Lanthanum-doped barium stannate nanocrystalline implanted TiO2-SnO2 electron transport layer and preparation method and application thereof
By implanting lanthanum-doped barium stannate nanocrystals into the electron transport layer of perovskite solar cells, the problems of low conductivity and stability of a single electron transport layer are solved, and the carrier mobility and photoelectric conversion efficiency are improved, thereby enhancing the The performance of perovskite solar cells.
Patent Information
- Application Number
- CN202411218679.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
The single electron transport layer commonly used in existing perovskite solar cells is difficult to transport electrons and holes due to low conductivity and imperfect band matching. The TiO2 electron transport layer absorbs ultraviolet light and emits high-energy electrons, which affects stability. sex.
The nanocrystalline colloidal solution of lanthanum doped barium stannate was prepared by liquid-phase laser irradiation technology, and implanted into the TiO2-SnO2 electron transport layer obtained by chemical liquid deposition method, and form lanthanum doped barium stannate by hydrothermal and heat treatment. The nanocrystal implanted TiO2-SnO2 electron transport layer provides additional carrier transport channels.
The carrier mobility and electron transmission efficiency are improved, the photoelectric conversion efficiency and stability of perovskite solar cells are enhanced, and the electron mobility reaches 320cm2V-1s-1, optimizing carrier transmission.
Smart Images

Figure CN119095457A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and specifically relates to a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, and a preparation method and application thereof. Background Art
[0002] In the photovoltaic field, organic-inorganic hybrid perovskite solar cells have developed rapidly due to their advantages of low cost, high efficiency, and low-temperature solution preparation. Their photoelectric conversion efficiency has exceeded 26%, almost comparable to that of single-crystal silicon solar cells. Considering that existing perovskite solar cells often use a single electron transport layer, due to low conductivity and imperfect band matching, it is impossible to meet the balanced transport of electrons and holes, resulting in the inability to further improve the efficiency of perovskite cells. In addition, the commonly used TiO2 electron transport layer absorbs ultraviolet light to emit high-energy electrons, which will also degrade the perovskite and affect stability.
[0003] Based on this, the prior art provides a TiO2-SnO2 electron transport layer by chemical liquid deposition, that is, the TiO2 electron transport layer is first deposited by hydrothermal treatment, and then the SnO2 electron transport layer is continuously deposited on the TiO2 electron transport layer by heat treatment. Compared with the existing TiO2 electron transport layer, the TiO2-SnO2 electron transport layer obtained by chemical liquid deposition has uniform coverage, excellent conductivity, and a smooth surface, and overcomes the problem that the TiO2 electron transport layer absorbs ultraviolet light and then emits high-energy electrons, thereby obtaining a higher quality electron transport layer. In addition, the TiO2-SnO2 electron transport layer obtained by chemical liquid deposition has high efficiency and good stability in perovskite solar cells, and the photoelectric conversion efficiency is also effectively improved, which greatly improves the photoelectric conversion efficiency and stability of perovskite solar cells based on the TiO2 electron transport layer, and has extremely high application prospects.
[0004] However, the TiO2-SnO2 electron transport layer obtained by chemical liquid deposition still has grain surfaces and thin film interfaces, which makes its carrier transport inevitably affected by surface and interface defects, namely, carrier non-radiative recombination centers, which in turn affects the photoelectric conversion efficiency. Summary of the invention
[0005] In view of the deficiencies in the above-mentioned prior art, the present invention provides a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, and a preparation method and application thereof. The present invention adopts liquid phase laser irradiation technology to obtain a lanthanum-doped barium stannate nanocrystal colloidal solution with uniform particle size and uniform dispersion in a solvent, and implants the lanthanum-doped barium stannate nanocrystals into the TiO2-SnO2 electron transport layer obtained based on a chemical liquid phase deposition method, thereby effectively improving the carrier mobility of the TiO2-SnO2 electron transport layer, and the surface interface remaining in the electron transport layer after heat treatment and crystallization provides an additional channel for carrier transmission, so that the obtained TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals has high electron transport efficiency and is dense, and the perovskite solar cell obtained by using the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals has high photoelectric conversion efficiency and good stability.
[0006] The present invention is achieved through the following technical solutions:
[0007] The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0008] The lanthanum-doped barium stannate target is immersed in a solvent, and the lanthanum-doped barium stannate target is irradiated with a liquid phase laser and ultrasonicated at the same time to prepare a lanthanum-doped barium stannate nanocrystal colloidal solution;
[0009] Titanium tetrachloride is used as a raw material, and titanium tetrachloride is dripped onto ice water, wherein the ice water is ice, water with a temperature below 4°C, or an ice-water mixture, and the ice is completely melted to obtain a titanium dioxide precursor solution, and after the titanium dioxide precursor solution is ultrasonically dispersed, a lanthanum-doped barium stannate nanocrystal colloidal solution is added thereto, and the solution is placed in a culture dish with a diameter of 60-150 mm, and a hydrothermal treatment is first performed to grow a layer of titanium dioxide wet film on the surface of the conductive glass, and then a heat treatment is performed to crystallize, that is, a TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals is prepared by a chemical liquid phase deposition method, and the chemical liquid phase deposition method includes a hydrothermal treatment and a heat treatment;
[0010] The tin dioxide aqueous solution is diluted into a colloidal solution. The tin dioxide is diluted by stirring, vibration and ultrasound. The dilution time is 2-12 hours. The tin dioxide is spin-coated on the TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals. The rotation speed of the tin dioxide colloid is 2000-4000r / min. After annealing, the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals is obtained.
[0011] Preferably, the solvent is water.
[0012] Preferably, the laser emission wavelength of the liquid phase laser irradiation is 1064nm, and the laser irradiation range is 0.8-1.3cm; the conditions of the liquid phase laser irradiation are: the laser irradiation is 5-10min at a pulse frequency of 10Hz, a pulse width of 8ns, a spot size of 13mm, an ambient temperature of 0-25°C, and a laser irradiation energy of 0.8-1.2J. The lanthanum-doped barium stannate target is irradiated, and the main influencing factor in the irradiation is the laser irradiation energy. If the laser irradiation energy is too large, the nanocrystals prepared will be uneven in size and large in particles, and the lanthanum-doped barium stannate target will even be broken. If the laser irradiation energy is too small, the lanthanum-doped barium stannate target cannot be prepared into nanocrystals.
[0013] Preferably, the amount of the titanium dioxide precursor solution is 20-40 g / L, the amount of the lanthanum-doped barium stannate nanocrystal colloidal solution is 0.01-0.1 g / L, and the volume ratio of the titanium dioxide precursor solution to the lanthanum-doped barium stannate nanocrystal colloidal solution is 100:0.5-1. If the amount of the lanthanum-doped barium stannate nanocrystal colloidal solution is too high, it will agglomerate in the titanium dioxide precursor solution to form larger particles, and lose the characteristics of uniform dispersion before heat treatment crystallization film formation, and the prepared lanthanum-doped barium stannate nanocrystal implanted TiO2 electron transport layer has low performance; if the amount of the lanthanum-doped barium stannate nanocrystal colloidal solution is too low, the ability to regulate the carrier extraction and transmission of the TiO2 electron transport layer implanted with the lanthanum-doped barium stannate nanocrystal is weak, and the photoelectric conversion efficiency and perovskite solar cell obtained within the range of 100:0.5-1 are both good.
[0014] Preferably, the conditions for the hydrothermal treatment are: hydrothermal treatment at 70-90°C for 60-90min. This step only needs to ensure that titanium tetrachloride and water fully react to generate titanium dioxide. Heating is to provide the chemical potential conditions required for the reaction; at the same time, the heating temperature can be below the boiling point of water. If the temperature is too low, the reaction rate is too slow, and if the temperature is too high, the reaction rate is too fast. For every 10°C increase in temperature, the rate increases by 2-4 times the original.
[0015] Preferably, the heat treatment conditions are: heat treatment at 100-150°C for 60-120 minutes. The purpose of the heat treatment is to fully volatilize the moisture in the wet film. The heating temperature can be above the boiling point of water. Too high a temperature will cause the culture dish and the conductive glass to break due to uneven heating.
[0016] Preferably, the volume fraction of tin dioxide in the colloidal solution is 1-5%.
[0017] Preferably, the annealing treatment conditions are: annealing at 100-150° C. for 30-90 min.
[0018] The present invention also protects the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals obtained by the above-mentioned preparation method. The TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals consists of a TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals and a SnO2 electron transport layer, which are stacked up and down, and the thickness of the TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals and the SnO2 electron transport layer are both 10-30nm.
[0019] The present invention also protects the application of a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in the preparation of a perovskite solar cell, which is characterized in that the perovskite solar cell is stacked in sequence by a metal electrode layer, a hole transport layer, a perovskite layer, a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals and a transparent conductive substrate.
[0020] The preparation method of perovskite solar cells is:
[0021] S1. implanting a transparent conductive substrate into a culture dish and immersing it in a mixed solution of a titanium dioxide precursor solution and a lanthanum-doped barium stannate nanocrystal colloidal solution, and depositing a TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals on the surface of the transparent conductive substrate by chemical liquid deposition;
[0022] S2, depositing a tin dioxide electron transport layer on one side of the TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals to obtain a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals;
[0023] S3, dropping a perovskite precursor solution onto the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, then dropping an anti-solvent under high-speed rotation conditions, and then performing a heat treatment at a temperature of 130-150° C. for a time of 10-15 minutes to obtain a perovskite layer;
[0024] S4, spin coating a passivation layer and a hole transport layer on the perovskite layer, and evaporating a metal on the hole transport layer to obtain a perovskite solar cell;
[0025] In step S4, the solute of the passivation layer is phenethylammonium iodide, the concentration is 0.02 mol / L, and the solvent is isopropanol; the spin coating rate of the phenethylammonium iodide solution is 4000-5000 r / min;
[0026] In step S4, the solute of the hole transport layer is 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene with a concentration of 0.05 mmol / mL and the solvent is chlorobenzene; the spin coating rate of the 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene solution is 4000-5000 r / min.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. Considering that the TiO2-SnO2 electron transport layer obtained by the chemical liquid deposition method in the prior art still has grain surfaces and thin film interfaces, its carrier transport will inevitably be affected by surface interface defects, namely, carrier non-radiative recombination centers. In the present invention, lanthanum-doped barium stannate nanocrystals are implanted during the preparation of the titanium dioxide electron transport layer, and lanthanum-doped barium stannate nanocrystals are used to passivate the surface interface defects of the TiO2-SnO2 electron transport layer, that is, to reduce non-radiative recombination in the form of improving carrier mobility, and at the same time serve as additional channels to improve carrier transport efficiency.
[0029] 2. This invention is the first to apply rare earth element-doped ternary oxides in the TiO2-SnO2 electron transport layer, that is, lanthanum-doped barium stannate is used as an additive, and its electron mobility is as high as 320cm 2 V -1 s -1 , exceeding 240cm of tin dioxide 2 V -1 s -1 , which can accelerate the extraction and transport of photogenerated electrons. The results show that embedding lanthanum-doped barium stannate in the electron transport layer is an effective strategy to optimize carrier transport.
[0030] 3. The present invention prepares a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals with uniform coverage, excellent conductivity and a smooth surface. The photoelectric conversion efficiency of the perovskite solar cell prepared based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals is effectively improved, which promotes the development of perovskite solar cells and has a high application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the structure of a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to Examples 1 to 3 of the present invention;
[0032] Figure 2 This is a physical picture of the lanthanum-doped barium stannate nanocrystal colloidal solution of Example 1;
[0033] Figure 3The transmission electron microscope image and particle size distribution diagram of the lanthanum-doped barium stannate nanocrystal colloidal solution of Example 1;
[0034] Figure 4 The current-voltage curve of the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 1;
[0035] Figure 5 The current-voltage curve of the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 2;
[0036] Figure 6 The current-voltage curve of the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 3;
[0037] Figure 7 This is a current-voltage curve of a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation in Comparative Example 1;
[0038] Figure 8 The current-voltage curve of the perovskite solar cell based on the TiO2-SnO2 electron transport layer without nanocrystal implantation in comparative example 2;
[0039] Fig. 9 The current-voltage curve of the perovskite solar cell based on the TiO2-SnO2 electron transport layer without nanocrystal implantation in comparative example 3;
[0040] Fig.10 This is a stability comparison chart of the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 3 and the perovskite solar cell based on the TiO2-SnO2 electron transport layer without nanocrystal implantation in Comparative Example 3.
[0041] Explanation of the reference numerals: 1. Transparent conductive substrate; 2. TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals; 3. Perovskite layer; 4. Hole transport layer; 5. Metal electrode. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described below in conjunction with specific embodiments, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. The applicant declares that the above embodiments are preferred implementations of the present invention, but the implementation of the present invention is not limited by the above embodiments, and any other equivalent replacement methods that do not deviate from the spirit and principle of the present invention are included in the protection scope of the present invention.
[0043] The present invention provides a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, which has high conductivity, cheap raw materials and simple process, and a preparation method thereof, and develops a high-efficiency and stable perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals. Lanthanum-doped barium stannate (LBSO) is an n-type semiconductor material with a high conductivity of up to 320 cm 2 V -1 s -1 The electron mobility of the TiO2-SnO2 electron transport layer is improved by implanting LBSO nanocrystals into the TiO2-SnO2 electron transport layer, which is simple to operate and can effectively improve the energy level of the TiO2-SnO2 electron transport layer and promote the extraction and transmission of carriers in the electron transport layer.
[0044] The technical solution of the present invention is further studied by using embodiments and comparative examples below. The specific research methods and results are as follows:
[0045] Example 1
[0046] The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0047] Step 1: Place the LBSO target in a glass bottle in a clean environment, add deionized water to wash, then separate the deionized water to obtain a clean target, mix the clean target with 10 mL of deionized water, and then irradiate it with a pulsed laser (Nd: YAG, 10 Hz, wavelength 1064 nm, energy 1 J) for 5 minutes to obtain a light yellow LBSO nanocrystal colloidal solution.
[0048] Step 2. In a clean environment, add 800 μL of titanium tetrachloride to 40 mL of frozen ultrapure water, and after it is completely melted, obtain a titanium dioxide precursor solution. Add 400 μL of LBSO nanocrystal colloidal solution to the titanium dioxide precursor solution to obtain a mixed solution, and then pour it into a culture dish with a diameter of 100 mm. Then immerse the cleaned FTO conductive glass in the mixed solution, first place it in a 70°C oven for hydrothermal treatment for 60 minutes, and after the hydrothermal treatment is completed, take out the conductive glass, thoroughly wash it with ultrapure water and anhydrous ethanol, and then blow dry it with nitrogen, and then place it in a 100°C oven for heat treatment for 60 minutes to obtain a TiO2 electron transport layer with a thickness of 20 nm and implanted with lanthanum-doped barium stannate nanocrystals.
[0049] Step 3. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with deionized water to a 2% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in step 2, set the speed to 4000 rpm, the time to 30 s, and after spin coating, heat treat at 100°C for 90 min to obtain a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals. The thickness of the tin dioxide layer is 20 nm.
[0050] The method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0051] S1. Prepare 1.25 mol / L Cs in an argon glove box. 0.05 FA 0.81 MA 0.14 PbI 2.55 Br 0.45 (CsFAMA) perovskite precursor solution: 8.12 mg of CH3NH3I, 86.76 mg of HC(=NH)NH3I, 9.97 mg of CH3NH3Br, 247.07 mg of PbI2 and 32.68 mg of PbBr2 were mixed in a small reagent bottle, and 400 μL of dimethylformamide and 100 μL of dimethyl sulfoxide were added to obtain a mixed solution, which was stirred at 50°C for 3 h and filtered with a 220 nm nylon 66 organic filter head to obtain 0.5 mL of 1.25 mol / L perovskite precursor solution for the experiment;
[0052] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, spin-coat it at high speed (4000 rpm) for 30 seconds, and immediately drop 200 μL of chlorobenzene solution when there are 10 seconds left in the high-speed spin-coating. After the drop-coating is completed, heat-treat it at 100°C for 60 minutes to prepare a CsFAMA perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0053] S3, spin coating a layer of phenethylamine iodide as a surface passivation layer on the FAPbI3 perovskite film of step S2, spin coating at high speed (5000 r / min) for 30 seconds without heat treatment, to obtain a surface passivated FAPbI3 perovskite film;
[0054] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface passivated CsFAMA perovskite film in step S3, spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0055] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, and a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals.
[0056] Example 2
[0057] The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0058] Step 1: Place the LBSO target in a glass bottle in a clean environment, add deionized water to wash, then separate the deionized water to obtain a clean target, mix the clean target with 10 mL of deionized water, and then irradiate it with a pulsed laser (Nd: YAG, 10 Hz, wavelength 1064 nm, energy 0.8 J) for 10 min to obtain a light yellow LBSO nanocrystal colloidal solution.
[0059] Step 2. In a clean environment, add 3200 μL of titanium tetrachloride to 200 mL of frozen ultrapure water, and after it is completely melted, obtain a titanium dioxide precursor solution. Add 1 mL of LBSO nanocrystal colloidal solution to the titanium dioxide precursor solution to obtain a mixed solution, and then pour it into a culture dish with a diameter of 160 mm. Then immerse the cleaned FTO conductive glass in the mixed solution, first place it in a 75°C oven for hydrothermal treatment for 90 minutes, and after the hydrothermal treatment is completed, take out the conductive glass, thoroughly wash it with ultrapure water and anhydrous ethanol, and then blow dry it with nitrogen, and then place it in a 150°C oven for heat treatment for 60 minutes to obtain a TiO2 electron transport layer with a thickness of 30 nm and implanted with lanthanum-doped barium stannate nanocrystals.
[0060] Step 3. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with water to a 1% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in step 2, set the speed to 4000 rpm, after 30 seconds, spin coat and heat treat at 150°C for 30 minutes to obtain a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, and the thickness of the tin dioxide layer is 10 nm.
[0061] The method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0062] S1. Prepare 1.55 mol / L Cs in an argon glove box. 0.05 FA 0.85 MA 0.10 PbI 2.91 Br 0.09 (FAMACs) Perovskite precursor solution: 20.2 mg of CH3NH3Cl, 226.7 mg of HC(=NH)NH3I, 17.5 mg of CH3NH3Br, 750.4 mg of PbI2 and 20.3 mg of CsI were mixed in a small reagent bottle, and 800 μL of dimethylformamide and 200 μL of dimethyl sulfoxide were added to obtain a mixed solution. The mixed solution was stirred at 60°C for 2 h, and filtered with a 220 nm nylon 66 organic filter head to obtain 1 mL of 1.55 mol / L perovskite precursor solution for the experiment;
[0063] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, spin-coat it at high speed (4000 rpm) for 30 seconds, and immediately drop 200 μL of chlorobenzene solution when there are 10 seconds left in the high-speed spin-coating. After the drop-coating is completed, heat-treat it at 100°C for 60 minutes to prepare a FAMACs perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0064] S3, spin coating a layer of phenethylamine iodide as a surface passivation layer on the FAPbI3 perovskite film of step S2, spin coating at high speed (5000 r / min) for 30 seconds without heat treatment, to obtain a surface passivated FAPbI3 perovskite film;
[0065] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface-passivated FAMACs perovskite film in step S3, spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0066] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, and a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals.
[0067] Example 3
[0068] The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0069] Step 1: Place the LBSO target in a glass bottle in a clean environment, add deionized water to wash, then separate the deionized water to obtain a clean target, mix the clean target with 10 mL of deionized water, and then irradiate it with a pulsed laser (Nd: YAG, 10 Hz, wavelength 1064 nm, energy 1 J) for 10 min to obtain a light yellow LBSO nanocrystal colloidal solution.
[0070] Step 2. In a clean environment, add 750 μL of titanium tetrachloride to 30 mL of frozen ultrapure water, and after it is completely melted, obtain a titanium dioxide precursor solution. Add 200 μL of LBSO nanocrystal colloidal solution to the titanium dioxide precursor solution to obtain a mixed solution, which is then poured into a culture dish with a diameter of 60 mm. The cleaned FTO conductive glass is immersed in the mixed solution, first placed in a 90°C oven for hydrothermal treatment for 60 minutes, and after the hydrothermal treatment is completed, the conductive glass is taken out, thoroughly washed with ultrapure water and anhydrous ethanol, and then blown dry with nitrogen, and then placed in a 130°C oven for heat treatment for 90 minutes to obtain a TiO2 electron transport layer with a thickness of 20 nm and implanted with lanthanum-doped barium stannate nanocrystals.
[0071] Step 3. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with water to a 4% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in step 2, set the speed to 4000 rpm, after 30 seconds, spin coat and heat treat at 130°C for 60 minutes to obtain a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, and the thickness of the tin dioxide layer is 30 nm.
[0072] The method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals comprises the following steps:
[0073] S1. Prepare 1.8 mol / L FAPbI3 perovskite precursor solution in an argon glove box: mix 24.3 mg CH3NH3I, 154 mg HC(=NH)NH3I and 414 mg PbI2 in a small reagent bottle, add 400 μL dimethylformamide and 100 μL dimethyl sulfoxide to obtain a mixed solution, stir the mixed solution at 60°C for 2 h, filter with a 220 nm nylon 66 organic filter head, and obtain 0.5 mL of 1.8 mol / L perovskite precursor solution for the experiment;
[0074] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, spin-coat it at high speed (6000 rpm) for 50 seconds, and immediately add 200 μL of ethyl acetate at the 10th second of high-speed spin-coating. After the addition is complete, heat-treat it at 150°C for 10 minutes to prepare a FAPbI3 perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0075] S3. Spin-coat a layer of phenethylammonium iodide as a surface passivation layer on the FAPbI3 perovskite film obtained in step S2 at a high speed (5000 r / min) for 30 seconds without heat treatment to obtain a surface passivated FAPbI3 perovskite film.
[0076] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface passivated FAPbI3 perovskite film in step S3, i.e., spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0077] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, and a perovskite solar cell based on a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals.
[0078] Comparative Example 1
[0079] The preparation method of the TiO2-SnO2 electron transport layer is the same as the preparation steps of Example 1, except that no lanthanum-doped barium stannate nanocrystals are implanted, and includes the following steps:
[0080] Step 1. In a clean environment, add 800 μL of titanium tetrachloride to 40 mL of frozen ultrapure water, and after it is completely melted, a titanium dioxide precursor solution is obtained. The titanium dioxide precursor solution is poured into a culture dish with a diameter of 100 mm, and then the cleaned FTO conductive glass is immersed in the titanium dioxide precursor solution. It is first placed in a 70°C oven for hydrothermal treatment for 60 minutes. After the hydrothermal treatment is completed, the conductive glass is taken out, and it is thoroughly washed with ultrapure water and anhydrous ethanol, and then blown dry with nitrogen. Then, it is placed in a 100°C oven for heat treatment for 60 minutes to obtain a TiO2 electron transport layer with a thickness of 20 nm.
[0081] Step 2. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with deionized water to a 2% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer in step 1, set the speed to 4000 rpm, the time to 30 s, and after spin coating, heat treat at 100 ° C for 90 min to obtain a TiO2-SnO2 electron transport layer with a thickness of 20 nm.
[0082] A method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation comprises the following steps:
[0083] S1. Prepare 1.25 mol / L Cs in an argon glove box. 0.05 FA 0.81 MA 0.14 PbI 2.55 Br 0.45 (CsFAMA) perovskite precursor solution: 8.12 mg of CH3NH3I, 86.76 mg of HC(=NH)NH3I, 9.97 mg of CH3NH3Br, 247.07 mg of PbI2 and 32.68 mg of PbBr2 were mixed in a small reagent bottle, and 400 μL of dimethylformamide and 100 μL of dimethyl sulfoxide were added to obtain a mixed solution, which was stirred at 50°C for 3 h and filtered with a 220 nm nylon 66 organic filter head to obtain 0.5 mL of 1.25 mol / L perovskite precursor solution for the experiment;
[0084] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer, spin-coat it at high speed (4000 rpm) for 30 seconds, and immediately add 200 μL of chlorobenzene solution when there are 10 seconds left in the high-speed spin-coating. After the addition is completed, heat-treat it at 100°C for 60 minutes to prepare a CsFAMA perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0085] S3, spin coating a layer of phenethylamine iodide as a surface passivation layer on the FAPbI3 perovskite film of step S2, spin coating at high speed (5000 r / min) for 30 seconds without heat treatment, to obtain a surface passivated FAPbI3 perovskite film;
[0086] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface passivated CsFAMA perovskite film in step S3, spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0087] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, to obtain a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation.
[0088] Comparative Example 2
[0089] The preparation method of the TiO2-SnO2 electron transport layer is the same as the preparation steps of Example 2, except that no lanthanum-doped barium stannate nanocrystals are implanted, and includes the following steps:
[0090] Step 1. In a clean environment, add 3200 μL of titanium tetrachloride to 200 mL of frozen ultrapure water, and after it is completely melted, obtain a titanium dioxide precursor solution. Pour the titanium dioxide precursor solution into a culture dish with a diameter of 160 mm, and then immerse the cleaned FTO conductive glass in the titanium dioxide precursor solution. First, place it in a 75°C oven for hydrothermal treatment for 90 minutes. After the hydrothermal treatment is completed, take out the conductive glass, wash it thoroughly with ultrapure water and anhydrous ethanol, and then blow it dry with nitrogen. Then, place it in a 150°C oven for heat treatment for 60 minutes to obtain a TiO2 electron transport layer with a thickness of 30 nm.
[0091] Step 2. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with water to a 1% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer in step 1, set the speed to 4000 rpm, after 30 seconds, spin coat and heat treat at 150°C for 30 minutes to obtain a TiO2-SnO2 electron transport layer with a thickness of 10 nm.
[0092] A method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation comprises the following steps:
[0093] S1. Prepare 1.55 mol / L Cs in an argon glove box. 0.05 FA 0.85 MA 0.10 PbI 2.91 Br 0.09 (FAMACs) Perovskite precursor solution: 20.2 mg of CH3NH3Cl, 226.7 mg of HC(=NH)NH3I, 17.5 mg of CH3NH3Br, 750.4 mg of PbI2 and 20.3 mg of CsI were mixed in a small reagent bottle, and 800 μL of dimethylformamide and 200 μL of dimethyl sulfoxide were added to obtain a mixed solution. The mixed solution was stirred at 60°C for 2 h, and filtered with a 220 nm nylon 66 organic filter head to obtain 1 mL of 1.55 mol / L perovskite precursor solution for the experiment;
[0094] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer, spin-coat it at high speed (4000 rpm) for 30 seconds, and immediately drop 200 μL of chlorobenzene solution when there are 10 seconds left in the high-speed spin coating. After the dropwise addition, heat treat it at 100°C for 60 minutes to prepare a FAMACs perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0095] S3, spin coating a layer of phenethylamine iodide as a surface passivation layer on the FAPbI3 perovskite film of step S2, spin coating at high speed (5000 r / min) for 30 seconds without heat treatment, to obtain a surface passivated FAPbI3 perovskite film;
[0096] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface-passivated FAMACs perovskite film in step S3, spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0097] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, to obtain a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation.
[0098] Comparative Example 3
[0099] The preparation method of the TiO2-SnO2 electron transport layer is the same as the preparation steps of Example 3, except that no lanthanum-doped barium stannate nanocrystals are implanted, and includes the following steps:
[0100] Step 1. In a clean environment, add 750 μL of titanium tetrachloride to 30 mL of frozen ultrapure water, and after it is completely melted, obtain a titanium dioxide precursor solution. Pour the titanium dioxide precursor solution into a culture dish with a diameter of 60 mm, and then immerse the cleaned FTO conductive glass in the titanium dioxide precursor solution. First place it in a 90°C oven for hydrothermal treatment for 60 minutes. After the hydrothermal treatment is completed, take out the conductive glass, wash it thoroughly with ultrapure water and anhydrous ethanol, and then blow it dry with nitrogen. Then, place it in a 130°C oven for heat treatment for 90 minutes to obtain a TiO2 electron transport layer with a thickness of 20 nm.
[0101] Step 2. In a clean environment, take 1 mL of a 15% tin dioxide aqueous solution, then dilute it with water to a 4% colloidal solution, take 100 μL and drop it on the TiO2-SnO2 electron transport layer in step 1, set the speed to 4000 rpm, after 30 seconds, spin coat and heat treat at 130°C for 60 minutes to obtain a TiO2-SnO2 electron transport layer with a thickness of 30 nm.
[0102] A method for preparing a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation comprises the following steps:
[0103] S1. Prepare 1.8 mol / L FAPbI3 perovskite precursor solution in an argon glove box: mix 24.3 mg CH3NH3I, 154 mg HC(=NH)NH3I and 414 mg PbI2 in a small reagent bottle, add 400 μL dimethylformamide and 100 μL dimethyl sulfoxide to obtain a mixed solution, stir the mixed solution at 60°C for 2 h, filter with a 220 nm nylon 66 organic filter head, and obtain 0.5 mL of 1.8 mol / L perovskite precursor solution for the experiment;
[0104] S2, take 50 μL of the perovskite precursor solution of step S1 and spin-coat it on the TiO2-SnO2 electron transport layer, spin-coat it at high speed (6000 rpm) for 50 seconds, and immediately add 200 μL of ethyl acetate at the 10th second of high-speed spin-coating. After the addition is complete, heat-treat it at 150°C for 10 minutes to prepare a FAPbI3 perovskite film with a uniform and flat surface and a thickness of 600 nm;
[0105] S3. Spin-coat a layer of phenethylammonium iodide as a surface passivation layer on the FAPbI3 perovskite film obtained in step S2 at a high speed (5000 r / min) for 30 seconds without heat treatment to obtain a surface passivated FAPbI3 perovskite film.
[0106] S4, spin-coating a hole transport layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) with a thickness of 200 nm on the surface passivated FAPbI3 perovskite film in step S3, i.e., spin-coating at high speed (4000 rpm) for 30 seconds, and then oxidizing in dry oxygen for 24 hours to obtain a hole transport layer;
[0107] S5: Deposit a layer with an area of 0.1 cm on the hole transport layer in step S4. 2 , an Au electrode with a thickness of 100 nm, to obtain a perovskite solar cell based on a TiO2-SnO2 electron transport layer without nanocrystal implantation.
[0108] Figure 1 Schematic diagram of the structure of the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to Examples 1 to 3.
[0109] from Figure 2 It can be seen that the lanthanum-doped barium stannate nanocrystal colloidal solution has an obvious Tyndall effect, and an obvious light path can be seen after irradiation with a laser pen.
[0110] from Figure 3 The transmission electron microscopy and particle size statistics results showed that lanthanum-doped barium stannate nanoparticles were generated under the action of laser and evenly dispersed in water, proving that the lanthanum-doped barium stannate nanocrystals did not undergo crystal structure changes under the action of laser, and the particle size was about 2.12nm.
[0111] Figure 4 The photoelectric conversion efficiency of the perovskite solar cell is 22.55%. Figure 7 The photoelectric conversion efficiency of the perovskite solar cell is 21.25%; Figure 5 The photoelectric conversion efficiency of the perovskite solar cell is 23.71%. Figure 8 The photoelectric conversion efficiency of the perovskite solar cell is 22.06%; Figure 6 The photoelectric conversion efficiency of the perovskite solar cell is 24.17%. Fig. 9 The photoelectric conversion efficiency of the perovskite solar cell is 21.85%; Figure 4 and Figure 7 contrast, Figure 5 and Figure 8 contrast, Figure 6 and Fig. 9 The comparison results show that the photoelectric conversion efficiency of the perovskite solar cells obtained after implanting lanthanum-doped barium stannate nanocrystals is improved compared with the perovskite solar cells without implantation.
[0112] The perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 3 and the perovskite solar cell based on the TiO2-SnO2 electron transport layer without nanocrystal implantation in Comparative Example 3 were placed in a drying cabinet at a temperature of 25°C and a relative humidity of 10-30% for stability testing. The results are as follows: Fig.10 As shown, the results show that the perovskite solar cell based on the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals in Example 3 has basically no change in photoelectric conversion efficiency after being placed for 1000 hours, indicating that it has good stability, and the stability is better than that of the perovskite solar cell based on the TiO2-SnO2 electron transport layer without nanocrystal implantation in Example 3.
[0113] In addition, unless otherwise specified, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art in the art. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods related to the documents. In the event of any conflict with any incorporated document, the content of this specification shall prevail.
Claims
1. A method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals, characterized in that: The steps include: The lanthanum-doped barium stannate target is immersed in water, and the lanthanum-doped barium stannate target is irradiated with a liquid phase laser and ultrasonicated at the same time to prepare a lanthanum-doped barium stannate nanocrystal colloidal solution; Titanium tetrachloride is used as a raw material, titanium tetrachloride is added dropwise onto ice water, and the ice is completely melted to obtain a titanium dioxide precursor solution. After the titanium dioxide precursor solution is ultrasonically dispersed, a lanthanum-doped barium stannate nanocrystal colloidal solution is added thereto, and a titanium dioxide wet film is firstly grown by hydrothermal treatment, and then a heat treatment is performed for crystallization to obtain a TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals; The tin dioxide aqueous solution is diluted into a colloidal solution, and the solution is spin-coated on the TiO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals. After annealing, the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals is obtained.
2. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The laser emission wavelength of liquid phase laser irradiation is 1064nm, and the laser irradiation range is 0.8-1.3cm.
3. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The conditions of liquid phase laser irradiation are: laser irradiation for 5-10 min at a pulse frequency of 10 Hz, a pulse width of 8 ns, a spot size of 13 mm, an ambient temperature of 0-25° C., and a laser irradiation energy of 0.8-1.2 J.
4. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The amount of the titanium dioxide precursor solution is 20-40 g / L, the amount of the lanthanum-doped barium stannate nanocrystal colloidal solution is 0.01-0.1 g / L, and the volume ratio of the titanium dioxide precursor solution to the lanthanum-doped barium stannate nanocrystal colloidal solution is 100:0.5-1.
5. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The conditions of the hydrothermal treatment are: hydrothermal treatment at 70-90°C for 60-90 minutes.
6. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The heat treatment conditions are: heat treatment at 100-150°C for 60-120 minutes.
7. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The volume fraction of tin dioxide in the colloidal solution is 1-5%.
8. The method for preparing a TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals according to claim 1, characterized in that: The annealing conditions are: annealing at 100-150°C for 30-90 minutes.
9. A TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The TiO2-SnO2 electron transport layer implanted with lanthanum doped barium stannate nanocrystals consists of a TiO2 electron transport layer implanted with lanthanum doped barium stannate nanocrystals and a SnO2 electron transport layer, and the thickness of the TiO2 electron transport layer implanted with lanthanum doped barium stannate nanocrystals and the SnO2 electron transport layer are both 10-30nm.
10. A use of the TiO2-SnO2 electron transport layer implanted with lanthanum-doped barium stannate nanocrystals as claimed in claim 9 in the preparation of a perovskite solar cell, characterized in that: The perovskite solar cell is stacked in sequence by a metal electrode layer (5), a hole transport layer (4), a perovskite layer (3), a TiO2-SnO2 electron transport layer (2) implanted with lanthanum-doped barium stannate nanocrystals, and a transparent conductive substrate (1).
Citation Information
Cited By
Method for modifying buried interface of perovskite solar cell
CN119866156A
Method for modifying the buried interface of a perovskite solar cell
CN119866156B