Perovskite solar cell module and preparation method thereof
The lower interface seed assisted growth layer was prepared by vacuum evaporation method and a high-quality perovskite film was formed, which solved the photoelectric performance and stability of α-FAPbI3 perovskite solar cells, and achieved high efficiency and high stability pertitanium Preparation of mineral solar cell modules.
Patent Information
- Application Number
- CN202411201275.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the photoelectric performance and stability of α-FAPbI3 perovskite solar cells are poor, and high-quality perovskite films cannot be prepared on a large scale.
The lower interface seed-assisted growth layer was prepared by vacuum evaporation method, which induces perovskite growth as a nucleation site, forming a large area high-quality perovskite film with large grains, no pinholes and few defects, and was then etched through laser etching. The partition lines are formed to improve the stability of the battery structure.
Improve the photoelectric performance and stability of perovskite solar cells, enhance the conductivity and charge extraction efficiency of the hole transport layer, reduce the interfacial charge recombination, improve the photoelectric conversion efficiency and stability, and the process is simple, stable and capable. repeat.
Smart Images

Figure CN119095454A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a perovskite solar cell module and a preparation method thereof. Background Art
[0002] Perovskite solar cells (PSCs) have become a research hotspot in the photovoltaic field due to their high efficiency, low cost, tunable photoelectric properties, and solution processability. According to the latest research progress, the photoelectric conversion efficiency of PSCs has reached 26.1%, close to the record efficiency of crystalline silicon (c-Si) cells (26.81%). This huge progress is attributed to their extraordinary perovskite properties, such as high cost-effectiveness, strong defect tolerance, long free carrier diffusion length, strong light absorption, efficient charge transfer, clear light absorption edge, and adjustable band gap, which have promoted their industrial application in the photovoltaic market. Perovskite solar cells can be roughly divided into two categories in terms of structure: upright (nip) structure and inverted (pin) structure. The upright structure was developed earlier than the inverted structure and has a slightly better efficiency than the inverted structure. However, the inverted structure has better stability and a simpler preparation process. It can be integrated into a tandem solar cell and is suitable for the preparation of large-area perovskite solar cells. Figure 1 As shown, generally, the inverted battery structure includes a conductive glass substrate 1, a transparent conductive film 2, a hole transport layer 3, a perovskite film 4, an electron transport layer 5 and a metal electrode 6.
[0003] As a perovskite material, the FA cation size in the perovskite lattice of FAPbI3 is relatively large, which easily leads to undesirable phase transitions, seriously affecting the photoelectric performance and stability of α-FAPbI3 perovskite films. So far, people have developed a variety of strategies to improve the performance of perovskite solar cells (PSCs) based on α-FAPbI3. Among them, the method of effectively obtaining high-quality α-FAPbI3 perovskite films through seed-assisted growth layers has attracted widespread attention. However, these methods are all carried out by spin coating, which limits their application outside the laboratory scale. Therefore, it is necessary to provide an improved technical solution for the above-mentioned deficiencies in the prior art. Summary of the invention
[0004] In view of the shortcomings of the prior art described above, the present invention aims to provide a perovskite solar cell module and a method for preparing the same, so as to solve the problems of poor photoelectric performance and stability of α-FAPbI3 perovskite films in the prior art, and the problem of being unable to prepare high-quality perovskite films on a large scale.
[0005] To achieve the above-mentioned object and other related objects, the present invention provides a method for preparing a perovskite solar cell module, the preparation method comprising the following steps:
[0006] S1. providing a substrate, wherein the substrate is covered with a transparent conductive film;
[0007] S2, performing a first laser etching on the transparent conductive film to form a first separation line on the transparent conductive film;
[0008] S3, forming a hole transport layer on the transparent conductive film;
[0009] S4, forming a lower interface seed auxiliary growth layer on the hole transport layer;
[0010] S5, forming a perovskite thin film layer on the lower interface seed auxiliary growth layer;
[0011] S6, forming an electron transport layer on the upper surface of the perovskite thin film layer;
[0012] S7, performing a second laser etching to form a second separation line on the hole transport layer, the lower interface seed auxiliary growth layer, the perovskite thin film layer and the electron transport layer;
[0013] S8, forming a metal electrode layer on the electron transport layer;
[0014] S9, performing a third laser etching to form a third separation line on the hole transport layer, the lower interface seed auxiliary growth layer, the perovskite film layer, the electron transport layer and the metal electrode layer.
[0015] Preferably, in step S1, the substrate is a rigid conductive substrate or a flexible conductive substrate.
[0016] Preferably, in step S1, the transparent conductive film is one or a combination of FTO, AZO, ITO and IWO.
[0017] Preferably, in step S3, the hole transport layer is prepared by a method selected from the group consisting of a spraying method, a coating method, a scraping method, a sputtering magnetron sputtering method, and a thermal evaporation method.
[0018] Preferably, in step S3, the hole transport layer is one or a combination of Sprio-OMe TAD, PTAA, PEDOT:PSS, nickel oxide, copper oxide, vanadium oxide, tungsten oxide, and cuprous thiocyanate.
[0019] Preferably, the lower interface seed auxiliary growth layer in step S4 is prepared by vacuum evaporation method, specifically:
[0020] The seed layer solid powder is used as an evaporation source, and evaporation is performed under vacuum conditions until a lower interface seed auxiliary growth layer with a thickness of 5 to 10 nm is formed on the surface of the hole transport layer; wherein the seed layer solid powder is CsPbBr3 or CsPbI3, and the vacuum degree is 10-5 Pa~10 -3 Pa.
[0021] Preferably, the method for preparing the perovskite thin film layer in step S5 is specifically as follows: first depositing a PbI2 thin film, then coating the PbI2 thin film with an organic ammonium halide solution by blade coating or slit coating, and then annealing and crystallizing to form a perovskite thin film layer.
[0022] Preferably, the solute of the organic ammonium halide solution is one or a combination of formamidine hydroiodide, methylamine hydroiodide, formamidine hydrochloride, methylamine hydrochloride, formamidine hydrobromide, and methylamine hydrobromide, and the solvent of the organic ammonium halide solution is one or a combination of isopropanol and ethanol.
[0023] Preferably, the thickness of the deposited PbI2 film is 200-400 nm.
[0024] Preferably, the annealing temperature is 130-180° C., and the annealing time is 10-40 min.
[0025] Preferably, the preparation method of the electron transport layer in step S6 includes one of spraying, coating, blade coating, sputtering, and thermal evaporation, and the electron transport layer is one or a combination of PCBM, C60, BCP, SnO2, titanium oxide, and zinc oxide.
[0026] Preferably, the metal electrode layer in step S8 is prepared by any one of thermal evaporation, sputtering and scraping, and the metal electrode layer material includes one of gold, silver, aluminum, copper, nickel, carbon and ITO.
[0027] The present invention also provides a perovskite solar cell module prepared by the above-mentioned preparation method, wherein the perovskite solar cell module comprises a substrate, a transparent conductive film, a hole transport layer, a lower interface seed auxiliary growth layer, a perovskite film layer, an electron transport layer, and a metal electrode layer which are stacked in sequence.
[0028] As described above, the perovskite solar cell module and the preparation method thereof of the present invention have the following beneficial effects:
[0029] The present invention provides a high-efficiency and high-stability large-area perovskite solar cell module and a preparation method thereof. A lower interface seed auxiliary growth layer is prepared by a vacuum evaporation method, and the lower interface seed auxiliary growth layer is used as a nucleation site to induce the growth of perovskite, thereby preparing a large-area high-quality perovskite film layer with large grains, no pinholes and few defects, thereby improving the photoelectric performance and stability of alpha-FAPbI3 perovskite, improving the conductivity and charge extraction efficiency of the hole transport layer, reducing interface charge recombination, and further improving the photoelectric conversion efficiency and stability of large-area perovskite solar cells. The preparation steps are simple, the process is stable, and the repeatability is strong. The module can be widely used in the industrial preparation process of perovskite films. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Shown is a process flow chart of preparing a perovskite solar cell module in a specific embodiment of the present invention.
[0031] Figure 2 It shows a schematic diagram of the structure of the perovskite solar cell module in specific embodiments 1 and 2 of the present invention.
[0032] Figure 3 It shows a schematic structural diagram of a perovskite solar cell module in specific embodiment 3 of the present invention.
[0033] Figure 4 Shown is a schematic structural diagram of a perovskite solar cell module in specific embodiment 4 of the present invention.
[0034] Component number description
[0035] 10 Substrate
[0036] 20 Transparent Conductive Film
[0037] 30 Hole transport layer
[0038] 40 Lower interface seed auxiliary growth layer
[0039] 50 Perovskite thin film layer
[0040] 60 Electron transport layer
[0041] 70 Metal electrode layer
[0042] 80 Indium oxide based transparent conductive oxide layer
[0043] P1 First dividing line
[0044] P2 Second dividing line
[0045] P3 Third dividing line DETAILED DESCRIPTION
[0046] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0047] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.
[0048] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0049] See also Figure 1 The present invention provides a method for preparing a perovskite solar cell module, the preparation method comprising the following steps:
[0050] S1, providing a substrate 10, wherein the substrate 10 is covered with a transparent conductive film 20;
[0051] S2, performing a first laser etching on the transparent conductive film 20 to form a first separation line on the transparent conductive film 20;
[0052] S3, forming a hole transport layer 30 on the transparent conductive film 20;
[0053] S4, forming a lower interface seed auxiliary growth layer 40 on the hole transport layer 30;
[0054] S5, forming a perovskite thin film layer 50 on the lower interface seed auxiliary growth layer 40;
[0055] S6, forming an electron transport layer 60 on the upper surface of the perovskite thin film layer 50;
[0056] S7, performing a second laser etching to form a second separation line on the hole transport layer 30, the lower interface seed auxiliary growth layer 40, the perovskite thin film layer 50 and the electron transport layer 60;
[0057] S8, forming a metal electrode layer 70 on the electron transport layer 60;
[0058] S9 , performing a third laser etching to form a third separation line on the hole transport layer 30 , the lower interface seed auxiliary growth layer 40 , the perovskite film layer 50 , the electron transport layer 60 and the metal electrode layer 70 .
[0059] Specifically, the present invention provides a method for preparing a large-area perovskite solar cell module with high efficiency and high stability, using the following interface seed auxiliary growth layer 40 as a nucleation site to induce perovskite growth, thereby preparing a large-area, high-quality perovskite film layer 50 with large grains, no pinholes, and few defects, thereby improving the photoelectric performance and stability of the α-FAPbI3 perovskite, and improving the conductivity and charge extraction efficiency of the hole transport layer 30, reducing interface charge recombination, and further improving the photoelectric conversion efficiency and stability of large-area perovskite solar cells.
[0060] As an example, in step S1 , the substrate 10 is a rigid conductive substrate 10 or a flexible conductive substrate 10 .
[0061] Preferably, the rigid conductive substrate 10 is flat glass, and the flexible conductive substrate is polyethylene naphthalate.
[0062] As an example, in step S1 , the transparent conductive film 20 is one or a combination of FTO (tin oxide doped with F element), AZO (zinc oxide doped with aluminum element), ITO (indium oxide doped with tin element), and IWO (indium oxide doped with tungsten element).
[0063] Specifically, FTO is fluorine-doped tin oxide, which is an n-type semiconductor material; AZO is aluminum-doped zinc oxide, which is also an n-type semiconductor material; ITO is indium tin oxide, which is an n-type semiconductor with extremely high transparency and conductivity; IWO is tungsten-doped indium oxide, which is also an n-type semiconductor material.
[0064] As an example, the preparation method of the hole transport layer 30 in step S3 is one of a spraying method, a coating method, a doctor blade method, a sputtering magnetron sputtering method, and a thermal evaporation method.
[0065] As an example, in step S3 , the hole transport layer 30 is one or a combination of Spiro-OMe TAD, PTAA, PEDOT:PSS, nickel oxide, copper oxide, vanadium oxide, tungsten oxide, and cuprous thiocyanate.
[0066] Specifically, Sprio-OMe TAD is an organic small molecule material with high hole mobility and good solubility, which is convenient for solution processing; PTAA is a polymer material with good hole transport performance and stability. PTAA has a high glass transition temperature (Tg), which helps to improve the thermal stability of the device, and due to its polymer properties, PTAA can form a uniform and dense film, which helps to improve the performance and stability of the battery; PEDOT:PSS is a conductive polymer with excellent conductivity and processing properties.
[0067] As an example, in step S4, the lower interface seed auxiliary growth layer 40 is prepared by vacuum evaporation method, specifically:
[0068] The seed layer solid powder is used as an evaporation source, and evaporation is performed under vacuum conditions until a lower interface seed auxiliary growth layer 40 with a thickness of 5 to 10 nm is formed on the surface of the hole transport layer 30, wherein the seed layer solid powder is CsPbBr3 or CsPbI3, and the vacuum degree is 10 -5 Pa~10 -3 Pa.
[0069] Specifically, the vacuum condition is a vacuum degree of 10 -5 Pa~10 -3 Pa, the thickness of the lower interface seed auxiliary growth layer 40 formed may include any value within a range of 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, etc.; preferably, the evaporation speed is ( wait).
[0070] As an example, the preparation method of the perovskite film layer 50 in step S5 is specifically as follows: first deposit a PbI2 film, then coat the PbI2 film with an organic ammonium halide solution by a doctor blade or slit coating method, and then anneal and crystallize to form the perovskite film layer 50.
[0071] As an example, the solute of the organic ammonium halide solution is one or a combination of formamidine hydroiodide, methylamine hydroiodide, formamidine hydrochloride, methylamine hydrochloride, formamidine hydrobromide, and methylamine hydrobromide, and the solvent of the organic ammonium halide solution is one or a combination of isopropanol and ethanol.
[0072] As an example, the thickness of the deposited PbI2 film is 200 to 400 nm (eg, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, etc.).
[0073] As an example, the annealing temperature is 130-180°C (eg, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc.), and the annealing time is 10-40 min (eg, 10 min, 20 min, 30 min, 40 min, etc.).
[0074] Specifically, the preparation method of the perovskite film layer 50 in step S5 is to form the perovskite film layer 50 by a solid-liquid mixing two-step method. The first step is to deposit PbI2 on the lower interface seed auxiliary growth layer 40 by a thermal evaporation method. The specific method is: the vacuum degree reaches 10 -3 Pa, turn on the power supply and adjust the current to control the evaporation speed of PbI2. (For example, 0.5 During the evaporation process, the thickness of the deposited film is detected by a quartz crystal film thickness monitor until the thickness of the deposited PbI2 film reaches 200-400nm (200nm, 250nm, 300nm, 350nm, 400nm, etc.), the DC power supply is turned off, the deposition of the PbI2 film is completed, and the hatch can be opened after the pressure of the evaporation chamber is released; the second step is to coat the organic ammonium halide solution on the PbI2 film by scraping or slit coating, and anneal and crystallize to form a perovskite film layer 50, specifically: in an atmospheric environment, the ambient humidity is 1 0% to 80% (such as 10%, 30%, 50%, 70%, 80%, etc.), coating the organic ammonium halide solution on the PbI2 film at a coating speed of 5 to 20 mm / s (such as 5 mm / s, 10 mm / s, 15 mm / s, 20 mm / s, etc.), and then annealing at 130 to 180° C. (such as 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., etc.) for 10 to 40 min (such as 10 min, 20 min, 30 min, 40 min, etc.) to react and form a perovskite film layer 50.
[0075] As an example, the preparation method of the electron transport layer 60 in step S6 includes one of spraying, coating, scraping, sputtering, and thermal evaporation, and the electron transport layer 60 is one or a combination of PCBM ([6,6]-phenyl-C61-butyric acid methyl ester), C60, BCP (2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline), SnO2, titanium oxide, and zinc oxide.
[0076] As an example, in step S8, the metal electrode layer 70 is prepared by any method of thermal evaporation, sputtering, and scraping, and the material of the metal electrode layer 70 includes one of gold, silver, aluminum, copper, nickel, carbon, and ITO.
[0077] Specifically, the metal electrode layer 70 mainly serves as a current collector, transmitting the generated current from the active layer to the external circuit. The metal electrode layer 70 may be distributed in a comb shape, and may transmit light that is not completely absorbed. The metal electrode layer 70 is deposited on the electron transport layer 60 by thermal evaporation, that is, the etched substrate is placed on a turntable in the vacuum chamber of the evaporation equipment, the metal is placed in a tungsten boat, and the metal electrode layer 70 is obtained by thermal evaporation at a certain rate. The growth rate of the metal electrode layer 70 is usually about 1000 Å. between.
[0078] In addition, in a specific embodiment of the present invention, the preparation method of the inverted perovskite solar cell module also includes the step of growing an indium oxide-based transparent conductive oxide layer 80 on the electron transport layer 30 by magnetron sputtering or reactive sputtering, and the thickness of the grown indium oxide-based transparent conductive oxide layer 80 is 10 to 200 nm; and this step is performed before or after the second laser etching.
[0079] Compared with the metal electrode layer 70 , the indium oxide transparent conductive oxide layer 80 is transparent, and the battery module can be made to have a certain light transmittance, and can also be used together with the metal electrode layer 70 as a conductive metal electrode layer.
[0080] The present invention also provides a perovskite solar cell module, which includes a substrate 10, a transparent conductive film 20, a hole transport layer 30, a lower interface seed auxiliary growth layer 40, a perovskite film layer 50, an electron transport layer 60, and a metal electrode layer 70 which are stacked in sequence.
[0081] In order to better understand the perovskite solar cell module and the preparation method thereof in the present invention, the perovskite solar cell module and the preparation method thereof in the present invention are described below with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.
[0082] Example 1
[0083] This embodiment provides an inverted perovskite solar cell module and a method for preparing the same. The structural schematic diagram of the perovskite solar cell module is shown in FIG. Figure 2 As shown, the preparation method comprises the following steps:
[0084] S1. Provide a substrate 10 (flat glass), on which a transparent conductive film 20 (FTO) is covered: wash the substrate 10 with the FTO transparent conductive film 20 with detergent, deionized water, acetone and ethanol in sequence, then dry the substrate 10 in an oven, and immediately send it to a laser etching device for subsequent processing;
[0085] S2, performing a first laser etching on the transparent conductive film 20 to form a first separation line P1 on the transparent conductive film 20;
[0086] S3, forming a hole transport layer 30 on the transparent conductive film 20:
[0087] The transparent conductive film 20 is irradiated with ultraviolet ozone for 10 minutes. After the ultraviolet light treatment, NiO is sputtered on the transparent conductive film 20 in a magnetron sputtering coating machine by a magnetron sputtering method. x After sputtering, the film is annealed. The NiO x The layer serves as a hole transport layer 30;
[0088] S4, forming a lower interface seed auxiliary growth layer 40 on the hole transport layer 30:
[0089] The lower interface seed auxiliary growth layer 40 is prepared by vacuum evaporation method. Specifically, the seed layer solid powder (CsPbBr3) is placed in a crucible as an evaporation source, the evaporation source is placed in the cavity of the evaporation machine, the substrate formed in step S3 is placed on the turntable of the vacuum chamber of the evaporation equipment, the door is closed, the vacuum is evacuated, and the ionization gauge reading is observed until the vacuum degree reaches 10 - 3 Pa turns on the power supply and controls the evaporation speed by adjusting the current to maintain the evaporation speed at During the evaporation process, the thickness of the deposited film is detected by a quartz crystal film thickness monitor until the thickness of the lower interface seed auxiliary growth layer 40 (CsPbBr3) deposited on the surface of the hole transport layer 30 reaches 5nm, and then the DC power supply is turned off, and the deposition of the lower interface seed auxiliary growth layer 40 (CsPbBr3) is completed;
[0090] S5, forming a perovskite thin film layer 50 on the lower interface seed auxiliary growth layer 40;
[0091] S51, depositing PbI2 thin film: using thermal evaporation method to deposit PbI2 on the lower interface seed auxiliary growth layer 40, that is, the vacuum degree reaches 10 -3 Pa, turn on the power supply, and adjust the current to control the evaporation speed of PbI2. During the evaporation process, the deposited film thickness is detected by a quartz crystal film thickness monitor until the thickness of PbI2 deposited on the surface of the hole transport layer 30 reaches 200nm, the DC power supply is turned off, and the PbI2 film deposition is completed;
[0092] S52, in an atmospheric environment, at an ambient temperature of 30%, coating an isopropanol solution containing formamidine hydroiodide on the PbI2 film by a doctor blade coating method, with a gap between the doctor blade and the substrate of 200 μm and a coating speed of 15 mm / s, and then annealing at 170° C. for 30 min to form a perovskite film layer 50;
[0093] S6, forming an electron transport layer 60 on the upper surface of the perovskite film layer 50, wherein the electron transport layer 60 includes a C60 film and a BCP film; the specific steps are as follows:
[0094] S61, depositing C60 on the perovskite thin film layer 50 by thermal evaporation, that is, placing the substrate obtained in step S5 on a turntable in a vacuum chamber of an evaporation device, with a background vacuum better than 1×10 -3 Pa, C60 The C60 film with a thickness of 20 nm was obtained by evaporation at a rate of 1.5 %.
[0095] S62, depositing a BCP film on the C60 film by thermal evaporation, that is, placing the substrate obtained in step S61 on a turntable in a vacuum chamber of an evaporation device, placing the BCP in a crucible, The BCP film with a thickness of 8 nm was obtained by evaporation at a rate of ;
[0096] S7, performing a second laser etching to form a second separation line P2 on the hole transport layer 30, the lower interface seed auxiliary growth layer 40, the perovskite thin film layer 50 and the electron transport layer 60;
[0097] S8. Forming a metal electrode layer 70 (copper electrode thin film layer) on the electron transport layer 60:
[0098] A copper conductive film is deposited on the electron transport layer 60 by a thermal evaporation method, that is, the substrate after etching in step S7 is placed on a turntable in a vacuum chamber of an evaporation device, copper particles are placed in a tungsten boat, and evaporated at a certain rate to obtain a metal electrode layer 70 (copper electrode film layer);
[0099] S9 , performing a third laser etching to form a third separation line P3 on the hole transport layer 30 , the lower interface seed auxiliary growth layer 40 , the perovskite film layer 50 , the electron transport layer 60 and the metal electrode layer 70 .
[0100] Example 2
[0101] This embodiment provides an inverted perovskite solar cell module based on a flexible substrate and a preparation method thereof. The structural schematic diagram of the perovskite solar cell module is shown in Figure 2 As shown, the preparation method comprises the following steps:
[0102] S1. Provide a rigid substrate 10 (flat glass), on which a transparent conductive film 20 (ITO) is covered: clean the flexible substrate 10 with the transparent conductive film 20 with detergent, deionized water, acetone and ethanol in sequence, and then dry it in an oven and immediately perform subsequent laser processing;
[0103] S2, performing a first laser etching on the transparent conductive film 20 on the flexible substrate 10 to form a first separation line P1 on the transparent conductive film 20;
[0104] S3, forming a hole transport layer 30 on the transparent conductive film 20:
[0105] The transparent conductive film 20 is irradiated with ultraviolet ozone for 10 minutes. After the ultraviolet treatment, NiO is sputtered on the transparent conductive film 20 by magnetron sputtering. x A thin film, serving as a hole transport layer 30;
[0106] S4, forming a lower interface seed auxiliary growth layer 40 on the hole transport layer 30:
[0107] The lower interface seed auxiliary growth layer 40 is prepared by vacuum evaporation. Specifically, the seed layer solid powder (CsPbBr3) is placed in a crucible as an evaporation source, the evaporation source is placed in the cavity of the evaporation machine, the substrate formed in step S3 is placed on the turntable of the vacuum chamber of the evaporation equipment, the door is closed, the vacuum is pumped, and the ionization gauge reading is observed until the vacuum degree reaches 10 - 3 Pa turns on the power supply and controls the evaporation speed by adjusting the current to maintain the evaporation speed at During the evaporation process, the deposited film thickness is detected by a quartz crystal film thickness monitor until the thickness of the lower interface seed auxiliary growth layer 40 (CsPbBr3) deposited on the surface of the hole transport layer 30 reaches 5nm;
[0108] S5, forming a perovskite thin film layer 50 on the lower interface seed auxiliary growth layer 40;
[0109] S51, depositing PbI2 thin film: using thermal evaporation method to deposit PbI2 on the lower interface seed auxiliary growth layer 40, that is, the vacuum degree reaches 10 -3 Pa, turn on the power supply, and adjust the current to control the evaporation speed of PbI2. During the evaporation process, the deposited film thickness is detected by a quartz crystal film thickness monitor until the thickness of PbI2 deposited on the surface of the hole transport layer 30 reaches 250nm, the DC power supply is turned off, and the PbI2 film deposition is completed;
[0110] S52. Under the condition of atmospheric environment and ambient temperature of 30%, an isopropanol solution containing formamidine hydrobromide and methylamine hydrobromide is coated on the PbI2 film by slit coating. The coating speed is 15 mm / s, and the distance between the coating blade and the substrate is 200 μm. After coating, the sample is placed in a vacuum chamber. The solvent is evaporated quickly by vacuuming to promote high-quality crystallization of perovskite. The time from vacuuming the atmosphere to 10 Pa is less than 15 seconds. Then the sample is annealed at 100°C for 20 minutes to form a perovskite film layer 50;
[0111] S6, forming an electron transport layer 60 on the upper surface of the perovskite thin film layer 50, the electron transport layer 60 comprising a C60 thin film and SnO x Film; the specific steps are as follows:
[0112] S61, depositing C60 on the perovskite thin film layer 50 by thermal evaporation, that is, placing the substrate obtained in step S5 on a turntable in a vacuum chamber of an evaporation device, with a background vacuum better than 1×10 -3 Pa, C60 The C60 film with a thickness of 20 nm was obtained by evaporation at a rate of 1.5 %.
[0113] S62, Preparation of SnO on C60 film by atomic layer deposition x The process conditions are as follows: vacuum degree 10Pa, firstly TDMASn (tetra(dimethylamine)tin) is introduced with a pulse time of 0.6s, then nitrogen is purged for 30s, then H2O is introduced with a pulse time of 0.6s, after the H2O pulse, nitrogen is purged again for 30s, and the above steps are repeated 60 times, and the substrate temperature is maintained at about 90℃ during the whole process, and a SnO film with a thickness of about 10nm is obtained. x film;
[0114] S7, performing a second laser etching to form a second separation line P2 on the hole transport layer 30, the lower interface seed auxiliary growth layer 40, the perovskite thin film layer 50 and the electron transport layer 60;
[0115] S8. Forming a metal electrode layer 70 (copper electrode thin film layer) on the electron transport layer 60:
[0116] A copper conductive film is deposited on the electron transport layer 60 by a thermal evaporation method, that is, the substrate after etching in step S7 is placed on a turntable in a vacuum chamber of an evaporation device, copper particles are placed in a tungsten boat, and evaporated at a certain rate to obtain a metal electrode layer 70 (copper electrode film layer);
[0117] S9 , performing a third laser etching to form a third separation line P3 on the hole transport layer 30 , the lower interface seed auxiliary growth layer 40 , the perovskite film layer 50 , the electron transport layer 60 and the metal electrode layer 70 .
[0118] Example 3
[0119] This embodiment provides an inverted perovskite solar cell module and a method for preparing the same. The structural schematic diagram of the perovskite solar cell module is shown in FIG. Figure 3 As shown, the preparation method comprises the following steps:
[0120] S1. Provide a substrate 10 (flat glass), on which a transparent conductive film 20 (FTO) is covered: wash the substrate 10 with the FTO transparent conductive film 20 with detergent, deionized water, acetone and ethanol in sequence, then dry the substrate 10 in an oven, and immediately send it to a laser etching device for subsequent processing;
[0121] S2, performing a first laser etching on the transparent conductive film 20 to form a first separation line P1 on the transparent conductive film 20;
[0122] S3, forming a hole transport layer 30 on the transparent conductive film 20:
[0123] The transparent conductive film 20 is irradiated with ultraviolet ozone for 10 minutes. After the ultraviolet light treatment, NiO is sputtered on the transparent conductive film 20 in a magnetron sputtering coating machine by a magnetron sputtering method. x After sputtering, the film is annealed. The NiO x The layer serves as a hole transport layer 30;
[0124] S4, forming a lower interface seed auxiliary growth layer 40 on the hole transport layer 30:
[0125] The lower interface seed auxiliary growth layer 40 is prepared by vacuum evaporation method. Specifically, the seed layer solid powder (CsPbBr3) is placed in a crucible as an evaporation source, the evaporation source is placed in the cavity of the evaporation machine, the substrate formed in step S3 is placed on the turntable of the vacuum chamber of the evaporation equipment, the door is closed, the vacuum is evacuated, and the ionization gauge reading is observed until the vacuum degree reaches 10 - 3 Pa turns on the power supply and controls the evaporation speed by adjusting the current to maintain the evaporation speed at During the evaporation process, the thickness of the deposited film is detected by a quartz crystal film thickness monitor until the thickness of the lower interface seed auxiliary growth layer 40 (CsPbBr3) deposited on the surface of the hole transport layer 30 reaches 5nm, and then the DC power supply is turned off, and the deposition of the lower interface seed auxiliary growth layer 40 (CsPbBr3) is completed;
[0126] S5, forming a perovskite thin film layer 50 on the lower interface seed auxiliary growth layer 40;
[0127] S51, depositing PbI2 thin film: using thermal evaporation method to deposit PbI2 on the lower interface seed auxiliary growth layer 40, that is, the vacuum degree reaches 10 -3 Pa, turn on the power supply, and adjust the current to control the evaporation speed of PbI2. During the evaporation process, the deposited film thickness is detected by a quartz crystal film thickness monitor until the thickness of PbI2 deposited on the surface of the hole transport layer 30 reaches 200nm, the DC power supply is turned off, and the PbI2 film deposition is completed;
[0128] S52, in an atmospheric environment, at an ambient temperature and humidity of 25°C and 30% respectively, coating an isopropanol solution containing formamidine hydroiodide on the PbI2 film by a doctor blade coating method, with a gap between the doctor blade and the substrate of 200 μm and a coating speed of 15 mm / s, and then annealing at 170°C for 30 min to react and form a perovskite film layer 50;
[0129] In step S6, an electron transport layer 60 is formed on the upper surface of the perovskite film layer 50. The electron transport layer 60 includes a C60 film and a SnO x Film; the specific steps are as follows:
[0130] S61, depositing C60 on the perovskite thin film layer 50 by thermal evaporation, that is, placing the substrate obtained in step S5 on a turntable in a vacuum chamber of an evaporation device, with a background vacuum better than 1×10 -3 Pa, C60 The C60 film with a thickness of 20 nm was obtained by evaporation at a rate of 1.5 %.
[0131] S62, Preparation of SnO on C60 film by atomic layer deposition x The process conditions are as follows: vacuum degree 10Pa, firstly TDMASn (tetra(dimethylamine)tin) is introduced with a pulse time of 0.6s, then nitrogen is purged for 30s, then H2O is introduced with a pulse time of 0.6s, after the H2O pulse, nitrogen is purged again for 30s, and the above steps are repeated 60 times, and the substrate temperature is maintained at about 90℃ during the whole process, and a SnO film with a thickness of about 10nm is obtained. x film;
[0132] S7, in SnO x An indium oxide-based transparent conductive oxide layer 80 is grown on the film by magnetron sputtering or RPD (reactive sputtering);
[0133] S8, performing a second laser etching to form a second separation line P2 on the hole transport layer 30, the lower interface seed auxiliary growth layer 40, the perovskite film layer 50, the electron transport layer 60 and the indium oxide-based transparent conductive oxide layer 80;
[0134] S9, forming a metal electrode layer 70 (copper electrode thin film layer) on the indium oxide-based transparent conductive oxide layer 80:
[0135] A copper conductive film is deposited on the electron transport layer 60 by a thermal evaporation method, that is, the substrate after etching in step S8 is placed on a turntable in a vacuum chamber of an evaporation device, copper particles are placed in a tungsten boat, and a metal electrode layer 70 (copper electrode film layer) is obtained by thermal evaporation at a certain rate;
[0136] S10 , performing a third laser etching to form a third separation line P3 on the hole transport layer 30 , the lower interface seed auxiliary growth layer 40 , the perovskite film layer 50 , the electron transport layer 60 , the indium oxide-based transparent conductive oxide layer 80 and the metal electrode layer 70 .
[0137] Example 4
[0138] This embodiment provides a method for preparing an inverted perovskite solar cell module. The structural schematic diagram of the perovskite solar cell module is shown in Figure 4 As shown, the preparation method comprises the following steps:
[0139] S1. Provide a substrate 10 (flat glass), on which a transparent conductive film 20 (FTO) is covered: wash the substrate 10 with the FTO transparent conductive film 20 with detergent, deionized water, acetone and ethanol in sequence, then dry the substrate 10 in an oven, and immediately send it to a laser etching device for subsequent processing;
[0140] S2, performing a first laser etching on the transparent conductive film 20 to form a first separation line P1 on the transparent conductive film 20;
[0141] S3, forming a hole transport layer 30 on the transparent conductive film 20:
[0142] The transparent conductive film 20 is irradiated with ultraviolet ozone for 10 minutes. After the ultraviolet light treatment, NiO is sputtered on the transparent conductive film 20 in a magnetron sputtering coating machine by a magnetron sputtering method. x After sputtering, the film is annealed. The NiO x The layer serves as a hole transport layer 30;
[0143] S4, forming a lower interface seed auxiliary growth layer 40 on the hole transport layer 30:
[0144] The lower interface seed auxiliary growth layer 40 is prepared by vacuum evaporation method. Specifically, the seed layer solid powder (CsPbBr3) is placed in a crucible as an evaporation source, the evaporation source is placed in the cavity of the evaporation machine, the substrate formed in step S3 is placed on the turntable of the vacuum chamber of the evaporation equipment, the door is closed, the vacuum is pumped, and the ionization gauge reading is observed until the vacuum degree reaches 10 -3Pa turns on the power supply and controls the evaporation speed by adjusting the current to maintain the evaporation speed at During the evaporation process, the thickness of the deposited film is detected by a quartz crystal film thickness monitor until the thickness of the lower interface seed auxiliary growth layer 40 (CsPbBr3) deposited on the surface of the hole transport layer 30 reaches 5nm, and then the DC power supply is turned off, and the deposition of the lower interface seed auxiliary growth layer 40 (CsPbBr3) is completed;
[0145] S5, forming a perovskite thin film layer 50 on the lower interface seed auxiliary growth layer 40;
[0146] S51, depositing PbI2 thin film: using thermal evaporation method to deposit PbI2 on the lower interface seed auxiliary growth layer 40, that is, the vacuum degree reaches 10 -3 Pa, turn on the power supply, and adjust the current to control the evaporation speed of PbI2. During the evaporation process, the deposited film thickness is detected by a quartz crystal film thickness monitor until the thickness of PbI2 deposited on the surface of the hole transport layer 30 reaches 200nm, the DC power supply is turned off, and the PbI2 film deposition is completed;
[0147] S52, in an atmospheric environment, at an ambient temperature and humidity of 25° C. and 30% respectively, coating an isopropanol solution containing formamidine hydroiodide on the PbI2 film by a doctor blade coating method, with a gap between the doctor blade and the substrate of 200 μm and a coating speed of 15 mm / s, and then annealing at 170° C. for 30 min to form a perovskite film layer 50;
[0148] S6, forming an electron transport layer 60 on the upper surface of the perovskite thin film layer 50, the electron transport layer 60 comprising a C60 thin film and SnO x Film; the specific steps are as follows:
[0149] S61, depositing C60 on the perovskite thin film layer 50 by thermal evaporation, that is, placing the substrate obtained in step S5 on a turntable in a vacuum chamber of an evaporation device, with a background vacuum better than 1×10 -3 Pa, C60 The C60 film with a thickness of 20 nm was obtained by evaporation at a rate of 1.5 %.
[0150] S62, Preparation of SnO on C60 film by atomic layer deposition x The process conditions are as follows: vacuum degree 10Pa, firstly TDMASn (tetra(dimethylamine)tin) is introduced with a pulse time of 0.6s, then nitrogen is purged for 30s, then H2O is introduced with a pulse time of 0.6s, after the H2O pulse, nitrogen is purged again for 30s, and the above steps are repeated 60 times, and the substrate temperature is maintained at about 90℃ during the whole process, and a SnO film with a thickness of about 10nm is obtained. x film;
[0151] S7, performing a second laser etching to form a second separation line P2 on the hole transport layer 30, the lower interface seed auxiliary growth layer 40, the perovskite thin film layer 50 and the electron transport layer 60;
[0152] S8, in SnO x An indium oxide-based transparent conductive oxide layer 80 is grown on the film by magnetron sputtering or RPD (reactive sputtering);
[0153] S9, forming a comb-shaped metal electrode layer 70 (comb-shaped copper electrode layer) on the indium oxide-based transparent conductive oxide layer 80:
[0154] A comb-shaped copper electrode layer is deposited on the indium oxide-based transparent conductive oxide layer 80 by a thermal evaporation method, that is, the substrate after etching in step S8 is placed on a turntable in a vacuum chamber of an evaporation device, copper particles are placed in a tungsten boat, and the metal electrode layer 70 (comb-shaped copper electrode layer) is obtained by thermal evaporation at a certain rate;
[0155] S10 , performing a third laser etching to form a third separation line P3 on the hole transport layer 30 , the lower interface seed auxiliary growth layer 40 , the perovskite film layer 50 , the electron transport layer 60 , the indium oxide-based transparent conductive oxide layer 80 and the metal electrode layer 70 .
[0156] Comparative Example 1
[0157] This comparative example provides a method for preparing a perovskite solar cell module. The difference between this preparation method and Example 1 is that this comparative example does not include the content in step S4, and the other steps and methods are the same as those in Example 1, which will not be repeated here.
[0158] Performance Testing
[0159] The perovskite solar cell modules prepared in Examples 1 to 4 and Comparative Example 1 were placed on the test bench, and their power conversion efficiency (PCE), open circuit voltage (Voc), fill factor (FF), and short circuit current (Isc) were tested under standard light intensity. The results show that the various parameters of the electrical performance of the perovskite solar cell modules prepared in Examples 1 to 4 are significantly improved, among which the open circuit voltage is improved most significantly, followed by the fill factor, mainly because after adding the lower interface seed auxiliary growth layer 40, the quality of the perovskite film is greatly improved due to its induced growth effect. In addition, it improves the interface between the hole transport layer 30 and the perovskite, reduces the charge recombination at the lower interface, and significantly improves the performance of the battery module.
[0160] Table 1 Comparison of electrical performance results of perovskite solar cell modules in Examples 1 to 4 and Comparative Example 1
[0161] project PCE(%) Voc(V) FF(%) <![CDATA[Isc(mA / cm 2 )]]> Comparative Example 1 17.62 11.56 74.23 2.05 Example 1 20.02 12.11 79.37 2.08 Example 2 20.33 12.10 79.87 2.10 Example 3 20.00 12.07 79.16 2.09 Example 4 19.45 12.08 77.75 2.07
[0162] In summary, the present invention provides a high-efficiency, high-stability large-area perovskite solar cell module and a preparation method thereof, wherein a lower interface seed auxiliary growth layer is prepared by a vacuum evaporation method, and the lower interface seed auxiliary growth layer is used as a nucleation site to induce perovskite growth, thereby preparing a large-area, high-quality perovskite film layer with large grains, no pinholes, and few defects, thereby improving the photoelectric performance and stability of α-FAPbI3 perovskite, and improving the conductivity and charge extraction efficiency of the hole transport layer, reducing interface charge recombination, and further improving the photoelectric conversion efficiency and stability of large-area perovskite solar cells; and the preparation steps are simple, the process is stable, and the repeatability is strong, and it can be widely used in the industrial preparation process of perovskite film. Therefore, the present invention effectively overcomes the various shortcomings in the prior art and has a high industrial utilization value.
[0163] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a perovskite solar cell module, characterized in that: The preparation method comprises the following steps: S1. providing a substrate, wherein the substrate is covered with a transparent conductive film; S2, performing a first laser etching on the transparent conductive film to form a first separation line on the transparent conductive film; S3, forming a hole transport layer on the transparent conductive film; S4, forming a lower interface seed auxiliary growth layer on the hole transport layer; S5, forming a perovskite thin film layer on the lower interface seed auxiliary growth layer; S6, forming an electron transport layer on the upper surface of the perovskite thin film layer; S7, performing a second laser etching to form a second separation line on the hole transport layer, the lower interface seed auxiliary growth layer, the perovskite thin film layer and the electron transport layer; S8, forming a metal electrode layer on the electron transport layer; S9, performing a third laser etching to form a third separation line on the hole transport layer, the lower interface seed auxiliary growth layer, the perovskite film layer, the electron transport layer and the metal electrode layer.
2. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: Step S1 includes one or a combination of the following conditions: The substrate is a rigid conductive substrate or a flexible conductive substrate; The transparent conductive film is one or a combination of FTO, AZO, ITO and IWO.
3. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: Step S3 includes one or a combination of the following conditions: The hole transport layer is prepared by a method selected from the group consisting of a spraying method, a coating method, a scraping method, a sputtering magnetron sputtering method, and a thermal evaporation method. The hole transport layer is one or a combination of Spiro-OMe TAD, PTAA, PEDOT:PSS, nickel oxide, copper oxide, vanadium oxide, tungsten oxide, and cuprous thiocyanate.
4. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: The lower interface seed auxiliary growth layer in step S4 is prepared by vacuum evaporation method, specifically: The seed layer solid powder is used as an evaporation source, and evaporation is performed under vacuum conditions until a lower interface seed auxiliary growth layer with a thickness of 5 to 10 nm is formed on the surface of the hole transport layer; wherein the seed layer solid powder is CsPbBr3 or CsPbI3, and the vacuum degree is 10 -5 Pa~10 -3 Pa.
5. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: The method for preparing the perovskite thin film layer in step S5 is specifically as follows: first depositing a PbI2 thin film, then coating the PbI2 thin film with an organic ammonium halide solution by blade coating or slit coating, and then annealing and crystallizing to form a perovskite thin film layer.
6. The method for preparing a perovskite solar cell module according to claim 5, characterized in that: The solute of the organic ammonium halide solution is one or a combination of formamidine hydroiodide, methylamine hydroiodide, formamidine hydrochloride, methylamine hydrochloride, formamidine hydrobromide, and methylamine hydrobromide, and the solvent of the organic ammonium halide solution is one or a combination of isopropanol and ethanol.
7. The method for preparing a perovskite solar cell module according to claim 5, characterized in that: Includes one or a combination of the following conditions: The thickness of the deposited PbI2 film is 200-400 nm; The annealing temperature is 130-180° C., and the annealing time is 10-40 minutes.
8. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: The preparation method of the electron transport layer in step S6 includes one of spraying, coating, blade coating, sputtering, and thermal evaporation, and the electron transport layer is one or a combination of PCBM, C60, BCP, SnO2, titanium oxide, and zinc oxide.
9. The method for preparing a perovskite solar cell module according to claim 1, characterized in that: The metal electrode layer in step S8 is prepared by any one of thermal evaporation, sputtering, and scraping, and the metal electrode layer material includes one of gold, silver, aluminum, copper, nickel, carbon, and ITO.
10. A perovskite solar cell module prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The perovskite solar cell module comprises a substrate, a transparent conductive film, a hole transport layer, a lower interface seed auxiliary growth layer, a perovskite film layer, an electron transport layer, and a metal electrode layer which are stacked in sequence.