Method for recycling all resources of waste lithium batteries

Through charged crushing and extraction-precipitant separation technology under an inert atmosphere, combined with distillation and solid-liquid separation, the problems of wastewater pollution, difficulty in recycling organic matters and reduced electrolytes in lithium battery recycling are solved, and efficient and environmentally friendly recycling of all lithium battery resources is achieved. , improving recycling rate and resource utilization rate.

CN119092869AInactive Publication Date: 2024-12-06QINGDAO QINDACHENG TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411201868.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium battery recycling technology has problems such as wastewater pollution after battery crushing, difficulty in recycling organic matter, reduced value of electrolytes, and low separation efficiency of metal foils. Most existing processes have pyrolysis or high-temperature processes that lead to waste of resources and environmental pollution.

Method used

The lithium battery is charged to crush under an inert atmosphere, and the electrolyte and binder are separated by extraction agent and precipitant agent. The LiPF6 electrolyte and positive and negative electrode binder are recovered through distillation and solid-liquid separation technology, and the LiPF6 electrolyte and positive and negative electrode binder are recovered through wind power sorting and metal sorting Technology separates copper and aluminum metals, and the entire process has no pyrolysis process.

Benefits of technology

It has achieved efficient and environmental protection in the full resource recycling of lithium batteries, and the effective recycling of fluorine-containing compounds such as electrolytes and binders, reducing pollution and equipment requirements in the subsequent exhaust gas recovery process, and improving recovery and resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092869A_ABST
    Figure CN119092869A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of waste lithium battery recycling, and particularly relates to a method for recycling all resources of waste lithium batteries. According to the recycling method, the waste charged lithium battery is charged and crushed under the protection of inert atmosphere to obtain coarse waste battery particles, and LiFP6 electrolyte, positive and negative electrode powder, a positive electrode binder, a negative electrode binder, a diaphragm, a negative electrode copper current collector and a positive electrode aluminum current collector are recycled step by step. Electrolytes such as LiFP6 in the waste battery are recovered in a product form, the recovered diaphragm can be returned to a diaphragm enterprise, and a copper current collector and an aluminum current collector are respectively recovered in a copper particle form and an aluminum particle form. According to the recycling method disclosed by the invention, fluorine-containing compounds such as electrolytes and binders in the waste lithium batteries can be effectively recycled, harmful pollutants such as hydrofluoric acid are not generated in the recycling process, and the requirements on equipment and the like in the subsequent tail gas recycling process are reduced. The whole waste lithium battery resource recycling process is free of pyrolysis, efficient, environmentally friendly, high in recycling rate and high in value of recycled products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste lithium battery recycling, and specifically relates to a method for full resource recycling of waste lithium batteries. Background Art

[0002] In recent years, with the increasing consumption of fossil fuels and people's increasing environmental awareness, chemical power sources have been widely used as alternative energy sources, especially in the field of electric vehicles. my country has become the world's largest producer and seller of new energy vehicles. The rapid growth of power lithium batteries means that the demand for the treatment of waste batteries is also increasing. The service life of new energy vehicle power batteries is about 5-8 years, and my country will usher in a climax of battery scrapping.

[0003] Lithium batteries are mainly composed of shells, positive electrode materials, negative electrode materials, current collectors, diaphragms and electrolytes, all of which are valuable components worth recycling. If they are not decomposed and recycled, it will be a huge loss of resources. At present, the domestic waste power lithium battery recycling industry is still in its initial exploratory stage. The degree of automated disassembly of power batteries is low. If the battery protective shell is not separated from the battery matrix properly, it will cause the circuit to catch fire or even explode.

[0004] There are two types of battery crushing methods: post-discharge crushing and charged crushing. However, since post-discharge crushing requires the use of a salt water pool for discharge, the processing time is very long, the area occupied is large, and a lot of salt-containing wastewater needs to be treated. At the same time, because the remaining power of the recovered batteries is different, if all are completely discharged, it will cause useless work. In addition, after the battery is damaged during immersion, the organic matter in the battery cannot be recovered (CN 108525817A, CN 113856842A, CN 113856842A). Regarding the recovery of valuable components in waste batteries, the following methods are usually used: (1) High-temperature pyrolysis method, that is, high-temperature roasting of power batteries that have undergone simple mechanical crushing, screening to obtain fine powders containing metals and metal oxides. The high-temperature pyrolysis method is relatively simple in industry and suitable for large-scale processing, but the decomposition of electrolytes and other components produces harmful pollutants, which are easy to cause air pollution. At the same time, this method cannot effectively utilize materials such as electrolytes and binders. (2) Wet chemical method, that is, the waste power batteries are crushed and then selectively dissolved with appropriate chemical reagents to separate the metal elements in the leaching solution. The wet chemical method has good process stability and is suitable for small and medium-scale recycling, but the cost is high and the waste liquid needs further treatment, otherwise it will also cause environmental pollution. (3) Physical disassembly method, that is, the waste power batteries are crushed, screened, magnetically separated and classified to obtain high-content substances for the next step of recycling. The physical disassembly method is very environmentally friendly and will not cause secondary pollution to the environment, but the processing efficiency is extremely low and time-consuming.

[0005] At present, the technical problems existing in battery recycling mainly include: (1) When the battery is broken after being discharged by soaking in salt water or water, not only will the wastewater generated after soaking cause environmental pollution, but it will also cause the problem that the organic matter in the battery cannot be recycled. (2) The recovery process of electrolytes such as lithium hexafluorophosphate in the electrolyte destroys the electrolyte molecules, greatly reducing the value of the electrolyte. For example, in the waste lithium battery recycling methods disclosed in patents CN 110203949 A, CN 111430832 B, CN 116692910 A, and CN 115490220 A, the electrolyte is finally recovered in the form of low-value lithium carbonate, calcium fluoride, and calcium phosphate. (3) The key to the full recycling of lithium batteries lies in how to effectively separate copper and aluminum metal foils and battery powder. The thickness of the positive and negative aluminum foils and copper foils of lithium batteries is only tens of microns. When peeling the battery powder from the copper and aluminum foils, it is also necessary to avoid excessive crushing of the copper and aluminum foils, which will affect the purity of the battery powder. At this stage, the main processes include friction de-powdering, pyrolysis, and solvent methods. The electrode powder obtained by the friction de-powdering process has high copper and aluminum contents, which greatly increases the subsequent metal recycling cost; the pyrolysis method will produce highly corrosive media such as hydrogen fluoride and cause waste of resources; the existing solvent method only considers separation, aluminum metal foil, and battery powder, but does not consider the separation of solvent and binder and the recycling of binder, nor does it consider the recycling of diaphragm.

[0006] Therefore, it is urgent to find a method for recycling waste lithium batteries that is simple to operate, has a high resource recovery rate, and is efficient and environmentally friendly. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for recycling waste lithium batteries. The whole process does not involve a pyrolysis process, is highly efficient and environmentally friendly, and has a high recovery rate. The technical solution adopted is:

[0008] A method for recycling all waste lithium batteries, characterized in that it comprises the following steps:

[0009] (1) crushing the waste charged lithium-ion batteries under the protection of an inert atmosphere to obtain coarse waste battery particles;

[0010] (2) adding an extractant I to the coarse waste battery particles to extract the electrolyte; then, separating the remaining fragments I by screening; and then obtaining the extract I and the positive and negative electrode powders I by solid-liquid separation; the remaining fragments I include a separator, a positive and negative electrode current collector with positive and negative electrode powders and a positive and negative electrode binder;

[0011] The extract I is distilled to recover the extractant I and the residue I; the residue I includes LiPF6 electrolyte, ethylene carbonate, propylene carbonate, trimethyl phosphate, vinylene sulfate, etc.;

[0012] After filtering the residue I to remove the insoluble matter, the residue I is added to the precipitation agent I, and the filtrate I and the solid are obtained by solid-liquid separation. The solid is dried to obtain the LiPF6 electrolyte; the filtrate I includes the precipitation agent I and ethylene carbonate, propylene carbonate, trimethyl phosphate, vinylidene sulfate, etc.; the filtrate I is distilled, and the precipitation agent I is recovered and recycled;

[0013] (3) adding the remaining fragments I to the extractant II for treatment to dissolve the positive and negative electrode binders, thereby separating the positive and negative electrode powders from the positive and negative electrode current collectors; subsequently, separating the remaining fragments II by screening, and then performing solid-liquid separation to obtain an extract II and positive and negative electrode powders II; wherein the remaining fragments II include a separator and positive and negative electrode current collectors;

[0014] The extract II is distilled to recover the extractant II and the residue II; the residue II includes the positive electrode binder and the negative electrode binder; after filtering the residue II to remove the insoluble matter, the residue II is added to the precipitation agent II, and the filtrate II and the solid are obtained by solid-liquid separation, and the positive electrode binder is obtained after the solid is dried; the filtrate II includes the precipitation agent II and the negative electrode binder;

[0015] The filtrate II is distilled to recover the precipitation agent II for recycling, and the residue is dried to obtain the negative electrode binder;

[0016] (4) drying the remaining fragments II and performing wind separation to separate the separator to obtain the remaining fragments III; the remaining fragments III include positive and negative electrode powders, negative electrode copper current collector and positive electrode aluminum current collector;

[0017] (5) Screening the remaining fragments III to separate the positive and negative electrode powders III to obtain the remaining fragments IV. The remaining fragments IV include the negative electrode copper current collector and the positive electrode aluminum current collector;

[0018] (6) The remaining fragment IV is subjected to metal separation to obtain a negative electrode copper current collector and a positive electrode aluminum current collector.

[0019] Preferably, in step (1), the inert atmosphere is one of nitrogen, helium or argon.

[0020] Preferably, in the step (2), the mass ratio of the extractant I to the coarse waste battery particles is 0.5:1 to 10:1, the treatment refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent thermal, the treatment temperature is 0 to 80°C, and the treatment time is 0.1 to 48h; after being added to the precipitation agent I, the mass ratio of the residue I after filtering to remove the insoluble matter to the precipitation agent I is 0.2:1 to 10:1, and the precipitation conditions are -30 to 30°C and the precipitation time is 0.1-48h.

[0021] More preferably, the mass ratio of the extractant I to the coarse waste battery particles is 2:1 to 8:1, the treatment temperature is 30 to 60°C, and the treatment time is 1 to 4 hours; after being added to the precipitation agent I, the mass ratio of the residue I after filtering out the insoluble matter to the precipitation agent I is 0.5:1 to 3:1, and the precipitation conditions are -30 to 10°C and the precipitation time is 2 to 5 hours.

[0022] Preferably, in the step (2), the extracting agent I is at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, dichloromethane, chloroform, dichloroethane, acetonitrile, acetone, ether, and ethylene glycol dimethyl ether; the precipitating agent I is at least one of dichloromethane, chloroform, tetrachloromethane, dichloroethane, benzene, toluene, xylene, hexane, cyclohexane, isooctane, acetonitrile, acetone, ether, ethylene glycol dimethyl ether, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, and tetrahydrofuran.

[0023] Preferably, in the step (3), the mass ratio of the extractant II to the remaining fragments I is 0.5:1-10:1, the treatment refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent heat, the treatment temperature is 0-130°C, and the treatment time is 0.1-48h; after adding to the precipitation agent II, the mass ratio of the residue II to the precipitation agent II after filtering to remove the insoluble matter is 0.2:1-20:1, and the precipitation conditions are 0-50°C and the precipitation time is 0.1-48h. More preferably, the mass ratio of the extractant II to the remaining fragments I is 2:1-8:1, the treatment temperature is 30-130°C, and the treatment time is 1-5h; after adding to the precipitation agent II, the mass ratio of the precipitation agent II to the residue II after filtering to remove the insoluble matter is 0.5:1-3:1, and the precipitation conditions are 10-30°C and the precipitation time is 0.5-2h.

[0024] Preferably, in step (3), the extractant II is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, tetrachloromethane, dichloroethane, benzene, toluene, xylene, hexane, cyclohexane, isooctane, acetonitrile, acetone, tetrahydrofuran, water, methanol, ethanol, propanol, and isopropanol; the precipitating agent II is at least one of water, methanol, ethanol, propanol, isopropanol, dichloromethane, chloroform, tetrachloromethane, dichloroethane, dichloroethylene, trichloroethylene, tetrachloroethylene, acetonitrile, acetone, ether, ethylene glycol dimethyl ether, petroleum ether, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, and tetrahydrofuran. The solid-liquid separation is at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, and spray drying.

[0025] Preferably, in steps (2) and (3), the solid-liquid separation is at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, and spray drying.

[0026] Preferably, in step (4), the wind separation method is cyclone separation, the stirring speed is 200-500 r / min, and the air flow speed is 5-10 m / s.

[0027] Preferably, in step (5), during screening, the sieve aperture is 40-250 mesh.

[0028] Preferably, in step (6), the metal separation method is at least one of an airflow specific gravity separator, an airflow specific gravity separator with a vibration motor, an airflow specific gravity separator with electrostatic separation, an aluminum foil metal separator, and an eddy current magnetic separator.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The recycling method of the present invention is applicable to waste lithium batteries such as waste charged lithium iron phosphate batteries, waste charged lithium cobalt oxide batteries, waste charged lithium manganese oxide batteries, waste charged nickel cobalt manganese oxide batteries, waste charged nickel cobalt aluminum oxide batteries, and waste charged lithium titanate batteries.

[0031] By adopting the recycling method of the present invention, electrolytes such as LiFP6 in waste batteries are recovered in the form of products, and the diaphragm can be returned to the diaphragm enterprise after recovery and continue to serve as materials for preparing diaphragms or other products. Copper and aluminum current collectors are recovered in the form of copper particles and aluminum particles, respectively. The positive electrode binder in the waste battery is recovered and can be reused as a positive electrode binder for lithium batteries, and can also be used as wires and cables, filter materials, building materials, etc. The positive and negative electrode powders are recovered and can be used for electrolysis of water, fuel cells, lithium-air battery catalysts, etc., and can also be used as lithium battery pole powders after repair, or metals can be recovered by hydrometallurgy.

[0032] The recycling method of the present invention can effectively recover fluorine-containing compounds such as electrolytes and binders in waste batteries, does not produce highly corrosive and harmful pollutants such as hydrofluoric acid, and reduces the requirements for equipment and the like in the subsequent tail gas recovery process. The whole resource recovery process of waste lithium batteries of the present invention is free of pyrolysis, is highly efficient and environmentally friendly, has a high recovery rate, and has a high value of the recovered products. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a flow chart of the method.

[0034] Figure 2 This is a physical picture of the recycled lithium hexafluorophosphate.

[0035] Figure 3 This is a physical picture of the recycled positive and negative electrode powders.

[0036] Figure 4 This is a physical picture of the recycled diaphragm.

[0037] Figure 5 This is a physical picture of the recycled positive electrode binder.

[0038] Figure 6 This is a physical picture of the recycled negative electrode binder. DETAILED DESCRIPTION

[0039] The accompanying drawings are for illustrative purposes only; the present invention is further described in detail below through examples in combination with the accompanying drawings, but they should not be construed as limiting the present invention. Without departing from the spirit and substance of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0040] Example 1

[0041] like Figure 1 As shown, first, the shell of the recycled charged waste lithium iron phosphate battery is removed in advance and the battery pack is taken out.

[0042] Step (1): Take one of the battery packs (275 g) and crush the waste lithium iron phosphate battery in a new inert gas protection atmosphere system with electricity to crush it into coarse waste battery particles with a size of about 1 square centimeter.

[0043] Step (2): Recycling of waste electrolyte, comprising the following steps:

[0044] In the first step, the coarsely crushed waste battery particles in step (1) are added to a mixed solution of 250g dimethyl carbonate and 250g methyl ethyl carbonate (extractant I), and the ultrasonic temperature is 30°C, the power is 150W, and the frequency is 40KHz. The ultrasonic process is carried out for 2h. After sieving, the larger fragments are sieved out, and the above operation can be repeated once. The fragments sieved out twice are combined to obtain the remaining fragments I. The sieved components are centrifuged to obtain positive / negative electrode powder I and extract I. The remaining fragments I include a separator, a positive and negative electrode current collector with positive and negative electrode powder and a positive and negative electrode binder, and the extract I includes dissolved LiPF6, dimethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, diethyl carbonate, trimethyl phosphate, vinylene sulfate, etc.

[0045] In the second step, the extract I is subjected to reduced pressure distillation to obtain an extractant I and a residue I. The temperature of the reduced pressure distillation is 60°C and the pressure is 150Pa. The residue I includes LiPF6, ethylene carbonate, propylene carbonate, trimethyl phosphate, vinylene sulfate, etc.

[0046] In the third step, the residue I was centrifuged to remove insoluble matter, and added to ether (precipitating agent I) at a ratio of 1:1. The solution temperature was then lowered to -25°C. The product was crystallized for 5 hours and vacuum dried to obtain 4.5g of LiPF6 electrolyte.

[0047] Step (3): Recycling of the separator and the positive and negative electrode materials, comprising the following steps:

[0048] In the first step, 150 g of N-methylpyrrolidone, 150 g of dimethyl sulfoxide and 150 g of ethanol (extractant II) are added to the remaining fragments I in step (2), and the power is 150 W, the frequency is 40 KHz, and the temperature is 60° C. Ultrasonication is performed for 5 hours. After sieving, the above operation is repeated twice to obtain the remaining fragments II. After centrifugation, positive / negative electrode powder 2 and extract II are obtained. Extract II includes N-methylpyrrolidone, dimethyl sulfoxide, ethanol, positive electrode binder and negative electrode binder.

[0049] In the second step, the extract II is subjected to reduced pressure distillation to obtain an extractant II and a residue II. The temperature of the reduced pressure distillation is 90°C and the pressure is 150 Pa. The residue II includes a positive electrode binder and a negative electrode binder.

[0050] In the third step, after removing the insoluble matter from the centrifugal residue II, ethanol (precipitating agent II) was added at a ratio of 1:1 at room temperature. After 1 hour, 1.5 g of positive electrode binder was obtained by centrifugal drying. The filtrate was distilled to recover ethanol, and the residue was dried to obtain 1.7 g of negative electrode binder.

[0051] Step (4): After drying the remaining fragments II after extraction in step (3), wind separation is carried out. The air flow speed used by the wind separator is 5m / s to obtain the remaining fragments III (fragment III is positive and negative electrode powder, copper particles, aluminum particles) and 5g of separator.

[0052] Step (5): The remaining fragments III in step (4) are screened to obtain positive and negative electrode powders III and remaining fragments IV, and the mesh size of the oscillating separation screen is 300 meshes.

[0053] Step (6): The remaining fragment IV in step (5) is subjected to gravity screening to obtain 18 g of copper particles and 39 g of aluminum particles.

[0054] Step (7): Combine the positive and negative electrode powders I in step (2), the positive and negative electrode powders II in step (3), and the positive and negative electrode powders IV in step (5) to obtain 165 g of positive and negative electrode powders.

[0055] like Figure 2-6 Shown are physical pictures of lithium hexafluorophosphate, positive and negative electrode powders, separators, positive electrode binders, and negative electrode binders recovered by the present invention.

[0056] The recovery rates of LiPF6, negative electrode binder, positive electrode binder, separator, positive and negative electrode powders, negative electrode copper current collector and positive electrode aluminum current collector in this embodiment are 87%, 95%, 96%, 99%, 99%, 99% and 98% respectively.

[0057] Embodiment 2-5,

[0058] Compared with Example 1, the only difference is that the ultrasonic temperature in step (2) is 20°C (Example 2), 40°C (Example 3), 50°C (Example 4), and 60°C (Example 5), and the ultrasonic treatment is performed for 2 hours. The electrolyte LiPF6 obtained is 4.2g, 4.6g, 4.8g, and 4.6g, respectively. This shows that the ultrasonic temperature has an effect on the extraction of electrolyte, but the temperature cannot be too high. If it is too high, the extractant I is easy to evaporate or reach the boiling point.

[0059] Embodiment 6-10

[0060] Compared with Example 1, the only difference is that the ultrasonic temperature in step (2) is set to 30°C, and the ultrasonic time is 0.5h (Example 6), 1h (Example 7), 4h (Example 8), 8h (Example 9), and 10h (Example 10), respectively, and the electrolyte LiPF6 obtained is 3.8g, 4.1g, 4.7g, 4.8g, and 4.8g, respectively. The longer the ultrasonic time, the more electrolyte is recovered, but the time cost needs to be considered.

[0061] Embodiment 11

[0062] Compared with Example 1, the only difference is that 250 g of dimethyl carbonate and 250 g of ethyl methyl carbonate (extractant 1) in step (2) are replaced by 500 g of ethyl methyl carbonate. Under this condition, the weight of the electrolyte obtained in step (2) is 4.6 g. The electrolyte recovery rate in this example reaches 88%.

[0063] Example 12

[0064] Compared with Example 11, the only difference is that the ultrasonic temperature in step (2) is set to 50°C, the ultrasonic time is set to 10 h, and the amount of ether (precipitating agent I) added is changed from 10:1 to 5:1. Under this condition, the weight of the electrolyte obtained in step (2) is 4.7 g.

[0065] Embodiment 13

[0066] Compared with Example 11, the only difference is that 150 g of N-methylpyrrolidone, 150 g of dimethyl sulfoxide and 150 g of ethanol (extractant II) in step (3) are replaced by 150 g of N-methylpyrrolidone, 150 g of N,N-dimethylformamide and 150 g of ethanol, the ultrasonic temperature is set to 70°C, and the ultrasonic time is 12 h. Under these conditions, the weights of the positive electrode binder and the negative electrode binder obtained in step (3) are 1.6 g and 1.7 g, respectively.

[0067] Examples 14-17

[0068] Compared with Example 13, the only difference is that the ultrasonic time is 8h (Example 14), 15h (Example 15), 20h (Example 16), and 30h (Example 17). Under this condition, the weights of the positive electrode binders obtained in step (3) are 1.6g, 1.6g, 1.7g, and 1.7g, respectively, and the weights of the negative electrode binders obtained are 1.7g, 1.7g, 1.8g, and 1.8g, respectively.

[0069] Embodiment 17

[0070] Compared with Example 13, the only difference is that ethanol (precipitating agent II) in step (3) is replaced by water. Under this condition, the weights of the positive electrode binder and the negative electrode binder obtained in step (3) are 1.6 g and 1.7 g, respectively.

[0071] Through examples, it is shown that the method of the present invention has mild conditions, is easy to operate, has a simple process, does not require complex equipment, and each process parameter is easy to achieve. It has the advantages of high efficiency, no pollution, high recovery rate, etc. At the same time, all resources are recovered for battery materials, avoiding waste of resources and pollution of the environment. The solvent used for recovery can be recycled and reused repeatedly, reducing costs, and can be recycled and processed in large quantities.

[0072] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for recycling all waste lithium batteries, characterized in that: The steps include: (1) crushing the waste charged lithium-ion batteries under the protection of an inert atmosphere to obtain coarse waste battery particles; (2) adding an extractant I to the coarse waste battery particles to extract the electrolyte; then, separating the remaining fragments I by sieving; After solid-liquid separation, extract I and positive and negative electrode powders I are obtained; The remaining fragments I include the separator, the positive and negative electrode current collectors with positive and negative electrode powders and positive and negative electrode binders; The extract I is distilled to recover the extractant I and the residue I; After filtering the residue I to remove the insoluble matter, the residue I is added to the precipitation agent I, and after solid-liquid separation, the obtained solid is dried to obtain the LiPF6 electrolyte, and the obtained liquid is the filtrate I, which is distilled to recover the precipitation agent I for recycling; (3) adding the remaining fragments I to the extractant II for treatment to dissolve the positive and negative electrode binders, thereby separating the positive and negative electrode powders from the positive and negative electrode current collectors; subsequently, separating the remaining fragments II by screening, and then performing solid-liquid separation to obtain an extract II and positive and negative electrode powders II; wherein the remaining fragments II include a separator and positive and negative electrode current collectors; The extract II is distilled to recover the extractant II and the residue II; after filtering the residue II to remove the insoluble matter, the residue II is added to the precipitation agent II, and after solid-liquid separation, the obtained solid is dried to obtain the positive electrode binder, and the obtained liquid is the filtrate II; The filtrate II is distilled to recover the precipitation agent II for recycling, and the residue is dried to obtain the negative electrode binder; (4) drying the remaining fragments II and performing wind separation to separate the diaphragm to obtain the remaining fragments III; (5) Screening the remaining fragments III to separate the positive and negative electrode powders III to obtain the remaining fragments IV; (6) The remaining fragment IV is subjected to metal separation to obtain a negative electrode copper current collector and a positive electrode aluminum current collector.

2. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (1), the inert atmosphere is at least one of nitrogen, helium or argon.

3. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (2), the mass ratio of the extractant I to the coarse waste battery particles is 2 to 8:1, the treatment method is at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent thermal, the treatment temperature is 20 to 50°C, and the treatment time is 1 to 5 hours; the extractant I is added to the precipitation agent I, and the mass ratio of the precipitation agent I to the residue I after filtering to remove insoluble matter is 0.5 to 3:1, and the precipitation conditions are -30 to 10°C and the precipitation time is 0.5 to 2 hours.

4. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (2), the extracting agent I is at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, dichloromethane, chloroform, dichloroethane, acetonitrile, acetone, ether, and ethylene glycol dimethyl ether; the precipitating agent I is at least one of dichloromethane, chloroform, tetrachloromethane, dichloroethane, benzene, toluene, xylene, hexane, cyclohexane, isooctane, acetonitrile, acetone, ether, ethylene glycol dimethyl ether, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, and tetrahydrofuran.

5. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (3), the mass ratio of the added extractant II to the remaining fragments I is 2 to 8:1, the treatment method is at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent thermal, the treatment temperature is 30 to 130°C, and the treatment time is 1 to 5 hours; after being added to the precipitation agent II, the mass ratio of the precipitation agent II to the residue II after filtering and removing the insoluble matter is 0.5 to 3:1, and the precipitation conditions are at 10 to 30°C and the precipitation time is 0.5 to 2 hours.

6. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (3), the extractant II is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, tetrachloromethane, dichloroethane, benzene, toluene, xylene, hexane, cyclohexane, isooctane, acetonitrile, acetone, tetrahydrofuran, water, methanol, ethanol, propanol, and isopropanol; the precipitating agent II is at least one of water, methanol, ethanol, propanol, isopropanol, dichloromethane, chloroform, tetrachloromethane, dichloroethane, dichloroethylene, trichloroethylene, tetrachloroethylene, acetonitrile, acetone, ether, ethylene glycol dimethyl ether, petroleum ether, methyl formate, methyl acetate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, and tetrahydrofuran. The solid-liquid separation is at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, and spray drying.

7. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the steps (2) and (3), the solid-liquid separation is at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, and spray drying.

8. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (4), the wind separation method is cyclone separation, the stirring speed is 200-500 r / min, and the air flow speed is 5-10 m / s.

9. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (5), during screening, the sieve aperture is 40 to 250 meshes.

10. The method for full resource recycling of waste lithium batteries according to claim 1, characterized in that: In the step (6), the metal separation method is at least one of airflow specific gravity separation, airflow specific gravity separation with a vibration motor, airflow specific gravity separation with electrostatic separation, aluminum foil metal separation, and eddy current magnetic separation.

Citation Information

Patent Citations

  • Full-automatic waste lithium ion battery recycling process and system

    CN108110356A

  • Process for treating waste lithium battery for extracting electrolyte and binder by solvent

    CN109818097A

  • Waste power lithium battery all-component cleaning and recycling method

    CN110635191A

  • Multi-component recycling method for waste lithium ion battery

    CN115172925A

  • Method for all-resource step-by-step classified recovery of recyclable components of waste lithium battery

    CN119092870A