Magnetoelectric nonvolatile memory and preparation method thereof

By integrating FeRAM and MRAM and optimizing the process, the problem of MRAM magnetic moment regulation is solved, and the magnetoelectric non-volatile memory with low power consumption, high speed and durability is realized, the problem of high energy consumption of existing memory is solved, and production is reduced cost.

CN119095389APending Publication Date: 2024-12-06INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194843.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The high energy consumption of existing memories, especially magnetic random memory (MRAM), is high when writing, and becomes an obstacle to the alternative technology of static random memory (SRAM).

Method used

Magnetic non-volatile memory is used to integrate ferroelectric memory (FeRAM) and magnetic memory (MRAM), write operations through FeRAM, and use FeRAM to generate an electric field to change the direction of MRAM magnetization, realizing low-power and high-speed data transmission, and through Optimize magnetron sputtering process and etching process to grow ultra-thin bottom electrode layers, and accurately control etching stop points.

Benefits of technology

It realizes low power consumption (femtosecond level per bit of data transmission), high speed (nanosecond level) and high durability memory, while also has the advantages of non-destructive reading, and is compatible with CMOS processes, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095389A_ABST
    Figure CN119095389A_ABST
Patent Text Reader

Abstract

The invention relates to a magnetoelectric nonvolatile memory and a preparation method thereof, belongs to the technical field of semiconductor devices, and solves the problem of high energy consumption of an existing memory. The magnetoelectric nonvolatile memory comprises a ferroelectric memory and a magnetic memory, the structure comprises a ferroelectric bottom electrode layer, a ferroelectric layer, an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer which are sequentially arranged from bottom to top.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a magnetoelectric non-volatile memory and a preparation method thereof. Background Art

[0002] As computing speed increases, the area and static power consumption of static random access memory (SRAM) are increasing, and area and power consumption have become the main consumption of chips.

[0003] SRAM is a high-speed cache technology. Its functional integration density will slow down rapidly after the 5nm process, and its manufacturing cost will increase. Therefore, it is necessary to find an alternative technology to SRAM.

[0004] The performance of magnetic random access memory (MRAM) can cover the two core indicators of cache storage capacity and access speed. However, compared with SRAM, high write energy consumption is a great obstacle for MRAM to replace SRAM. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a magnetoelectric non-volatile memory and a preparation method thereof, so as to solve the problem of high energy consumption of existing memories.

[0006] The purpose of the present invention is mainly achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a magnetoelectric non-volatile memory, which includes a ferroelectric memory and a magnetic memory; its structure includes a ferroelectric bottom electrode layer, a ferroelectric layer, an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer arranged in sequence from bottom to top.

[0008] Optionally, the thickness of the ferroelectric layer is 8-12 nm.

[0009] Optionally, the material of the ferroelectric layer is Hf 0.5 Zr 0.5 O2.

[0010] Optionally, the material of the MRAM bottom electrode layer is W or Ta.

[0011] Optionally, the material of the pinning layer is a CoPt multilayer film with a thickness of 8-12 nm.

[0012] Optionally, the material of the hard mask layer is TiN or Ta.

[0013] In a second aspect, the present invention provides a method for preparing a magnetoelectric non-volatile memory, which is used to obtain the above-mentioned magnetoelectric non-volatile memory, comprising the following steps:

[0014] Step 1: depositing a ferroelectric bottom electrode layer, a ferroelectric layer, and a top electrode layer in sequence, and annealing to form a ferroelectric phase;

[0015] Step 2: Etching to remove the top electrode and expose the ferroelectric layer;

[0016] Step 3: sequentially growing an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer on the ferroelectric layer to obtain a magnetic tunnel junction film; annealing to form a system with perpendicular magnetic anisotropy;

[0017] Step 4: Etching the tunnel junction;

[0018] Step 5: Protect the deposited medium of the processed tunnel junction;

[0019] Step 6: Process the MRAM bottom electrode and deposit a dielectric for protection;

[0020] Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain a magnetoelectric non-volatile memory.

[0021] Optionally, in step 4, the etching stops at the MRAM bottom electrode layer or the free layer.

[0022] Optionally, in step 1, the annealing temperature is 500-600°C.

[0023] In a third aspect, the present invention provides a method for reading and writing the above-mentioned magnetoelectric non-volatile memory, comprising: applying a write voltage between the tunneling layer and the ferroelectric bottom electrode layer, and using FeRAM to perform a write operation; applying a read voltage between the tunneling layer and the hard mask layer, and using MRAM to perform a read operation.

[0024] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0025] (1) The present invention innovatively proposes to integrate ferroelectric memory (FeRAM) and magnetic memory (MRAM) together, and to change the magnetization direction of MRAM by generating an electric field through FeRAM. The magnetoelectric non-volatile memory of the present invention uses FeRAM for writing operation and MRAM for reading operation, so that the memory of the present invention has low power consumption (the energy consumed per bit of data transmission is in the femtosecond (fJ) level), high speed (nanoseconds ns), high durability (10 12 times), and has the advantage of non-destructive reading.

[0026] (2) The difficulty of this memory is how to effectively regulate the magnetic moment of MRAM. Since MRAM is made of all metal, metal has a shielding effect on the electric field. Therefore, it is difficult for the electric field of the ferroelectric memory to reach the magnetic layer of the MRAM, and the magnetism cannot be regulated by the electric field. In order to solve the above technical problems, the present invention adopts an ultra-thin bottom electrode (<1nm) for this memory, so that the electric field can pass through the bottom electrode to reach the free layer of the MRAM. However, it is difficult to grow such a thin bottom electrode layer. The present invention optimizes the magnetron sputtering process and controls the process parameters within a specific range to eventually grow an ultra-thin bottom electrode layer.

[0027] In addition, since the bottom electrode layer is very thin, it is difficult to stop etching on the MRAM bottom electrode layer and the free layer, and the etching accuracy must be precisely controlled. The present invention can accurately control the etching to stop on the MRAM bottom electrode layer or the free layer by optimizing the etching process and controlling the process parameters within a specific range.

[0028] (3) The present invention is compatible with CMOS technology and does not require the development of new technology, which is beneficial to reducing production costs.

[0029] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can be obvious from the description or understood by practicing the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0031] Figure 1 A schematic diagram of the writing operation of the magnetoelectric non-volatile memory of the present invention;

[0032] Figure 2 A schematic diagram of a magnetoelectric non-volatile memory read operation of the present invention;

[0033] Figure 3 Schematic diagram of changing the magnetization direction of MRAM for magnetoelectric memory write operation. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0035] In a first aspect, the present invention provides a magnetoelectric nonvolatile memory, such as Figure 1 and Figure 2As shown, it includes a ferroelectric bottom electrode layer, a ferroelectric layer, an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer arranged in sequence from bottom to top, that is, the ferroelectric layer is arranged on the ferroelectric bottom electrode layer, the MRAM bottom electrode layer is arranged on the ferroelectric layer, the free layer is arranged on the MRAM bottom electrode layer, the tunneling layer is arranged on the free layer, the reference layer is arranged on the tunneling layer, the intermediate layer is arranged on the reference layer, the pinning layer is arranged on the intermediate layer, the protective layer is arranged on the pinning layer, and the hard mask layer is arranged on the protective layer. The pinning layer is used to pin the reference layer to a fixed direction.

[0036] Specifically, the material of the ferroelectric bottom electrode layer is W, Ta, etc., and the thickness is 8-12 nm, for example, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm.

[0037] The ferroelectric layer is a Hf-based ferroelectric layer with a thickness of 8-12 nm, for example, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, and is made of Hf 0.5 Zr 0.5 O2.

[0038] The material of the MRAM bottom electrode layer is W, Ta, etc., and the thickness is 0.3-1 nm, for example, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm.

[0039] The material of the free layer is CoFeB, and the thickness is 1-3 nm, for example, 1 nm, 1.2 nm, 1.5 nm, 1.8 nm, 2 nm, 2.2 nm, 2.5 nm, 2.7 nm, 2.8 nm, 3 nm.

[0040] The material of the tunneling layer is MgO, and the thickness is 0.8-3 nm, for example, 0.8 nm, 0.9 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm.

[0041] The material of the reference layer is a material with good magnetic properties, such as CoFeB. The thickness of the reference layer is 0.8-1.2 nm, for example, 0.8 nm, 0.9 nm, 1 nm, 1.1 nm, 1.2 nm.

[0042] The material of the intermediate layer is a non-magnetic material, such as W, Ta. The thickness of the intermediate layer is 0.5-0.8 nm, such as 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm.

[0043] It should be noted that the pinning layer is used to pin the reference layer to a fixed direction, and its material is a CoPt multilayer film with a thickness of 8-12 nm, for example, 8 nm, 9 nm, 10 nm, 11 nm, and 12 nm.

[0044] The function of the protective layer is to protect the MRAM structure from the external environment and prevent oxidation and other chemical reactions. The material of the protective layer is Ru, and the thickness is 3-7nm, for example, 3nm, 4nm, 5nm, 6nm, 7nm.

[0045] The material of the hard mask layer is TiN or Ta, and the thickness is 80-110nm, for example, 80nm, 90nm, 95nm, 100nm, 105nm, 110nm. In a second aspect, the present invention also provides a method for preparing a ferroelectric non-volatile memory, which is used to prepare the above-mentioned ferroelectric non-volatile memory, comprising the following steps:

[0046] Step 1: depositing a ferroelectric bottom electrode layer (8-12 nm), a ferroelectric layer (8-12 nm), and a top electrode layer (90-110 nm) on a Si wafer or a circuit wafer in sequence, and annealing to form a ferroelectric phase;

[0047] Step 2: Remove the top electrode by wet etching to expose the ferroelectric layer;

[0048] Step 3: Under vacuum conditions, a magnetron sputtering device is used to sequentially grow an MRAM bottom electrode layer (0.3nm-1nm), a free layer (1-3nm), a tunneling layer (0.8-3nm), a reference layer (0.8-1.2nm), an intermediate layer (0.5-0.8nm), a pinning layer (8-12nm), a protective layer (3-7nm) and a hard mask layer (100nm) on the ferroelectric layer to obtain a magnetic tunnel junction film; annealing is performed to form a system with good perpendicular magnetic anisotropy;

[0049] Step 4: Etching the tunnel junction; using an ICP etcher, the 100 nm thick hard mask layer is etched using the reaction gas CF4; then the tunnel junction is physically etched using the hard mask layer in an argon atmosphere;

[0050] Step 5: Protect the deposited medium of the processed tunnel junction;

[0051] Step 6: Process the MRAM bottom electrode and deposit dielectric for protection;

[0052] Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain an MRAM structure, and then obtain a magnetoelectric non-volatile memory.

[0053] Specifically, in step 1, the annealing temperature is 500-600° C., for example, 500° C., 520° C., 550° C., 570° C., 580° C., 590° C., 600° C. The annealing time is 0.5-1.5 h, for example, 0.5 h, 1 h, 1.5 h.

[0054] In step 3, the process parameters of magnetron sputtering are as follows:

[0055] The pressure is 6.5×10 -6 -1×10 -7 Torr, for example, 6.5 × 10 -6 Torr, 7×10 -6 Torr, 7.5×10 - 6 Torr, 8×10 -6 Torr, 8.5×10 -6 Torr, 9×10 -6 Torr, 9.5×10 -6 Torr, 1×10 -7 Torr.

[0056] The growth rate is 0.01-0.05 nm / s, for example, 0.01 nm / s, 0.02 nm / s, 0.03 nm / s, 0.04 nm / s, 0.05 nm / s.

[0057] The water cooling temperature is 15-18°C, for example, 15°C, 16°C, 17°C, 18°C.

[0058] In addition, in step 3, the annealing temperature is 300-400°C, for example, 300°C, 320°C, 350°C, 370°C, 400°C.

[0059] The annealing time is 80-100 s, for example, 80 s, 85 s, 90 s, 95 s, 100 s.

[0060] Specifically, in step 4, the etching stops at the free layer or the MRAM bottom electrode layer. The vacuum degree of the etching chamber is 0.5-1.5 mTorr, for example, 0.5 mTorr, 1 mTorr, 1.5 mTorr.

[0061] The etching temperature is -1 to 1°C, for example, -1°C, 0°C, 1°C.

[0062] The etching rate is 0.9-1.2 nm / s, for example, 0.9 nm / s, 1 nm / s, 1.1 nm / s, 1.2 nm / s.

[0063] It should be noted that, during the etching process of step 4, optical emission spectroscopy (OES) is used to monitor the composition of the etched film layer in real time, so as to timely know which layer of the tunnel junction is etched, and then control the etching to stop at the corresponding layer.

[0064] Specifically, step 5 includes: first depositing SiN, and then depositing SiO2 on the SiN, the thickness of the deposited SiN is 40-60nm, for example, 40nm, 45nm, 50nm, 55nm, 60nm. The thickness of the deposited / SiO2 is 290-310nm, for example, 290nm, 295nm, 300nm, 305nm, 310nm.

[0065] It should be pointed out that, unless otherwise specified, the processes and process parameters involved in the preparation method of the present invention all adopt the existing technology.

[0066] In a third aspect, the present invention also provides a method for reading and writing a ferroelectric non-volatile memory, using the above-mentioned magnetoelectric non-volatile memory for reading and writing, comprising: applying a write voltage ( Figure 1 and Figure 3 ), using FeRAM for write operation; applying a read voltage between the tunneling layer and the hard mask layer ( Figure 2 ), using MRAM for read operations.

[0067] The present invention integrates ferroelectric memory (FeRAM) and magnetic memory (MRAM) together, and changes the magnetization direction of MRAM by generating an electric field through FeRAM. The magnetoelectric non-volatile memory of the present invention uses FeRAM for writing operation and MRAM for reading operation, so that the memory of the present invention has low power consumption (the energy consumed for each bit of data transmission is at the femtosecond (fJ) level), high speed (nanoseconds ns), high durability (10 12 times), and has the advantage of non-destructive reading.

[0068] Example 1

[0069] Step 1: Deposit the ferroelectric bottom electrode layer (W, 8nm), ferroelectric layer (Hf 0.5 Zr 0.5 O2, 8nm), top electrode layer (90nm), annealing (500℃, 1.5h) to form ferroelectric phase;

[0070] Step 2: Remove the top electrode by wet etching to expose the ferroelectric layer;

[0071] Step 3: Under vacuum conditions, the MRAM bottom electrode layer (W, 0.3nm), free layer (CoFeB, 1nm), tunneling layer (MgO, 0.8nm), reference layer (CoFeB, 0.8nm), intermediate layer (W, 0.5nm), pinning layer (CoPt multilayer film, 8nm), protective layer (Ru, 3nm) and hard mask layer (TiN, 80nm) are grown on the ferroelectric layer in sequence using a magnetron sputtering device to obtain a magnetic tunnel junction film. The bottom electrode is placed in a vacuum of 6.5×10-6 Torr growth, the growth rate is 0.01nm / s, and the water cooling temperature of the equipment is 15°C. Then the tunnel junction is rapidly annealed at 300°C for 80s to form a system with good perpendicular magnetic anisotropy;

[0072] Step 4: Etching the tunnel junction; using an ICP etcher, the 80nm thick hard mask layer is etched using the reaction gas CF4; then the tunnel junction is physically etched using the hard mask layer in an argon atmosphere, the vacuum degree of the etching chamber is 0.5mTorr, the etching temperature is -1°C, and the etching rate is 0.9nm / s. OES is used to monitor the composition of the etched film layer in real time, and then analyze which layer of the tunnel junction is etched, and finally the etching stops at the MRAM bottom electrode layer;

[0073] Step 5: Protect the deposited medium of the processed tunnel junction;

[0074] Step 6: Process the MRAM bottom electrode and deposit dielectric for protection;

[0075] Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain an MRAM structure, and then obtain a magnetoelectric non-volatile memory.

[0076] Example 2

[0077] Step 1: Deposit the ferroelectric bottom electrode layer (Ta, 12nm), ferroelectric layer (Hf 0.5 Zr 0.5 O2, 12nm), top electrode layer (110nm), and then annealing (600℃, 0.5h) to form a ferroelectric phase;

[0078] Step 2: Remove the top electrode by wet etching to expose the ferroelectric layer;

[0079] Step 3: Under vacuum conditions, the MRAM bottom electrode layer (Ta, 1nm), free layer (CoFeB, 3nm), tunnel layer (MgO, 3nm), reference layer (CoFeB, 1.2nm), intermediate layer (Ta, 0.8nm), pinning layer (CoPt multilayer film, 12nm), protective layer (Ru, 7nm) and hard mask layer (TiN, 110nm) are grown on the ferroelectric layer in sequence using a magnetron sputtering device to obtain a magnetic tunnel junction film. The bottom electrode is placed in a vacuum of 1×10 -7 Torr, the growth rate is 0.05nm / s, and the water cooling temperature of the equipment is 18°C. Then the tunnel junction is rapidly annealed at 300°C for 100s to form a system with good perpendicular magnetic anisotropy;

[0080] Step 4: Etching the tunnel junction; using an ICP etcher, the 110nm thick hard mask layer is etched using the reaction gas CF4; then the tunnel junction is physically etched using the hard mask layer in an argon atmosphere, the vacuum degree of the etching chamber is 1.5mTorr, the etching temperature is 1°C, the etching rate is 1.2nm / s, and the composition of the etched film layer is monitored in real time using OES, and then the layer of the tunnel junction that is etched is analyzed, and finally the etching stops at the free layer;

[0081] Step 5: Protect the deposited medium of the processed tunnel junction;

[0082] Step 6: Process the MRAM bottom electrode and deposit dielectric for protection;

[0083] Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain an MRAM structure, and then obtain a magnetoelectric non-volatile memory.

[0084] Example 3

[0085] Step 1: Deposit the ferroelectric bottom electrode layer (W, 10nm), ferroelectric layer (Hf 0.5 Zr 0.5 O2, 10nm), top electrode layer (100nm), and then annealing (550℃, 1h) to form a ferroelectric phase;

[0086] Step 2: Remove the top electrode by wet etching to expose the ferroelectric layer;

[0087] Step 3: Under vacuum conditions, the MRAM bottom electrode layer (W, 0.5nm), free layer (CoFeB, 2nm), tunneling layer (MgO, 1nm), reference layer (CoFeB, 1nm), intermediate layer (W, 0.7nm), pinning layer (CoPt multilayer film, 10nm), protective layer (Ru, 5nm) and hard mask layer (TiN, 100nm) are grown on the ferroelectric layer in sequence using a magnetron sputtering device to obtain a magnetic tunnel junction film. The bottom electrode is placed in a vacuum of 8×10 -6 Torr growth, the growth rate is 0.03nm / s, and the water cooling temperature of the equipment is 16°C. Then the tunnel junction is rapidly annealed at 350°C for 90s to form a system with good perpendicular magnetic anisotropy;

[0088] Step 4: Etching the tunnel junction; using an ICP etcher, the 100nm thick hard mask layer is etched using the reaction gas CF4; then the tunnel junction is physically etched using the hard mask layer in an argon atmosphere, the vacuum degree of the etching chamber is 1mTorr, the etching temperature is 0°C, the etching rate is 1nm / s, and the composition of the etched film layer is monitored in real time using OES, and then the layer of the tunnel junction that is etched is analyzed, and finally the etching stops at the MRAM bottom electrode layer;

[0089] Step 5: Protect the deposited medium of the processed tunnel junction;

[0090] Step 6: Process the MRAM bottom electrode and deposit a dielectric for protection;

[0091] Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain an MRAM structure, and then obtain a magnetoelectric non-volatile memory.

[0092] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A magnetoelectric non-volatile memory, It is characterized in that The magnetoelectric nonvolatile memory includes a ferroelectric memory and a magnetic memory; its structure includes a ferroelectric bottom electrode layer, a ferroelectric layer, an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer arranged in sequence from bottom to top.

2. The magnetoelectric nonvolatile memory according to claim 1, It is characterized in that The thickness of the ferroelectric layer is 8-12nm.

3. The magnetoelectric nonvolatile memory according to claim 1, It is characterized in that The material of the ferroelectric layer is Hf 0.5 Zr 0.5 O 2 .

4. The magnetoelectric nonvolatile memory according to claim 1, It is characterized in that The material of the MRAM bottom electrode layer is W or Ta.

5. The magnetoelectric non-volatile memory according to any one of claims 1 to 4, It is characterized in that The material of the pinning layer is a CoPt multilayer film with a thickness of 8-12nm.

6. The magnetoelectric nonvolatile memory according to claim 5, It is characterized in that The material of the hard mask layer is TiN or Ta.

7. A method for preparing a magnetoelectric non-volatile memory, It is characterized in that The method for obtaining the magnetoelectric non-volatile memory according to any one of claims 1 to 6 comprises the following steps: Step 1: depositing a ferroelectric bottom electrode layer, a ferroelectric layer, and a top electrode layer in sequence, and annealing to form a ferroelectric phase; Step 2: Etching to remove the top electrode and expose the ferroelectric layer; Step 3: sequentially growing an MRAM bottom electrode layer, a free layer, a tunneling layer, a reference layer, an intermediate layer, a pinning layer, a protective layer and a hard mask layer on the ferroelectric layer to obtain a magnetic tunnel junction film; annealing to form a system with perpendicular magnetic anisotropy; Step 4: Etching the tunnel junction; Step 5: Protect the deposited medium of the processed tunnel junction; Step 6: Process the MRAM bottom electrode and deposit a dielectric for protection; Step 7: Use CMP to planarize, expose the top and bottom electrodes, deposit metal, and etch the electrodes to obtain a magnetoelectric non-volatile memory.

8. The preparation method according to claim 7, It is characterized in that In step 4, etching stops at the MRAM bottom electrode layer or the free layer.

9. The preparation method according to claim 7, It is characterized in that In step 1, the annealing temperature is 500-600°C.

10. A method for reading and writing a magnetoelectric non-volatile memory according to any one of claims 1 to 6, It is characterized in that include: A write voltage is applied between the tunneling layer and the ferroelectric bottom electrode layer, and a write operation is performed using the FeRAM; A read voltage is applied between the tunneling layer and the hard mask layer, and a read operation is performed using the MRAM.