Wafer-level electrochemical transistor array and preparation method thereof
By introducing flexible substrate layer and patterned wettable surfaces into organic electrochemical transistors, the signal crosstalk problem caused by difficulty in electrolyte patterning is solved, and large-area, high-throughput semiconductor and electrolyte materials are achieved, and the device is improved The stability and integration level solve the problems of low wafer-level micro-nano processing level and low device yield in the prior art.
Patent Information
- Application Number
- CN202411293794.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The difficulty in electrolyte patterning of existing organic electrochemical transistors leads to crosstalk between devices, and relying on complex silicon-based lithography processes to be incompatible with solvents, resulting in low wafer-level micro-nano processing and low device yield.
Using the structure of flexible substrate layer, electrode layer, organic semiconductor layer, hydrophobic sacrificial layer and gel electrolyte layer, a patterned wettable surface is formed through SEBS spin coating and UVO treatment, achieving large area and high level of semiconductor materials and electrolyte materials. Throughput preparation to reduce inter-device variability and signal delay.
By introducing hydrophobic sacrificial layer and UVO processing technology, it is easy to obtain accurate wettable surfaces, and achieve large-scale, uniform electrically stable electrochemical transistor device integration, enhance the cyclic stability and service life of the device and reduce signal loss.
Smart Images

Figure CN119095390A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic electrochemical transistors, and in particular to a wafer-level electrochemical transistor array and a preparation method thereof. Background Art
[0002] As integrated circuits gradually enter the "non-silicon era", the need to develop advanced semiconductor preparation processes suitable for transistors based on new materials is becoming increasingly urgent. So far, various types of carbon-based semiconductor transistors have made significant progress, such as graphene transistors, carbon nanotube field-effect transistors, organic transistors, and molybdenum disulfide field-effect transistors. Among them, organic electrochemical transistors have the advantages of simple preparation process, low operating voltage, high sensitivity, and good compatibility with flexible substrates. They show broad application prospects and huge market space in the field of carbon-based semiconductor transistor electronic devices.
[0003] Currently, flowing liquid electrolytes and soft gel electrolytes limit the electrolyte patterning of OECTs, resulting in shared ions between fabricated transistors, which results in crosstalk between devices and delayed signal transmission. In addition, driven by Moore's Law, more functional chips are expanded and integrated onto a single wafer, while different materials (such as metals, inorganic oxides, organic polymers, and two-dimensional semiconductors), thin film deposition processes (spin coating, evaporation, and sputtering, etc.), and photolithography processes can damage and contaminate each other, making the thin film contact interface chaotic. Therefore, the wafer-level integration of organic electrochemical transistors faces problems such as large differences between devices and low device yield.
[0004] Therefore, it is necessary to develop a wafer-level electrochemical transistor array and a preparation method thereof to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a wafer-level electrochemical transistor array and a method for preparing the same, aiming to solve the problem of crosstalk between device signals caused by the difficulty in patterning the electrolyte in the electrochemical transistor, and at the same time utilize the controllable patterned hydrophilic and hydrophobic areas of the wettability material to achieve large-area, high-throughput preparation of semiconductor materials and electrolyte materials, thereby solving the problems of low wafer-level micro-nano processing of electrochemical transistors and heavy reliance on complicated silicon-based photolithography processes and solvent incompatibility.
[0006] The technical solution adopted by the present invention is as follows: A wafer-level electrochemical transistor array comprises a flexible substrate layer, an electrode layer, an organic semiconductor layer, a hydrophobic sacrificial layer, and a gel electrolyte layer. The electrode layer comprises a source electrode, a drain electrode, and a gate electrode. The source electrode, the drain electrode, and the gate electrode are all arranged above the flexible substrate layer. The hydrophobic sacrificial layer is arranged above the source electrode, the drain electrode, and the gate electrode. The organic semiconductor layer is arranged in a hydrophilic region between the source electrode and the drain electrode. The gel electrolyte covers the hydrophilic region above the organic semiconductor layer and the gate electrode. The hydrophobic sacrificial layer is obtained by high-temperature annealing after SEBS spin coating, and a patterned wettability surface is formed by UVO treatment and mask shielding.
[0007] A method for preparing a wafer-level electrochemical transistor array comprises the following steps: Step 1: Clean the 3-inch wafer, blow dry it with nitrogen or heat dry it in a constant temperature oven for more than 6 hours after cleaning; Step 2: Spin-coat a 2% Micro-90 aqueous solution on a 3-inch wafer as an anti-adhesion layer; Step 3: Deposit a parylene C film using chemical vapor deposition; solid dichloroparaxylene dimer is sublimed at 150 °C and cracked in a pyrolysis furnace at 750 °C under a vacuum of 5 mbar, depositing a parylene C film with a thickness of 1-5 μm at a rate of 5 Å / s; Step 4: At a vacuum degree of 1×10 -4 Under Pa conditions, Cr adhesion layer was evaporated; Step 5: At a vacuum degree of 1×10 -4 Au electrode was evaporated under Pa conditions; Step 6: Spin-coat the prepared SEBS solution onto the wafer deposited with the parylene C film, and dry the spin-coated substrate to obtain a SEBS hydrophobic sacrificial layer; Step 7: Align the mask with the organic semiconductor pattern with the wafer, and use UVO treatment to separate the SEBS between the source and drain electrodes from the substrate and obtain a wettable pattern (hydrophilic silicon wafer after UVO treatment, hydrophobic SEBS shielded by the mask); Step 8: Spin-coating a hydrophilic organic semiconductor material on the SEBS and curing; Step 9: Align the mask with the gel electrolyte pattern with the wafer, and use UVO treatment to separate the SEBS on the gate from the substrate and obtain a wettable pattern; Step 10: dripping gel electrolyte on the semiconductor channel and curing at a constant temperature; Step 11: Water dissolves the Micro-90 and releases the parylene substrate.
[0008] The beneficial effects of the present invention are as follows: 1. By introducing a hydrophobic sacrificial layer SEBS film and UVO or plasma surface treatment technology to enhance the contrast between hydrophobic and hydrophilic areas, a precise patterned wettability surface can be easily obtained.
[0009] 2. By introducing wettability patterns, precise shape and position control of a small amount of solution on a wafer-level substrate can be achieved without the need for surfactants and external equipment, thereby obtaining large-scale, uniform electrochemical transistor devices with stable electrical properties and realizing the integration of organic transistor devices at the wafer level.
[0010] 3. By introducing a hydrophobic SEBS layer, the electrochemical transistor can be encapsulated to reduce the damage of oxygen and water vapor to the device and enhance the cycle stability and service life of the device.
[0011] 4. Use wafer-level ultra-flexible substrates to reduce the contact resistance at the interface between electronic materials and biological tissues, achieve good conformal contact and signal sensing of electrochemical transistors on complex biological surfaces, and reduce signal loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the proportional relationship of the various components in the drawings of this specification does not represent the proportional relationship in actual material selection and design, which is only a schematic diagram of the structure or position, wherein: Figure 1 It is a schematic diagram of the structure of the present invention; Figure 2 is the wettability pattern of SEBS treated with UVO in the present invention; Description of the reference numerals in the accompanying drawings: 1-flexible substrate layer, 2-source electrode, 3-drain electrode, 4-gate electrode, 5-organic semiconductor layer, 6-hydrophobic sacrificial layer, 7-gel electrolyte layer, 8-hydrophilic silicon wafer after UVO treatment. DETAILED DESCRIPTION
[0013] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.
[0014] Combine the following Figure 1 to Figure 2 , the present invention is described in detail.
[0015] like Figure 1As shown, a wafer-level electrochemical transistor array includes a flexible substrate layer 1, an electrode layer, an organic semiconductor layer 5, a hydrophobic sacrificial layer 6, and a gel electrolyte layer 7. The electrode layer includes a source electrode 2, a drain electrode 3, and a gate electrode 4. The source electrode 2, the drain electrode 3, and the gate electrode 4 are all arranged above the flexible substrate layer 1. The hydrophobic sacrificial layer 6 is arranged above the source electrode 2, the drain electrode 3, and the gate electrode 4. The organic semiconductor layer 5 is arranged in a hydrophilic region between the source electrode 2 and the drain electrode 3. The gel electrolyte 7 covers the hydrophilic region above the organic semiconductor layer 5 and the gate electrode 4. The hydrophobic sacrificial layer 6 is obtained by high-temperature annealing after SEBS spin coating, and a patterned wettability surface is formed by ultraviolet ozone UVO treatment and mask shielding.
[0016] The flexible substrate layer (1) is made of at least one of polyparaxylene, styrene-ethylene-butylene-styrene thermoplastic elastomer, polyimide, polydimethylsiloxane or polyurethane.
[0017] The preparation material of the electrode layer is one of thermally evaporated gold, gold nanowires, graphene or carbon nanotubes, and the thickness of the electrode layer ranges from 80 to 150 nm.
[0018] The preparation material of the organic semiconductor layer (5) is one or both of p-type polymer PEDOT:PSS and n-type polymer BBL, and the thickness of the organic semiconductor layer (5) is in the range of 100-200 nm.
[0019] The preparation material of the hydrophobic sacrificial layer (6) is one of SEBS, octadecyltrimethoxysilane or heptadecafluorodecyltrimethoxysilane, and the thickness of the hydrophobic sacrificial layer (6) is in the range of 200-300 nm.
[0020] The preparation material of the gel electrolyte layer (7) is prepared by mixing a hydrophilic polymer with an ionic liquid or a salt, wherein the polymer is one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, chitosan, sodium polystyrene sulfonate or polyacrylonitrile, the ionic liquid is at least one of [EMIM][TFSI], [EMIM][FSI], [EMIM][DCA], [BMIM][PF6] or [EMIM][BF4], and the salt is at least one of Li salt, Na salt, Ca salt or K salt.
[0021] A method for preparing a wafer-level electrochemical transistor array comprises the following steps: Step 1: Clean the 3-inch Si / SiO2 wafer, blow dry it with nitrogen or heat dry it in a constant temperature oven for more than 6 hours after cleaning; Step 2: Spin-coat a 2% Micro-90 aqueous solution on a 3-inch wafer as an anti-adhesion layer; Step 3: Deposit a parylene C film using chemical vapor deposition; solid dichloroparaxylene dimer is sublimed at 150 °C and cracked in a pyrolysis furnace at 750 °C under a vacuum of 5 mbar, depositing a parylene C film with a thickness of 1-5 μm at a rate of 5 Å / s; Step 4: At a vacuum degree of 1×10 -4 Under Pa conditions, Cr adhesion layer was evaporated; Step 5: At a vacuum degree of 1×10 -4 Au electrode was evaporated under Pa conditions; Step 6: Spin-coat the prepared SEBS solution onto the wafer deposited with the parylene C film, and dry the spin-coated substrate to obtain a SEBS hydrophobic sacrificial layer; Step 7: Align the mask with the organic semiconductor pattern with the wafer, and use UVO treatment to separate the SEBS between the source and drain electrodes from the substrate and obtain a wettable pattern (hydrophilic silicon wafer 8 after UVO treatment, hydrophobic SEBS shielded by the mask); Step 8: Spin-coating a hydrophilic organic semiconductor material on the SEBS and curing; Step 9: Align the mask with the gel electrolyte pattern with the wafer, and use UVO treatment to separate the SEBS on the gate from the substrate and obtain a wettable pattern; Step 10: dripping gel electrolyte on the semiconductor channel and curing at a constant temperature; Step 11: Water dissolves the Micro-90 and releases the parylene substrate.
[0022] The drying method adopts at least one of constant temperature hot plate heating, oven heating, far infrared heating and hot air heating.
[0023] Example 1 (control group): 1. Clean the 3-inch Si / SiO2 wafer (SiO2: 100 nm) and place it in a constant temperature oven for more than 6 hours after cleaning; 2. Spin-coat and deposit the fluorinated polymer Novec 1700 (3M) (1000 rpm, 30 s) on a 3-inch wafer as an anti-adhesion layer of parylene; 3. Deposit parylene C thin film using chemical vapor deposition at a vacuum of 5 mbar (rate: 5 Å / s, film thickness: ~2 μm); 4. At a vacuum degree of 1×10 -4 Under Pa conditions, the Cr adhesion layer was evaporated with a thickness of about ~3 nm; 5. At a vacuum degree of 1×10 -4Under Pa conditions, the Au electrode was evaporated with a thickness of about ~50 nm, a channel length of 20 mm, and a channel width of 1.2 cm; 6. Spin-coat the n-type hydrophilic organic semiconductor material BBL on the wafer (5 mg / mL, 3000 rpm, 60 s); 7. Place the wafer with the patterned semiconductor solution on a constant temperature hot stage for drying (100 °C, 10 min), and place the dried film in deionized water for solvent exchange to remove the organic solvent and form a BBL film; 8. Drop a gel electrolyte (chitosan: acetic acid: NaCl: glycerol: deionized water = 1: 0.67: 32: 2: 1) on the semiconductor channel and solidify the gel electrolyte at room temperature; 9. Use tweezers to peel off and release the parylene substrate; 10. Under test conditions: leakage voltage (V D ) = -0.1 V, gate voltage (V G ) scanning range is -0.2~0.6 V, and the device switching ratio (I on / I off ) = 1.4 × 10 3 , transconductance (g m ) = 0.34 ± 0.21 mS, and the device yield is 68% due to the shedding of the BBL film during the solvent exchange process.
[0024] Embodiment 2: 1. Clean the 3-inch Si / SiO2 wafer (SiO2: 100 nm) and place it in a constant temperature oven for more than 6 hours after cleaning; 2. Spin-coat and deposit the fluorinated polymer Novec 1700 (3M) (1000 rpm, 30 s) on a 3-inch wafer as an anti-adhesion layer of parylene; 3. Deposit parylene C thin film using chemical vapor deposition at a vacuum of 5 mbar (rate: 5 Å / s, film thickness: ~2 μm); 4. At a vacuum degree of 1×10 -4 Under Pa conditions, the Cr adhesion layer was evaporated with a thickness of about ~3 nm; 5. At a vacuum degree of 1×10 -4 Under Pa conditions, the Au electrode was evaporated with a thickness of about ~50 nm, a channel length of 20 mm, and a channel width of 1.2 cm; 6. Spin-coat the prepared SEBS solution (6 mg / mL) onto the wafer with the parylene film deposited on it (3000 rpm, 60 s), and place the spin-coated substrate on a constant temperature hot plate for drying (100 °C, 3 min) to obtain a dense SEBS sacrificial layer; 7. Place the mask with the organic semiconductor pattern on top of the wafer, align it with the mark on the wafer, and treat it with UVO (15 min) to separate the SEBS hydrophobic layer between the source and drain electrodes from the substrate and obtain a wettable pattern; 8. Spin-coat the n-type hydrophilic organic semiconductor material BBL (5 mg / mL, 3000 rpm, 60 s) on SEBS. During the spin-coating process, the semiconductor solution is retained in the hydrophilic area, while the excess semiconductor solution is removed along the hydrophobic area; 9. Place the wafer with the patterned semiconductor solution on a constant temperature hot stage for drying (100 °C, 10 min), and place the dried film in deionized water for solvent exchange to remove the organic solvent and form a BBL film; 10. Drop a gel electrolyte (chitosan: acetic acid: NaCl: glycerol: deionized water = 1: 0.67: 32: 2: 1) on the semiconductor channel and solidify the gel electrolyte at room temperature; 1. Use tweezers to peel off and release the parylene substrate; 2. Under test conditions: leakage voltage (V D ) = -0.1 V, gate voltage (V G ) scanning range is -0.2~0.6 V, and the device switching ratio (I on / I off ) = 8.36 × 10 3 , transconductance (g m ) = 0.39 ± 0.18 mS, and the device yield is 81%.
[0025] Embodiment 3: 1. Clean the 3-inch Si / SiO2 wafer (SiO2: 100 nm) and place it in a constant temperature oven for more than 6 hours after cleaning; 2. Spin-coat and deposit the fluorinated polymer Novec 1700 (3M) (1000 rpm, 30 s) on a 3-inch wafer as an anti-adhesion layer of parylene; 3. Deposit parylene C thin film using chemical vapor deposition at a vacuum of 5 mbar (rate: 5 Å / s, film thickness: ~2 μm); 4. At a vacuum degree of 1×10 -4Under Pa conditions, the Cr adhesion layer was evaporated with a thickness of about ~3 nm; 5. At a vacuum degree of 1×10 -4 Under Pa conditions, the Au electrode was evaporated with a thickness of about ~50 nm, a channel length of 20 mm, and a channel width of 1.2 cm; 6. Spin-coat the prepared SEBS solution (6 mg / mL) onto the wafer with the parylene film deposited on it (3000 rpm, 60 s), and place the spin-coated substrate on a constant temperature hot plate for drying (100 °C, 3 min) to obtain a dense SEBS sacrificial layer; 7. Place the mask with the organic semiconductor pattern on top of the wafer, align it with the mark on the wafer, and treat it with UVO (15 min) to separate the SEBS hydrophobic layer between the source and drain electrodes from the substrate and obtain a wettable pattern; 8. Spin-coat the n-type hydrophilic organic semiconductor material BBL (5 mg / mL, 3000 rpm, 60 s) on SEBS. During the spin-coating process, the semiconductor solution is retained in the hydrophilic area, while the excess semiconductor solution is removed along the hydrophobic area; 9. Place the wafer with the patterned semiconductor solution on a constant temperature hot stage for drying (100 °C, 10 min), and place the dried film in deionized water for solvent exchange to remove the organic solvent and form a BBL film; 10. Place the mask with the gel electrolyte pattern on the wafer, align it with the mark on the wafer, and treat it with UVO (15 min) to separate the SEBS on the gate from the substrate and obtain a wettable pattern; 11. Drop a gel electrolyte (chitosan: acetic acid: NaCl: glycerol: deionized water = 1:0.67:32:2:1) on the semiconductor channel, rotate the wafer to remove the electrolyte on the hydrophobic SEBS film, and cure the gel electrolyte at room temperature; 12. Use tweezers to peel off and release the parylene substrate; Under test conditions: Drain voltage (V D ) = -0.1 V, gate voltage (V G ) scanning range is -0.2~0.6 V, and the device switching ratio (I on / I off ) = 2.3 × 10 4 , transconductance (g m ) = 0.43 ± 0.05 mS, and the device yield is 96%.
[0026] It can be seen from Examples 1-3 that: according to a wafer-level electrochemical transistor array, from bottom to top, it includes a flexible substrate layer 1, an electrode layer, an organic semiconductor layer 5 and an ion gel electrolyte layer 7; the electrodes include a source electrode 2, a drain electrode 3 and a gate electrode 4; a hydrophobic sacrificial layer 5 is arranged above the source electrode 2, the drain electrode 3 and the gate electrode 4, and an ion gel electrolyte layer 6 is arranged above the gate electrode 4 and the organic semiconductor 5; the hydrophobic sacrificial layer 5 is removed after UVO treatment to form a patterned wettability surface, and the hydrophilic material will be precisely retained in the hydrophilic area on the hydrophobic sacrificial layer 5, and the excess material will be removed along the SEBS surface.
[0027] Compared with the untreated electrochemical transistor (i.e., the organic electrochemical transistor prepared by the preparation method of the electrochemical transistor with a wettability pattern on the wafer (i.e., the organic electrochemical transistor prepared in Examples 2-3), the organic electrochemical transistor prepared by the preparation method of the electrochemical transistor with a wettability pattern on the wafer can realize the preparation of a fully patterned device, and the size of its switching ratio is improved, and the transconductance difference between devices is improved. This is because after the introduction of the wettability pattern, the semiconductor and electrolyte sizes of each device are guaranteed to be consistent, reducing the crosstalk between devices. At the same time, by introducing the wettability pattern, the surface with a high hydrophilic-hydrophobic contrast is integrated with the liquid semiconductor solution and the quasi-solid gel electrolyte, and the use of very little solution solves the problem that the electrolyte of the electrochemical transistor cannot be expanded and patterned on a large scale.
[0028] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A wafer-level electrochemical transistor array, characterized in that: The invention comprises a flexible substrate layer (1), an electrode layer, an organic semiconductor layer (5), a hydrophobic sacrificial layer (6), and a gel electrolyte layer (7); the electrode layer comprises a source electrode (2), a drain electrode (3), and a gate electrode (4); the source electrode (2), the drain electrode (3), and the gate electrode (4) are all arranged above the flexible substrate layer (1); the SEBS hydrophobic sacrificial layer (6) is arranged above the source electrode (2), the drain electrode (3), and the gate electrode (4); the organic semiconductor layer (5) is arranged in a hydrophilic region between the source electrode (2) and the drain electrode (3); and the gel electrolyte (7) covers the hydrophilic region above the organic semiconductor layer (5) and the gate electrode (4); the hydrophobic sacrificial layer (6) is obtained by spin coating SEBS and then annealing at high temperature, and a patterned wettable surface is formed by UVO treatment and mask shielding.
2. The wafer-level electrochemical transistor array according to claim 1, characterized in that: The flexible substrate layer (1) is made of at least one of polyparaxylene, styrene-ethylene-butylene-styrene thermoplastic elastomer, polyimide, polydimethylsiloxane or polyurethane.
3. The wafer-level electrochemical transistor array according to claim 1, characterized in that: The preparation material of the electrode layer is one of thermally evaporated gold, gold nanowires, graphene or carbon nanotubes, and the thickness of the electrode layer ranges from 80 to 150 nm.
4. The wafer-level electrochemical transistor array according to claim 1, characterized in that: The preparation material of the organic semiconductor layer (5) is one or both of p-type polymer PEDOT:PSS and n-type polymer BBL, and the thickness of the organic semiconductor layer (5) is in the range of 100-200 nm.
5. The wafer-level electrochemical transistor array according to claim 1, characterized in that: The preparation material of the hydrophobic sacrificial layer (6) is one of SEBS, octadecyltrimethoxysilane or heptadecafluorodecyltrimethoxysilane, and the thickness of the hydrophobic sacrificial layer (6) is in the range of 200-300 nm.
6. The wafer-level electrochemical transistor array according to claim 1, characterized in that: The preparation material of the gel electrolyte layer (7) is prepared by mixing a hydrophilic polymer with an ionic liquid or a salt, wherein the polymer is one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, chitosan, sodium polystyrene sulfonate or polyacrylonitrile, the ionic liquid is at least one of [EMIM][TFSI], [EMIM][FSI], [EMIM][DCA], [BMIM][PF6] or [EMIM][BF4], and the salt is at least one of Li salt, Na salt, Ca salt or K salt.
7. A method for preparing a wafer-level electrochemical transistor array according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Clean the 3-inch wafer, blow dry it with nitrogen or heat dry it in a constant temperature oven for more than 6 hours after cleaning; Step 2: Spin-coat a 2% Micro-90 aqueous solution on a 3-inch wafer as an anti-adhesion layer; Step 3: Deposit a parylene C film using chemical vapor deposition; solid dichloroparaxylene dimer is sublimed at 150 °C and cracked in a pyrolysis furnace at 750 °C under a vacuum of 5 mbar, depositing a parylene C film with a thickness of 1-5 μm at a rate of 5 Å / s; Step 4: At a vacuum degree of 1×10 -4 Under Pa conditions, Cr adhesion layer was evaporated; Step 5: At a vacuum degree of 1×10 -4 Au electrode was evaporated under Pa conditions; Step 6: Spin-coat the prepared SEBS solution onto the wafer deposited with the parylene C film, and dry the spin-coated substrate to obtain a SEBS hydrophobic sacrificial layer; Step 7: Align the mask with the organic semiconductor pattern with the wafer, and use UVO treatment to separate the SEBS between the source and drain electrodes from the substrate and obtain a wettable pattern; Step 8: Spin-coating a hydrophilic organic semiconductor material on the SEBS and curing; Step 9: Align the mask with the gel electrolyte pattern with the wafer, and use UVO treatment to separate the SEBS on the gate from the substrate and obtain a wettable pattern; Step 10: dripping gel electrolyte on the semiconductor channel and curing at a constant temperature; Step 11: Water dissolves the Micro-90 and releases the parylene C substrate.
8. The method for preparing a wafer-level electrochemical transistor array according to claim 7, characterized in that: The drying method adopts at least one of constant temperature hot plate heating, oven heating, far infrared heating and hot air heating.
Citation Information
Cited By
Hydrophilic and hydrophobic patterning-based oxide thin film transistor array preparation and physiological electric signal monitoring method