1500 DEG C-resistant oxide film thermocouple and preparation method thereof
By using interlaced thin-film thermocouples with indium tin oxide and solid solution materials of samarium, calcium, and cobalt oxide in high temperature environments, the problems of high cost and small thermoelectric output of traditional high-temperature thermocouples are solved, and low cost, high output and Long-life high-temperature measurement performance, suitable for industrial applications.
Patent Information
- Application Number
- CN202411210785.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional high-temperature thermocouple materials have high cost, limited temperature measurement range, small thermoelectric output and are easily affected by catalysis, which cannot meet the accuracy, reliability and economic requirements of industrial high-temperature measurement.
Indium tin oxide is used as the N-type semiconductor oxide electrode, and samarium, calcium and cobalt oxide solid solution is used as the P-type semiconductor oxide electrode. Combined with high-temperature resistant electrical insulating substrate and temperature resistant metal pins, interleaving is prepared through magnetron sputtering technology. The structure of oxide film thermocouple accurately regulates the element content to improve high temperature resistance.
It realizes high-temperature measurement performance with low cost, high thermoelectric output and long life, and can work stably under an environment below 1500℃, and is suitable for temperature measurement in industrial high-temperature environments.
Smart Images

Figure CN119095464A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin film thermal sensor devices and relates to an oxide thin film thermocouple resistant to 1500°C and a preparation method thereof. Background Art
[0002] In the field of high temperature measurement, thermocouples, as a widely used temperature measurement sensor, play a vital role. Especially in industrial high temperature environments, thermocouples have become an indispensable tool due to their reliability and stability. In recent years, with the continuous advancement of industrial technology and the growing demand for applications, thin film thermocouples have emerged as a new type of sensing method. This sensor has significant advantages such as small size, fast response speed, and easy integration, and is very suitable for integration into various industrial equipment and process flows. Therefore, in high-tech and heavy industrial fields such as aerospace, steel metallurgy, energy and chemical industry, the market demand for thin film thermocouples is huge, and its application prospects are also very broad.
[0003] Traditional high-temperature thermocouple materials mainly rely on precious metals, such as platinum (Pt), rhodium (Rh), tungsten (W), rhenium (Re), etc. These materials show good chemical stability at high temperatures and have long been the mainstream choice. However, the application of precious metal materials also brings a series of problems, such as high cost, limited temperature measurement range, small thermoelectric output, and susceptibility to catalysis. These problems are particularly prominent in industrial applications and cannot meet the high requirements for high-temperature measurement accuracy, reliability, and economy. Therefore, the development of new high-temperature measurement materials and technologies has become a top priority.
[0004] In order to overcome the limitations of traditional thermocouple materials, researchers continue to explore and develop new high-temperature resistant oxide thin film thermocouples. This type of thermocouple is expected to achieve high accuracy and long life in high-temperature measurements, thus meeting the stringent requirements of industrial applications. At present, studies have shown that N-type semiconductor oxide indium tin oxide (ITO) exhibits good chemical and electrical stability in an air environment at 1500°C, making it an ideal high-temperature oxide thermocouple material. However, there are still many technical challenges to achieve the widespread application of high-temperature resistant oxide thin film thermocouples. Among them, one of the most critical issues is the development of P-type semiconductor oxide materials with high temperature resistance, high thermoelectric output, and relatively low cost. This is because, in order to prepare oxide thin film thermocouples with excellent performance, it is necessary to have both P-type and N-type semiconductor oxide materials with matching performance. In addition, it is also necessary to use advanced sputtering and other technical means to complete the precise preparation of oxide thin film thermocouples. The overcoming of this series of technical difficulties will have a profound impact on the development of high-temperature measurement technology.
[0005] In this context, the present application proposes an oxide thin film thermocouple that can withstand temperatures of 1500°C. By precisely controlling the content of specific elements in the solid solution, a P-type semiconductor oxide material with excellent high temperature resistance is prepared to solve the above technical problems. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide an oxide thin film thermocouple that can withstand 1500°C and a preparation method thereof. The thin film thermocouple has the characteristics of low cost, high output and long life, and can be used in high-temperature measurement environments below 1500°C to solve the problems of existing precious metal thin film thermocouples, such as high cost, limited temperature measurement range, small thermoelectric output and susceptibility to catalysis.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] An oxide thin film thermocouple resistant to 1500°C comprises a substrate and an N-type oxide electrode element and a P-type oxide electrode element arranged on the substrate, wherein the material of the N-type oxide electrode element is indium tin oxide, and the material of the P-type oxide electrode element is a solid solution of samarium, calcium and cobalt oxides.
[0009] Furthermore, the ends of the N-type oxide electrode element and the P-type oxide electrode element are staggered and connected to form a staggered point, and the other ends of the N-type oxide electrode element and the P-type oxide electrode element are respectively covered with metal pins.
[0010] Furthermore, the metal pin is made of temperature-resistant metal.
[0011] Furthermore, the temperature-resistant metal includes platinum and gold.
[0012] Furthermore, the mining of the substrate is a high temperature resistant electrically insulating substrate.
[0013] Furthermore, the high temperature resistant electrical insulating substrate includes sapphire, quartz and ceramic.
[0014] Furthermore, the mass ratio of indium oxide to tin oxide in the indium tin oxide is ≥9:1.
[0015] Furthermore, the atomic ratio of the samarium, calcium and cobalt oxide solid solution is as follows: cobalt accounts for 1 / 3 of the metal elements in the samarium, calcium and cobalt oxide solid solution; samarium and calcium account for 2 / 3, wherein calcium accounts for 4 / 15 to 1 / 3 of the metal elements in the samarium, calcium and cobalt oxide solid solution, and the rest is samarium, and the oxygen content does not exceed 4 times that of cobalt.
[0016] Furthermore, the atomic ratio of the samarium, calcium and cobalt oxide solid solution is that cobalt accounts for 2 / 5 of the metal elements in the samarium, calcium and cobalt oxide solid solution; the samarium and calcium account for 3 / 5, wherein the samarium accounts for 23 / 50 to 12 / 25 of the metal elements in the samarium, calcium and cobalt oxide solid solution, and the rest is calcium, and the oxygen content does not exceed 3 times that of cobalt.
[0017] On the other hand, the present invention also provides a method for preparing the oxide thin film thermocouple with a temperature resistance of 1500° C., characterized in that it comprises the following steps:
[0018] S1. A substrate for preparing an oxide thin film thermocouple using a high temperature resistant electrically insulating substrate;
[0019] S2. Using indium tin oxide as a target material for magnetron sputtering, patterning is performed on the substrate to form an N-type oxide electrode element;
[0020] S3. Using samarium, calcium and cobalt oxide solid solution as a target material for magnetron sputtering, patterning on the substrate to form a P-type oxide electrode element, and making the ends of the N-type oxide electrode element and the P-type oxide electrode element staggered to form an interlaced point;
[0021] S4. Use a temperature-resistant metal as a target material for magnetron sputtering and perform patterning on the substrate to form metal pins at the other ends of the N-type oxide electrode element and the P-type oxide electrode element, respectively.
[0022] Furthermore, the samarium, calcium and cobalt oxide solid solution is prepared by a sol-gel method, and the preparation method comprises the following steps:
[0023] Step 1. Weigh samarium oxide, calcium carbonate and cobalt according to a set atomic ratio, dissolve the weighed samarium oxide, calcium carbonate and cobalt in nitric acid to obtain a mixed solution, and then add glycerol to the mixed solution to form a gel;
[0024] Step 2: drying the gel to form powder, and calcining the powder at 700-1000° C. for 10 hours in an atmospheric environment;
[0025] Step 3. In an atmospheric environment, annealing the calcined product in step 2 at 1000° C. to 1500° C. for 100 to 150 hours, and rapidly cooling for 3 to 5 minutes to form a solid solution of samarium, calcium and cobalt oxides;
[0026] Step 4. Grind the solid solution of samarium, calcium and cobalt oxides and press them into blocks, and sinter them at 1500° C. for 15 hours in an atmospheric environment to prepare a solid solution target of samarium, calcium and cobalt oxides.
[0027] The beneficial effects of the present invention are:
[0028] The present invention provides a 1500°C resistant oxide thin film thermocouple using sapphire, quartz, ceramic and other materials as high temperature resistant electrical insulation substrates, indium tin oxide and samarium, calcium and cobalt oxide solid solutions as two electrode elements of the thin film thermocouple, platinum, gold and other heat resistant metals as metal pins, and by precisely controlling the content of elements such as samarium, calcium and cobalt in the oxide solid solution, a P-type semiconductor oxide material with excellent high temperature resistance is prepared, combined with N-type semiconductor oxide indium tin oxide, so as to realize the preparation of a new type of high temperature resistant oxide thin film thermocouple. After testing, the 1500°C resistant oxide thin film thermocouple prepared in this application has a temperature resistance of up to 1500°C, and the thermoelectric output under the working condition of 1500°C is about 200mV, and the service life exceeds 10 months.
[0029] Compared with the existing precious metal thin film thermocouples, the 1500°C resistant oxide thin film thermocouple of the present invention has the characteristics of low cost, high output and long life, and can well meet the temperature measurement requirements of high temperature environments of 1500°C and below, and has a wide range of application scenarios. The introduction of this technology will help promote the development of high temperature measurement technology and provide more efficient and reliable measurement methods for aerospace, steel metallurgy, energy and chemical industries.
[0030] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0032] Figure 1 This is a front axonometric schematic diagram of an oxide thin film thermocouple capable of withstanding 1500° C. in the present invention.
[0033] Reference numerals: substrate 1 , N-type oxide electrode element 21 , P-type oxide electrode element 22 , cross point 23 , metal pin 3 . DETAILED DESCRIPTION
[0034] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0035] Among them, the drawings are only used for illustrative explanations, and they only represent schematic diagrams rather than actual pictures, and should not be understood as limitations on the present invention. In order to better illustrate the embodiments of the present invention, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of actual products. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.
[0036] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right", "front", "rear", etc. indicate the orientation or position relationship, they are based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as limiting the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0037] See also Figure 1 , is an oxide thin film thermocouple resistant to 1500°C, comprising a substrate 1, an N-type oxide electrode element 21, a P-type oxide electrode element 22 and a metal pin 3, wherein the ends of the N-type oxide electrode element 21 and the P-type oxide electrode element 22 are connected to form a staggered point 23, and the ends of the other ends are respectively covered with a metal pin 3;
[0038] Specifically, in this embodiment, the material of the substrate 1 is a high-temperature resistant electrically insulating substrate such as sapphire, quartz, and ceramic, the material of the N-type oxide electrode element 21 is indium tin oxide (ITO), the material of the P-type oxide electrode element 22 is an oxide solid solution of samarium (Sm), calcium (Ca), and cobalt (Co), and the metal pin 3 is a heat-resistant metal such as platinum (Pt) and gold (Au) for lead interconnection.
[0039] The indium oxide (In2O 3) The mass ratio with tin oxide (SnO2) is ≥9:1.
[0040] The atomic ratio of the samarium (Sm), calcium (Ca) and cobalt (Co) oxide solid solution is as follows: cobalt (Co) accounts for 1 / 3, samarium (Sm) and calcium (Ca) account for 2 / 3, wherein calcium (Ca) accounts for 4 / 15 to 1 / 3 of the total metal elements, and the rest is samarium (Sm), and the content of oxygen (O) does not exceed 4 times that of cobalt (Co).
[0041] In another embodiment, the atomic ratio of the samarium (Sm), calcium (Ca) and cobalt (Co) oxide solid solution can be selected as follows: cobalt (Co) accounts for 2 / 5, samarium (Sm) and calcium (Ca) account for 3 / 5, among which samarium (Sm) accounts for 23 / 50 to 12 / 25 of the total metal elements, and the rest is calcium (Ca), and the content of oxygen (O) does not exceed 3 times that of cobalt (Co).
[0042] The solid solution of samarium (Sm), calcium (Ca) and cobalt (Co) oxides of the P-type oxide electrode element 22 is prepared by a sol-gel method, comprising the following steps:
[0043] 1) weighing samarium oxide (Sm2O3), calcium carbonate (CaCO3) and cobalt (Co) according to the above atomic ratio, dissolving the materials in nitric acid, and then adding glycerol to the mixed solution to form a gel;
[0044] 2) drying the gel to form powder, and calcining the powder at 700-1000° C. for 10 hours in an atmospheric environment;
[0045] 3) annealing the calcined product at 1000° C. to 1500° C. in an atmospheric environment for 100 to 150 hours, and rapidly cooling the product for 3 to 5 minutes to form a solid solution of samarium (Sm), calcium (Ca) and cobalt (Co) oxides.
[0046] 4) Grinding samarium (Sm), calcium (Ca) and cobalt (Co) oxide solid solution, adding a small amount of ethanol and pressing into blocks, sintering at 1500°C for 15 hours in an atmospheric environment, and then cooling with the furnace to make samarium (Sm), calcium (Ca) and cobalt (Co) oxide solid solution target.
[0047] The method for preparing the oxide thin film thermocouple with a temperature resistance of 1500°C comprises the following steps:
[0048] 1) Using sapphire as the substrate for preparing oxide thin film thermocouples, the substrate was subjected to standard RCA cleaning;
[0049] 2) using the target material of indium tin oxide (ITO) with the mass ratio to perform magnetron sputtering, and patterning the substrate using a hard mask technology to form an N-type oxide electrode element 21, and the thickness of the sputtered film is 500nm to 3μm;
[0050] Preferably, in order to enhance the temperature resistance, the total gas pressure in the sputtering chamber is controlled to be ≤10mTorr during the sputtering process, and the gas ratio is controlled to be 1 / 2 to 7 / 10 for nitrogen, 3 / 10 to 2 / 10 for oxygen, and 1 / 10 for argon.
[0051] 3) using the samarium (Sm), calcium (Ca) and cobalt (Co) oxide solid solution target material for magnetron sputtering, and patterning on the substrate using a hard mask technique to form a P-type oxide electrode element 22, with a sputtered film thickness of 500nm to 3μm;
[0052] 4) Use a target material such as platinum (Pt) or gold (Au) for magnetron sputtering and use hard mask technology for patterning to form a metal pin 3.
[0053] After testing, the 1500°C temperature-resistant oxide thin film thermocouple prepared in this embodiment has a temperature resistance of up to 1500°C, and a thermoelectric output of about 200mV under the working condition of 1500°C, and a service life of more than 10 months.
[0054] In other embodiments, the oxide thin film thermocouple can be processed by other surface patterning technologies besides the hard mask technology, such as thermal spray direct writing technology, screen printing technology, etc.; and the oxide thin film thermocouple can be used to prepare other high-temperature thermal sensing elements, including but not limited to temperature sensors, high-temperature heat flux meters, high-temperature radiometers, high-temperature thermal flow meters, etc.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. An oxide thin film thermocouple resistant to 1500°C, comprising a substrate and an N-type oxide electrode element and a P-type oxide electrode element arranged on the substrate, Features: The material of the N-type oxide electrode element is indium tin oxide, and the material of the P-type oxide electrode element is samarium, calcium and cobalt oxide solid solution.
2. The 1500°C resistant oxide thin film thermocouple according to claim 1, Features: The ends of the N-type oxide electrode element and the P-type oxide electrode element are staggered and connected to form a staggered point, and the other ends of the N-type oxide electrode element and the P-type oxide electrode element are respectively covered with metal pins.
3. The 1500°C resistant oxide thin film thermocouple according to claim 2, Features: The metal pin is made of heat-resistant metal.
4. The 1500°C resistant oxide thin film thermocouple according to claim 3, Features: The temperature-resistant metals include platinum and gold.
5. The 1500°C resistant oxide thin film thermocouple according to claim 1, Features: The base material is a high temperature resistant electrical insulating base material.
6. The 1500°C resistant oxide thin film thermocouple according to claim 5, Features: The high temperature resistant electrical insulating substrate includes sapphire, quartz and ceramic.
7. The 1500°C resistant oxide thin film thermocouple according to claim 1, Features: The mass ratio of indium oxide to tin oxide in the indium tin oxide is ≥9:
1.
8. The 1500°C resistant oxide thin film thermocouple according to claim 1, Features: The atomic ratio of the samarium, calcium and cobalt oxide solid solution is as follows: cobalt accounts for 1 / 3 of the metal elements in the samarium, calcium and cobalt oxide solid solution; samarium and calcium account for 2 / 3, wherein calcium accounts for 4 / 15 to 1 / 3 of the metal elements in the samarium, calcium and cobalt oxide solid solution, and the rest is samarium, and the oxygen content does not exceed 4 times that of cobalt.
9. The 1500°C resistant oxide thin film thermocouple according to claim 1, Features: The atomic ratio of the samarium, calcium and cobalt oxide solid solution is as follows: cobalt accounts for 2 / 5 of the metal elements in the samarium, calcium and cobalt oxide solid solution; samarium and calcium account for 3 / 5, wherein samarium accounts for 23 / 50 to 12 / 25 of the metal elements in the samarium, calcium and cobalt oxide solid solution, and the rest is calcium, and the oxygen content does not exceed 3 times that of cobalt.
10. A method for preparing the oxide thin film thermocouple with a temperature resistance of 1500°C as claimed in claim 8 or 9, It is characterized in that The steps include: Step 1. Prepare a substrate of an oxide thin film thermocouple using a high temperature resistant electrical insulating substrate, and perform standard RCA cleaning on the substrate; Step 2: Using indium tin oxide as a target material for magnetron sputtering, patterning the substrate using a hard mask technique to form an N-type oxide electrode element; Step 3. Using samarium, calcium and cobalt oxide solid solution as a target material for magnetron sputtering, patterning on the substrate using a hard mask technology to form a P-type oxide electrode element, and making the ends of the N-type oxide electrode element and the P-type oxide electrode element staggered and connected to form a staggered point; Step 4. Use a temperature-resistant metal as a target material to perform magnetron sputtering and perform patterning on the substrate to form metal pins at the other ends of the N-type oxide electrode element and the P-type oxide electrode element, respectively.
11. The preparation method according to claim 10, Features: The samarium, calcium and cobalt oxide solid solution is prepared by a sol-gel method, and the preparation method comprises the following steps: Step 1. Weigh samarium oxide, calcium carbonate and cobalt according to a set atomic ratio, dissolve the weighed samarium oxide, calcium carbonate and cobalt in nitric acid to obtain a mixed solution, and then add glycerol to the mixed solution to form a gel; Step 2: drying the gel to form powder, and calcining the powder at 700-1000° C. for 10 hours in an atmospheric environment; Step 3. In an atmospheric environment, annealing the calcined product in step 2 at 1000° C. to 1500° C. for 100 to 150 hours, and rapidly cooling for 3 to 5 minutes to form a solid solution of samarium, calcium and cobalt oxides; Step 4. Grind the solid solution of samarium, calcium and cobalt oxides and press them into blocks, and sinter them at 1500° C. for 15 hours in an atmospheric environment to prepare a solid solution target of samarium, calcium and cobalt oxides.