inner cylinder of the instrument so that the pointer of the oil barrel reaches the 100cc scale and faces the sensor. Then press the "RESET" button of the timer on the display screen, and release the inner cylinder of the instrument at the same time. When the timing numbers on the timer no longer change, it means that the measurement is completed, and record the time for 100cc of air to pass vertically through a 1 square inch sample. Then repeat the test 3 times and take the average value, which is the air permeability of the diaphragm.

[0075] The test method for the average pore size of the diaphragm adopts the bubble point method, and the steps are as follows: first, the diaphragm sample is cut to a suitable size, and then the sample is completely immersed in a test liquid (dimethyl silicone oil) with a known surface tension under a vacuum environment, and then the immersed sample is installed in the test device and ensures that it is well sealed. Then slowly increase the gas pressure in the device while monitoring the pressure. When the gas starts to bubble continuously, record the bubble point pressure at this time. Then calculate the maximum pore size based on the bubble point pressure, the surface tension of the test liquid and the contact angle; then repeat the test 10 times and take the average value.

[0076] In some embodiments, the negative electrode material includes elemental sulfur and elemental carbon, and the mass ratio of the elemental sulfur to the elemental carbon is (1:2) to (2:1).

[0077] Further preferably, the mass ratio of the elemental sulfur to the elemental carbon is in the range of one or any two of 1:2, 1.4:1.6, 1.5:1.5, 1.8:1.2, and 2:1.

[0078] The use of a negative electrode material combining sulfur and carbon can take into account the activity, stability and capacity of sodium ion deintercalation. When sulfur and carbon in the above preferred range ratio are compounded to prepare the negative electrode material, the resulting sodium ion secondary battery can have better cycle performance and rate performance.

[0079] In some embodiments, the particle size D of the negative electrode material is v50 ≤5μm.

[0080] More preferably, the particle size D of the negative electrode material is v50 =A range value of one or any two of 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, and 5 μm.

[0081] The particle size of the negative electrode material is related to the compaction density of the negative electrode plate and the rate at which sodium ions are deintercalated. When the negative electrode material in the above-mentioned particle size range is selected to prepare the negative electrode plate, the sulfur in the negative electrode material can significantly improve the energy density of the overall secondary battery, while the carbon can fully alleviate the volume effect caused by the reaction between elemental sulfur and sodium. The negative electrode plate has a high compaction density, high sodium deintercalation activity, and good stability, and the electrochemical performance of the sodium ion secondary battery is better.

[0082] In some embodiments, the sodium ion secondary battery satisfies:

[0083] 1<(β×b×d) / (θ×a×c)<1.1;

[0084] Among them, βg / m 2 is the mass per unit area of ​​the negative electrode material in the negative electrode sheet, θg / m 2 is the mass per unit area of ​​the positive electrode material in the positive electrode sheet, a wt% is the total mass percentage of tunnel-shaped metal oxides and layered metal oxides in the positive electrode material, b wt% is the total mass percentage of sulfur-containing substances and carbon-containing substances in the negative electrode material, c mAh / g is the reversible capacity of the positive electrode material at 25°C, and d mAh / g is the reversible capacity of the negative electrode material at 25°C.

[0085] The selection of positive and negative electrode materials in the sodium ion secondary battery described in the present application is interrelated with the heterojunction material in the diaphragm coating. When the ratio of the mass per unit area of ​​the electrode material and the reversible capacity of the sodium ion secondary battery meets the above range, it can ensure that the positive and negative electrode materials can maintain a higher utilization rate, the sodium ion deintercalation efficiency is higher, and the deintercalation stability and long-term effect are good.

[0086] More preferably, a wt% = 95-98.5wt%, a wt% = one or any two of 95wt%, 95.5wt%, 96wt%, 96.5wt%, 97wt%, 97.5wt%, 98wt%, 98.5wt%.

[0087] More preferably, b wt%=94-97.5wt%, b wt%=one or any two of 94wt%, 94.5wt%, 95wt%, 95.5wt%, 96wt%, 96.5wt%, 97wt%, 97.5wt%.

[0088] Further preferably, c mAh / g = 108-170 mAh / g, c mAh / g = one or any two of 108 mAh / g, 110 mAh / g, 115 mAh / g, 120 mAh / g, 125 mAh / g, 130 mAh / g, 140 mAh / g, 150 mAh / g, 160 mAh / g, and 170 mAh / g.

[0089] More preferably, d mAh / g = 450-1000 mAh / g, d mAh / g = one or any two of 450 mAh / g, 480 mAh / g, 500 mAh / g, 550 mAh / g, 600 mAh / g, 650 mAh / g, 700 mAh / g, 750 mAh / g, 800 mAh / g, 900 mAh / g, and 1000 mAh / g.

[0090] In the sodium ion secondary battery described in the present application, based on the design of the positive electrode, the negative electrode and the diaphragm coating, a suitable correspondence between the proportion of active materials in the electrode sheet and its reversible capacity is constructed, which can make the sodium in the sodium ion secondary battery more completely deintercalated and deintercalated, and effectively ensure the cycle stability and rate performance.

[0091] The present invention is further described below with specific examples, which are not to be construed as limiting the scope of the present invention:

[0092] Example 1

[0093] A sodium ion secondary battery, the preparation method comprising the following steps:

[0094] (1) Preparation of positive electrode: tunnel-shaped metal oxide Na 0.44 MnO2 and layered metal oxides Na 0.8 MnO2 is mixed in proportion as the positive electrode material, with a reversible capacity of 160 mAh / g and a particle size of D v50 The thickness of the positive electrode sheet is 130 μm, and then the positive electrode sheet is 10 μm, and then the positive electrode sheet is 130 μm thick ...30 μm thick, and then the positive electrode sheet is 10 μm, and then the positive electrode sheet is 130 μm thick, and then the positive electrode sheet is 130 μm thick, and then the positive electrode sheet is 10 μm, and then the positive electrode sheet is 130 μm thick, and then the positive electrode sheet is 130 μm thick, and

[0095] (2) Preparation of negative electrode sheet: Elemental carbon and elemental sulfur are mixed in proportion as negative electrode material, with a reversible capacity of 633 mAh / g and a particle size of D v50 The thickness of the negative electrode sheet is 190 μm, and then the negative electrode sheet is mixed with carbon nanotubes, CMC, and SBR in a mass ratio of 94:2.1:1.5:2.4, and water is used as a solvent to prepare a slurry, which is coated on a copper foil current collector, dried, and cut to obtain a negative electrode sheet with a thickness of 190 μm.

[0096] (3) Preparation of the diaphragm: A PP diaphragm with an average pore size of 2 μm and an air permeability of 300 s / 100 mL was used as a substrate, and then a NiS-NiTe2 heterostructure material was coated on one surface and dried to obtain a diaphragm containing a coating;

[0097] The preparation method of the NiS-NiTe2 heterostructure material is as follows: Ni(OH)2 powder, S powder and Te powder in element ratio are mixed and placed in a quartz tube, and then the quartz tube is evacuated and placed in an environment of 600°C for reaction for 1 hour, and after cooling, the NiS-NiTe2 heterostructure material is washed three times with carbon disulfide and dried to obtain the NiS-NiTe2 heterostructure material; then the NiS-NiTe2 heterostructure material and PVDF are mixed in an NMP solvent at a mass ratio of 97:3, and then coated on a base film, dried, and prepared a coating;

[0098] (4) The positive electrode sheet, the negative electrode sheet and the separator (the coating side is close to the negative electrode sheet) are stacked and assembled into a soft-pack battery cell, and an electrolyte prepared by dissolving 1M NaPF6 in EC / DEC (1:1) and 5% FEC solvent is injected to obtain the sodium ion secondary battery.

[0099] The parameters of each electrode and diaphragm are shown in Tables 1 and 2.

[0100] Example 2

[0101] A sodium ion secondary battery, which differs from Example 1 only in that the tunnel-shaped metal oxide Na 0.44 MnO2 replaced by Na 0.61 [Mn 0.27 Fe 0.34 Ti 0.39 ]O2, the reversible capacity of the positive electrode material is 164mAh / g, and the thickness of the negative electrode sheet is different.

[0102] Example 3

[0103] A sodium ion secondary battery, which differs from Example 1 only in that the layered metal oxide Na 0.8 MnO2 replaced by Na 0.74 CoO2, the reversible capacity of the positive electrode material is 156mAh / g, and the thickness of the negative electrode sheet is different.

[0104] Example 4

[0105] A sodium ion secondary battery, which differs from Example 1 only in that the NiS-NiTe2 heterostructure material is replaced by a CuS-CuTe2 heterostructure material, and the preparation method of the CuS-CuTe2 heterostructure material differs from that of the NiS-NiTe2 heterostructure material only in that Ni(OH)2 is replaced by Cu(OH)2, and other conditions remain the same.

[0106] Example 5

[0107] A sodium ion secondary battery, which differs from Example 1 only in that the NiS-NiTe2 heterostructure material is replaced by a FeS-FeTe2 heterostructure material, and the preparation method of the FeS-FeTe2 heterostructure material differs from that of the NiS-NiTe2 heterostructure material only in that Ni(OH)2 is replaced by Fe(OH)2, and other conditions remain the same.

[0108] Example 6

[0109] A sodium ion secondary battery, which differs from Example 1 only in that the NiS-NiTe2 heterostructure material is replaced by a CoS-CoTe2 heterostructure material, and the preparation method of the CoS-CoTe2 heterostructure material differs from the NiS-NiTe2 heterostructure material only in that Ni(OH)2 is replaced by Co(OH)2, and other conditions remain the same.

[0110] Examples 7 to 28

[0111] A sodium ion secondary battery, which is different from Example 1 only in that the parameters of each electrode or separator during preparation are different, as shown in Table 1.

[0112] Embodiments 29 to 30

[0113] A sodium ion secondary battery, which is different from Example 1 only in that the thickness of the negative electrode plate is different.

[0114] Comparative Example 1

[0115] A sodium ion secondary battery, which is different from Example 1 only in that no coating is applied on the separator.

[0116] Comparative Example 2

[0117] A sodium ion secondary battery, which is different from Example 1 only in that the negative electrode material is pure elemental carbon without adding elemental sulfur.

[0118] Comparative Example 3

[0119] A sodium ion secondary battery, which is different from Example 1 only in that the negative electrode material is pure elemental sulfur without adding elemental carbon.

[0120] Comparative Example 4

[0121] A sodium ion secondary battery, which is different from Example 1 only in that the coating does not contain heterogeneous structural materials, and the coating is prepared by coating PVDF on the surface of a base film to form a coating with the same thickness as that of Example 1.

[0122] Where K = (β × b × d) / (θ × a × c), M is the mass ratio of the tunnel-shaped metal oxide to the layered metal oxide in the positive electrode material. The value is achieved by adjusting the mass per unit area of ​​the active material, the mass percentage of the active material in the electrode, and the type of material. Specifically, it is achieved by adjusting the thickness of the electrode, the proportion of active material added during the preparation of the electrode, and the selection of active materials with different reversible capacities. D v50隧 is the particle size D of the tunnel-shaped metal oxide v50 , D v50层 is the particle size D of the layered metal oxide v50 , D v10隧 is the particle size D of the tunnel-shaped metal oxide v10 , D v99隧 is the particle size D of the tunnel-shaped metal oxide v99 , N is the particle dispersion of the tunnel-shaped metal oxide, H is the thickness of the single-side coating of the separator, I is the air permeability of the separator, J is the average pore size of the separator, M is the mass ratio of the tunnel-shaped metal oxide to the layered metal oxide in the positive electrode material, and m is the mass ratio of elemental sulfur to elemental carbon in the negative electrode material. If there is no related substance, for example, the positive electrode material does not contain a tunnel-shaped metal oxide, the particle size D of the substance is not recorded. v50隧 For parameters such as , fill in " / " in the corresponding position.

[0123] Table 1

[0124]

[0125]

[0126] Table 2

[0127] parameter H(μm) I(s / 100mL) J(μm) M m Example 1 3 420 2 2:8 1:1 Example 2 3 420 2 2:8 1:1 Example 3 3 420 2 2:8 1:1 Example 4 3 422 2.5 2:8 1:1 Example 5 3 430 1.5 2:8 1:1 Example 6 3 440 2.5 2:8 1:1 Example 7 3 420 2 4:6 1:1 Example 8 3 420 2 5:5 1:1 Example 9 3 420 2 6:4 1:1 Example 10 3 420 2 8:2 1:1 Embodiment 11 3 420 2 10:0 1:1 Example 12 3 420 2 0:10 1:1 Example 13 2 390 2 2:8 1:1 Embodiment 14 4 450 2 2:8 1:1 Embodiment 15 5 480 2 2:8 1:1 Example 16 3 420 2 2:8 1:1 Embodiment 17 3 420 2 2:8 1:1 Embodiment 18 3 420 2 2:8 1:1 Embodiment 19 3 420 2 2:8 1:1 Embodiment 20 3 420 2 2:8 1:1 Embodiment 21 3 420 2 2:8 1:1 Embodiment 22 3 420 2 2:8 1:1 Embodiment 23 3 420 2 2:8 1:1 Embodiment 24 3 420 2 2:8 1:1 Embodiment 25 3 420 2 2:8 1:2 Embodiment 26 3 420 2 2:8 1.4:1.6 Embodiment 27 3 420 2 2:8 1.8:1.2 Embodiment 28 3 420 2 2:8 2:1 Embodiment 29 3 420 2 2:8 1:1 Embodiment 30 3 420 2 2:8 1:1 Comparative Example 1 / 300 2 2:8 1:1 Comparative Example 2 3 420 2 2:8 0:1 Comparative Example 3 3 420 2 2:8 1:0 Comparative Example 4 3 350 2 2:8 1:1

[0128] Effect example

[0129] The sodium ion secondary batteries obtained in each embodiment and comparative example were tested as follows:

[0130] (1) First discharge capacity test: The voltage range is 1.5V to 4.05V. The secondary battery is first charged to 4.05V at a rate of 0.2C, then charged at a constant voltage of 4.05V with a cut-off condition of 0.05C. After standing for 5 minutes, it is discharged to 1.5V at 0.2C.

[0131] (2) Cyclic performance test: voltage range 1.5-4.05 V, rest time 5 min, current rate 1C, charging stage 1C rate charging to 4.05 V, 4.05 V constant voltage to 0.05C, discharge stage 1C discharge to 1.5 V, cycle 500 times;

[0132] (3) Rate performance test: The voltage range is 1.5 to 4.05 V. The secondary battery is first fully charged to 4.05 V at a rate of 0.2 C, then charged to 0.05 C at a constant voltage of 4.05 V, and left to stand for 5 min. Discharge process: adjust to the corresponding rate of 5 C and discharge to 1.5 V.

[0133] The test results are shown in Table 2.

[0134] Table 2

[0135]

[0136]

[0137]

[0138] From Table 2 we can see that:

[0139] (1) The sodium ion secondary battery described in the present application uses a carbon-sulfur system negative electrode material and a tunnel-structured metal oxide and / or a layered metal oxide as a positive electrode material, which provides sufficient sites for the deintercalation of sodium ions and has a relatively ideal structural stability. It can not only achieve an improvement in the overall energy density of the secondary battery, but also achieve an initial discharge capacity of up to 120 mAh / g during charge and discharge tests. At the same time, a heterogeneous structure material coating is also provided on the diaphragm of the secondary battery. The coating can increase the chemical affinity of polysulfides, accelerate the catalytic conversion process of sulfur, and improve the redox kinetics of sulfur, ultimately improving the utilization rate of sulfur in the negative electrode material and inhibiting the shuttle effect of polysulfides, so that the secondary battery has ideal cycle performance and rate performance. After 500 long cycles, the discharge capacity retention rate of the product can reach more than 75%, and the discharge capacity at a rate of 5C can still reach more than 110 mAh / g.

[0140] (2) According to Example 1 and Examples 7 to 12, it can be seen that when constructing the positive electrode sheet, the positive electrode material can achieve higher sodium ion deintercalation activity and structural stability using a tunnel-shaped structured metal oxide or a layered metal oxide. The structures and interlayer spacings of the two are different. When the two are used in combination, the sodium ion secondary battery can further coordinate the balance of its energy density, cycle performance and rate performance. When the addition ratio of the two is appropriate, the comprehensive electrochemical performance of the sodium ion secondary battery is better.

[0141] (3) According to Example 1 and Examples 16 to 24, it can be seen that the tunnel-structured metal oxide can provide good sodium deintercalation structural stability for the overall positive electrode material, and the particle size and particle dispersion of the tunnel-structured metal oxide can further regulate the number of sodium deintercalation sites and deintercalation efficiency of the overall positive electrode material within a certain range. It can be seen that when the tunnel-structured metal oxide and the layered metal oxide with a suitable range of particle size and particle dispersion are selected, the product has a more ideal cycle performance and rate performance.

[0142] (4) It can be seen from Example 1, Examples 13 to 15 and Comparative Example 1 that the provision of a coating containing MS-MTe2 heterostructure material is the key to the sodium ion secondary battery being able to maintain excellent cycle performance and rate performance after the sulfur-carbon negative electrode material system is provided, and as the coating thickness increases, the capacity retention rate of the sodium ion secondary battery after a long cycle is higher, and the discharge specific capacity at a high rate is higher. As shown in Comparative Example 4, if a conventional modified coating is used, the same effect of improving performance may not be achieved.

[0143] (5) It can be seen from Example 1, Examples 25 to 28, and Comparative Examples 2 and 3 that the use of a sulfur-carbon negative electrode material system in a sodium ion secondary battery can take into account both the high energy density of sulfur-based materials and the high stability of carbon-based materials. If only sulfur-based materials are used as negative electrode materials, although the overall energy density is higher and the discharge specific capacity of the secondary battery is higher, the cycle performance and rate performance are poor; if only carbon-based materials are used as negative electrode materials, the energy density of the secondary battery is low and the cycle performance is also unsatisfactory. When the sulfur and carbon in the negative electrode material are preferably within an appropriate range, the sodium ion secondary battery can achieve better comprehensive electrochemical performance.

Claims

1. A sodium ion secondary battery, characterized in that: Including positive electrode sheet, negative electrode sheet and diaphragm; The positive electrode sheet includes a positive electrode material, and the positive electrode material includes at least one of a tunnel-shaped metal oxide and a layered metal oxide; The negative electrode plate includes a negative electrode material, and the negative electrode material includes a sulfur-containing substance and a carbon-containing substance; The diaphragm includes a coating, the coating includes a MS-MTe2 heterostructure material, and the M includes at least one of Fe, Ni, Co, and Cu.

2. The sodium ion secondary battery according to claim 1, characterized in that: The tunnel-shaped metal oxide includes Na x XO2, X includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0<x<0.5; And / or, the layered metal oxide comprises Na y YO2, Y includes at least one of V, Cr, Mn, Fe, Co, Ni, and Cu, and 0.5≤y<1.

3. The sodium ion secondary battery according to claim 2, characterized in that: The mass ratio of the tunnel-shaped metal oxide to the layered metal oxide is (2:8) to (8:2).

4. The sodium ion secondary battery according to claim 1, characterized in that: The particle size D of the tunnel-shaped metal oxide v50 ≤30 μm, and / or the particle size D of the layered metal oxide v50 ≤30μm.

5. The sodium ion secondary battery according to claim 1, characterized in that: The negative electrode material includes elemental sulfur and elemental carbon, and the mass ratio of the elemental sulfur to the elemental carbon is (1:2) to (2:1).

6. The sodium ion secondary battery according to claim 1, characterized in that: Includes at least one of the following (1) to (3): (1) The particle size D of the negative electrode material v50 ≤5μm; (2) The thickness of the coating is 2 to 5 μm; (3) The particle dispersion degree of the tunnel-shaped metal oxide is 0.3-6.

7. The sodium ion secondary battery according to claim 1, characterized in that: The air permeability of the diaphragm is 50-500 s / 100 mL, and / or the average pore size of the diaphragm is 1-3 μm.

8. The sodium ion secondary battery according to claim 1, characterized in that: The sodium ion secondary battery satisfies: 1<(β×b×d) / (θ×a×c)<1.1; Among them, βg / m 2 is the mass per unit area of ​​the negative electrode material in the negative electrode sheet, θg / m 2 is the mass per unit area of ​​the positive electrode material in the positive electrode sheet, a wt% is the total mass percentage of tunnel-shaped metal oxides and layered metal oxides in the positive electrode material, b wt% is the total mass percentage of sulfur-containing substances and carbon-containing substances in the negative electrode material, c mAh / g is the reversible capacity of the positive electrode material at 25°C, and d mAh / g is the reversible capacity of the negative electrode material at 25°C.

9. The sodium ion secondary battery according to claim 1, characterized in that: The sodium ion secondary battery satisfies at least one of (1) to (4): (1)a wt%=95~98.5wt%; (2)b wt%=94~97.5wt%; (3)c mAh / g=108~170mAh / g; (4)d mAh / g=450~1000mAh / g.

10. An electrical device, characterized in that: It comprises the sodium ion secondary battery according to any one of claims 1 to 9, wherein the sodium ion secondary battery is used as a power supply for the electrical device.