Composite sulfide electrolyte membrane, preparation method thereof and lithium ion battery
By preparing a composite film of high concentration ionic liquid and sulfide electrolyte in lithium-ion batteries, the problems of low conductivity and poor contact are solved, and the high conductivity and stable performance of lithium-ion batteries are achieved.
Patent Information
- Application Number
- CN202411027496.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-06
Smart Images

Figure CN119092797A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion battery separators, and in particular to a composite sulfide electrolyte membrane and a preparation method thereof, and a lithium-ion battery. Background Art
[0002] The existing polymer and sulfide composite electrolyte membranes use polymers only as binders. Since they cannot transmit lithium ions, they will cause certain damage to the conductivity and cannot improve the contact problem between the positive and negative electrodes of solid-state batteries and the electrolyte membrane. In addition, the polymer gel system will react with the sulfide electrolyte due to its high polarity, further deteriorating the overall conductivity, and there is also a safety risk of leakage. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the defects in the prior art and provide a composite sulfide electrolyte membrane and a preparation method thereof, and a lithium ion battery.
[0004] The present invention solves the above technical problems through the following technical solutions:
[0005] A method for preparing a composite sulfide electrolyte membrane comprises the following steps:
[0006] an ionic liquid mixing step, mixing the first ionic liquid and the second ionic liquid to obtain an ionic liquid mixture;
[0007] a lithium salt adding step, adding a lithium salt to the ionic liquid mixture to obtain a high-concentration ionic liquid;
[0008] A mixing step of mixing a sulfide electrolyte and a solvent in the high-concentration ionic liquid to obtain a slurry;
[0009] A membrane forming step, coating the slurry and drying it under a first drying condition to obtain a preliminary composite electrolyte membrane;
[0010] The polymerization step is to polymerize the preliminary composite electrolyte membrane by ultraviolet light initiation to obtain a composite sulfide electrolyte membrane.
[0011] Preferably, the first ionic liquid comprises a cation having the following structural formula:
[0012]
[0013] Wherein, the structure of R1 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the first ionic liquid is FSI - TFSI - , BF - 4.
[0014] Preferably, the second ionic liquid comprises a cation having the following structural formula:
[0015]
[0016] Wherein, the structure of R2 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the second ionic liquid is FSI - TFSI - , BF - 4.
[0017] Preferably, the lithium salt includes any one or a combination of the following:
[0018] LiFSI, LiTFSI, LiBF4;
[0019] And / or, the sulfide electrolyte includes any one of the following:
[0020] Li3PS4, Li 10 GeP2S 12 ,Li7P3S 11 ;
[0021] And / or, the solvent includes any one of the following:
[0022] Alkanes with 6 to 10 carbon atoms, carboxylates with 6 to 16 carbon atoms, toluene and xylene.
[0023] Preferably, the concentration of the lithium salt in the high-concentration ionic liquid is ≥2 mol / L.
[0024] Preferably, the mass ratio of the first ionic liquid to the second ionic liquid is 1:(2-3).
[0025] Preferably, in the mixing step, the mixing method adopted includes any one of the following:
[0026] Ball mill mixing, homogenizer mixing, stirring mixing.
[0027] Preferably, the first drying condition is baking, the baking temperature is 80° C.-120° C., and the baking time is ≥12 h.
[0028] A composite sulfide electrolyte membrane is prepared by the above preparation method.
[0029] A lithium ion battery comprises a diaphragm, wherein the diaphragm is the aforementioned composite sulfide electrolyte membrane.
[0030] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0031] The positive progressive effect of the present invention is that: the present invention discloses an ionic liquid which is in-situ polymerized as a binder and contains a saturated lithium salt to form an ion gel, which is compounded with a sulfide to prepare a composite electrolyte membrane, which has high ionic conductivity and good interface contact, and the battery assembled therefrom has good cycle performance and rate performance in a wide temperature range. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a flow chart of a method for preparing a composite sulfide electrolyte membrane according to a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] It should be noted that in the claims and description of this patent, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including one" do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0035] like Figure 1 As shown, this embodiment discloses a method for preparing a composite sulfide electrolyte membrane, which includes an ionic liquid mixing step, a lithium salt adding step, a mixing step, a membrane forming step and a polymerization step.
[0036] The ionic liquid mixing step refers to mixing the first ionic liquid and the second ionic liquid to obtain an ionic liquid mixture.
[0037] Further, in this embodiment, the mass ratio of the first ionic liquid to the second ionic liquid is 1:(1-5), preferably 1:(2-3).
[0038] The first ionic liquid includes a cation having the following general structural formula:
[0039]
[0040] Wherein, the structure of R1 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the first ionic liquid is FSI - TFSI - , BF - 4.
[0041] The second ionic liquid includes a cation having the following general structural formula:
[0042]
[0043] Among them, the structure of R2 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the second ionic liquid is FSI - TFSI - , BF - 4.
[0044] The preparation method of the composite sulfide electrolyte of this embodiment uses the first ionic liquid and the second ionic liquid. Since the R1 and R2 groups in the cationic structure contain one or more ester groups, the polyionic liquid formed by polymerization has a higher bonding effect.
[0045] The lithium salt adding step refers to adding lithium salt into the ionic liquid mixture to obtain a high concentration ionic liquid.
[0046] Further, in this embodiment, the lithium salt includes one or more of LiFSI, LiTFSI, and LiBF4. In this embodiment, the structure of the above lithium salt can be consistent with the anion group of the ionic liquid.
[0047] Furthermore, in this embodiment, the concentration of the lithium salt in the high-concentration ionic liquid is ≥ 2 mol / L. At this concentration, the lithium salt concentration is saturated, and the sulfide electrolyte will not decompose even if the ionic liquid has weak polarity.
[0048] The mixing step refers to mixing the sulfide electrolyte and the solvent in the high concentration ionic liquid to obtain a slurry.
[0049] Specifically, in this embodiment, the sulfide electrolyte is Li3PS4, Li 10 GeP2S 12 ,Li7P3S 11 , Li6PS5X type electrolyte, X represents halogen C1, Br, I, a type of sulfide.
[0050] The solvent includes, but is not limited to, alkanes with carbon atoms of 6 to 10, carboxylates with carbon atoms of 6 to 16, toluene, and xylene. The above solvent used in this embodiment is a non-polar solvent and will not decompose the sulfide electrolyte.
[0051] The mass ratio of the first ionic liquid to the sulfide electrolyte is (1-3): 100. The mass ratio of the sulfide electrolyte to the solvent is 100: (80-100). In the mixing step, the mixing method used includes but is not limited to ball mill mixing, homogenizer mixing, and stirring mixing.
[0052] The membrane forming step refers to obtaining a preliminary composite electrolyte membrane by coating the slurry and drying it under a first drying condition.
[0053] Specifically, in this embodiment, a double-roller machine is used for coating, and the first drying condition refers to baking, the baking temperature is 80° C.-120° C., and the baking time is ≥12 hours.
[0054] The polymerization step refers to polymerizing the preliminary composite electrolyte membrane by ultraviolet light to obtain a composite sulfide electrolyte membrane.
[0055] In the preparation method of the composite sulfide electrolyte of the present embodiment, due to the use of high-concentration lithium salt ionic liquid, the [Li+] in the slurry is always in a high concentration or close to saturation state. Even if the ionic liquid used is weakly polar or medium polar, the [Li+] in the sulfide electrolyte in the solid phase structure is difficult to react with the ionic liquid, and the cation structure of the ionic liquid used has a large steric hindrance, which will further hinder the reaction between the sulfide electrolyte and the ionic liquid, so that the conductivity of the sulfide electrolyte is always maintained at a high state.
[0056] In this embodiment, an ionic liquid is in situ polymerized as a binder, and a saturated lithium salt is included to form an ion gel, which is compounded with a sulfide to prepare a composite electrolyte membrane having high ionic conductivity and good interface contact. The battery assembled therefrom has good cycle performance and rate performance over a wide temperature range.
[0057] In another typical embodiment of the present application, a composite sulfide electrolyte membrane is provided. The composite sulfide electrolyte membrane is prepared by the above preparation method.
[0058] In another typical embodiment of the present application, a lithium-ion battery is provided, comprising a separator, wherein the separator is the above-mentioned composite sulfide electrolyte membrane.
[0059] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0060] Embodiment 1:
[0061] (1) 3 g of the first ionic liquid and 6 g of the second ionic liquid were mixed, and lithium salt was added so that the lithium salt concentration was LiFSI concentration = 2 mol / L;
[0062] (2) The mixed ionic liquid obtained in (1), 150 g of Li6PS5Cl, 150 g of isopentyl isovalerate and zirconium beads were added to a ball mill and mixed.
[0063] (3) The slurry in (2) is coated by a double-roller machine and baked at 120° C. for 12 h;
[0064] (4) By irradiating with ultraviolet light, a composite electrolyte membrane is obtained.
[0065] Embodiment 2:
[0066] 3 g of the first ionic liquid and 9 g of the second ionic liquid were mixed, and lithium salt was added so that the lithium salt concentration was LiFSI concentration = 2 mol / L;
[0067] The mixed ionic liquid obtained in (1), 100 g of Li6PS5Cl, 80 g of xylene and zirconium beads were added to a ball mill and mixed.
[0068] The slurry in (2) was coated by a double-roller machine and baked at 80°C for 24h;
[0069] By irradiating with ultraviolet light, a composite electrolyte membrane is obtained.
[0070] Embodiment 3:
[0071] 3 g of the first ionic liquid and 6 g of the second ionic liquid were mixed, and lithium salt was added so that the lithium salt concentration was LiFSI concentration = 2 mol / L, LiBF4 concentration = 0.5 mol / L;
[0072] The mixed ionic liquid obtained in (1), 150 g of Li6PS5Cl, 150 g of hexyl butyrate and zirconium beads were added to a ball mill and mixed.
[0073] The slurry in (2) was coated by a double-roller machine and baked at 80°C for 24h;
[0074] By irradiating with ultraviolet light, a composite electrolyte membrane is obtained.
[0075] Embodiment 4:
[0076] 3 g of the first ionic liquid and 6 g of the second ionic liquid were mixed, and lithium salt was added so that the lithium salt concentration was LiFSI concentration = 2 mol / L, LiBF4 concentration = 0.5 mol / L;
[0077] The mixed ionic liquid obtained in (1), 100 g of Li3PS4, 100 g of n-heptane and zirconium beads were added to a ball mill and mixed.
[0078] The slurry in (2) was coated by a double-roller machine and baked at 80°C for 24h;
[0079] By irradiating with ultraviolet light, a composite electrolyte membrane is obtained.
[0080] Table 1 shows the first ionic liquid and the second ionic liquid used in Examples 1-4.
[0081]
[0082]
[0083] Comparative Example 1:
[0084] 3 g of SBR, 100 g of Li6PS5Cl, 100 g of isopentyl isovalerate and zirconium beads were added into a ball mill and mixed. The mixture was coated by a double-roll mill and then baked to obtain the electrolyte membrane of Comparative Example 1.
[0085] The electrolyte membranes obtained in Examples 1 to 4 and Comparative Example 1 were made into standard mechanical test specimens for tensile testing, and the electrolyte membranes of Examples 1 to 4 and Comparative Example 1 were assembled into full battery soft pack cells for testing. The test pressures were set to 0 and 3 MPa, and the test temperatures were set to 30°C and 60°C by a pressurizing tool. The mechanical properties and electrochemical properties of the tests were as follows:
[0086] Mechanical strength / MPa Bending strength / MPa Example 1 77 33 Example 2 82 29 Example 3 69 36 Example 4 75 30 Comparative Example 1 30 24
[0087] Test conditions: 0MPa, 30℃
[0088] 0.1C(mAh / g) 0.3C(mAh / g) 0.5C(mAh / g) 1C(mAh / g) 300-week capacity retention rate (%) Example 1 199 166 123 67 77% Example 2 201 168 128 75 81% Example 3 201 170 125 69 77% Example 4 201 173 126 73 79% Comparative Example 1 188 - - - -
[0089] Test conditions: 3MPa, 30℃
[0090] 0.1C(mAh / g) 0.3C(mAh / g) 0.5C(mAh / g) 1C(mAh / g) 300-week capacity retention rate (%) Example 1 206 183 160 127 89% Example 2 204 182 157 124 92% Example 3 205 188 167 133 94% Example 4 205 185 162 127 90% Comparative Example 1 202 124 62 - -
[0091] Test conditions: 0MPa, 60℃
[0092] 0.1C(mAh / g) 0.3C(mAh / g) 0.5C(mAh / g) 1C(mAh / g) 300-week capacity retention rate (%) Example 1 206 182 154 102 83% Example 2 205 177 142 96 82% Example 3 206 184 162 110 85% Example 4 205 182 155 105 83% Comparative Example 1 186 99 - - -
[0093] Test conditions: 3MPa, 60℃
[0094] 0.1C(mAh / g) 0.3C(mAh / g) 0.5C(mAh / g) 1C(mAh / g) 300-week capacity retention rate (%) Example 1 206 185 169 152 92% Example 2 205 181 168 150 93% Example 3 206 187 176 155 96% Example 4 206 184 171 153 94% Comparative Example 1 201 173 150 127 64%
[0095] Among them, “—” indicates short circuit.
[0096] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0097] The electrolyte membranes of Examples 1 to 4 are superior to those of Comparative Example 1 in terms of mechanical strength and bending strength, indicating that the electrolyte membranes prepared by the preparation method of the composite sulfide electrolyte membrane of this embodiment have better mechanical properties. Under different test conditions, the electrolyte membranes of Examples 1 to 4 are superior to those of Comparative Example 1 in terms of capacity retention and discharge capacity at different rates, indicating that the electrolyte membranes prepared by the preparation method of the composite sulfide electrolyte membrane of this embodiment have better electrochemical stability and performance.
Claims
1. A method for preparing a composite sulfide electrolyte membrane, characterized in that: The following steps are involved: an ionic liquid mixing step, mixing the first ionic liquid and the second ionic liquid to obtain an ionic liquid mixture; a lithium salt adding step, adding a lithium salt to the ionic liquid mixture to obtain a high-concentration ionic liquid; A mixing step of mixing a sulfide electrolyte and a solvent in the high-concentration ionic liquid to obtain a slurry; A membrane forming step, coating the slurry and drying it under a first drying condition to obtain a preliminary composite electrolyte membrane; The polymerization step is to polymerize the preliminary composite electrolyte membrane by ultraviolet light initiation to obtain a composite sulfide electrolyte membrane.
2. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The first ionic liquid comprises a cation having the following structural formula: Wherein, the structure of R1 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the first ionic liquid is FSI - TFSI - , BF - 4.
3. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The second ionic liquid comprises a cation having the following structural formula: Wherein, the structure of R2 is a carbon chain composed of C1-C4, and the carbon chain contains at least one ester group, and the anion structure of the second ionic liquid is FSI - TFSI - , BF - 4.
4. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The lithium salt includes any one or a combination of the following: LiFSI, LiTFSI, LiBF4; And / or, the sulfide electrolyte includes any one of the following: Li3PS4,Li 10 GeP2S 12 ,Li7P3S 11 ; And / or, the solvent includes any one of the following: Alkanes with 6 to 10 carbon atoms, carboxylates with 6 to 16 carbon atoms, toluene and xylene.
5. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The concentration of the lithium salt in the high-concentration ionic liquid is ≥2 mol / L.
6. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The mass ratio of the first ionic liquid to the second ionic liquid is 1:(2-3).
7. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: In the mixing step, the mixing method used includes any one of the following: Ball mill mixing, homogenizer mixing, stirring mixing.
8. The method for preparing a composite sulfide electrolyte membrane according to claim 1, characterized in that: The first drying condition is baking, the baking temperature is 80° C.-120° C., and the baking time is ≥12 hours.
9. A composite sulfide electrolyte membrane, characterized in that: The sulfide electrolyte membrane is prepared by the preparation method according to any one of claims 1 to 8.
10. A lithium ion battery comprising a separator, characterized in that: The separator is the composite sulfide electrolyte membrane according to claim 10.
Citation Information
Patent Citations
An electrolyte for secondary lithium battery and secondary lithium battery using this electrolyte
CN101087035A
Gel-type polymer electrolyte used for lithium-sulfur secondary battery system and preparation method
CN102130364A
Photo-cured solid state composite electrolyte and preparation method thereof
CN109786812A
High-voltage-resistant ionic liquid lithium battery electrolyte and lithium battery
CN110416617A
Composite gel polymer electrolyte and preparation method and application thereof
CN110444807A