Conductive hollow metal particle and preparation method thereof
By removing core particles in hollow conductive metal particles and annealing to form a cavity structure, the problem of insufficient conductivity in the prior art is solved, better conductivity and contact area are achieved, and continuity during pressurization and Conductive properties.
Patent Information
- Application Number
- CN202380035093.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-06
- Filing Date
- 2023-05-05
- Publication Date
- 2024-12-06
AI Technical Summary
The existing hollow metal particles cannot provide sufficient contact area and conductivity stably, especially due to the inconsistent size caused by uneven particle size distribution, resulting in insufficient conductivity of the connected object.
Hollow conductive metal particles with soft properties are adopted, which have a metal layer on the surface and no fixed core particles inside. The cavity structure is formed through the kernel particle removal and annealing process to ensure that the metal layer continues to crack during pressurization and exists inside. The unfixed particles have a solid material inside to support deformation of the metal layer.
The contact area with the connected object is increased, conductivity is improved, and the continuity of the metal layer is maintained during pressurization, reducing resistance.
Smart Images

Figure CN119095681A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to conductive hollow metal particles and a preparation method thereof. Background Art
[0002] In the past, there were metal particles used for electrical connection of anisotropic conductive films, devices or substrates, for example, hollow metal particles. However, the existing hollow metal particles cannot stably provide a sufficient contact area for providing sufficient conductivity to a connection object such as a terminal. In addition, the existing hollow metal particles have a large particle size distribution. As shown above, the hollow metal particles with a large particle size distribution have uneven sizes, and only a part of the particles with larger sizes participate in the connection, which cannot provide a sufficient number of particles and contact area for participating in the connection. As a result, it is impossible to provide sufficient conductivity for the connection object. Summary of the invention
[0003] Problem that the invention aims to solve
[0004] The present invention aims to solve the above-mentioned problems of the prior art, and its purpose is to provide a conductive hollow metal particle with soft characteristics and a preparation method thereof, which can increase the contact area with the connection object and thus improve the conductivity.
[0005] Means used to solve problems
[0006] The hollow conductive metal particles of the present invention used to achieve the above-mentioned purpose are conductive hollow metal particles with soft characteristics, that is, they include a metal layer on the surface and have a hollow particle structure, the above-mentioned hollow particle structure does not have a fixed core particle near the inner side of the above-mentioned metal layer, and there is a cavity space near the inner side of the above-mentioned metal layer, and when the above-mentioned conductive metal particles are pressurized and deformed at a deformation rate of 20%, there is no broken or damaged part that causes discontinuity of the above-mentioned metal layer.
[0007] In one embodiment, the hollow conductive metal particles of the present invention are characterized in that when the above-mentioned conductive metal particles are pressurized and deformed at a deformation rate of 20% and are in a state without being broken or damaged to cause the above-mentioned metal layer to be discontinuous, the force applied to the above-mentioned conductive metal particles by the above-mentioned pressurization can be greater than 0.5mN and less than 20mN.
[0008] In one embodiment, the metal layer may contain at least one selected from the group consisting of copper, silver, gold, indium, nickel and alloys thereof.
[0009] In one embodiment, the hollow conductive metal particles of the present invention are characterized in that there is unfixed solid material inside the particles adjacent to the inner side of the above-mentioned metal layer, and the maximum particle size or length of the above-mentioned solid material inside the particles can be less than 90% of the maximum particle size of the above-mentioned conductive metal particles.
[0010] In one embodiment, the hollow conductive metal particles of the present invention are characterized in that there is unfixed solid material inside the particles adjacent to the inner side of the above-mentioned metal layer. When the above-mentioned conductive metal particles are pressurized and deformed at a deformation rate of 20%, the solid material inside the particles may not resist the deformation of the above-mentioned metal layer and exert a supporting force on the above-mentioned metal layer.
[0011] In one embodiment, the hollow conductive metal particle of the present invention is characterized by having unfixed solid material inside the particle adjacent to the inner side of the metal layer, and the solid material inside the particle may contain at least one of a polymer resin or a carbide of the polymer resin.
[0012] In one embodiment, the particle size of the hollow metal particles may be greater than 0.01 μm and less than 1,000 μm.
[0013] In one embodiment, the thickness of the metal layer may be greater than or equal to 0.002 μm and less than or equal to 50 μm.
[0014] In one embodiment, the metal layer may include: a first plating layer; and a second plating layer formed on the first plating layer and containing at least one selected from the group consisting of copper, silver, gold, indium, nickel and alloys thereof.
[0015] In addition, the preparation method of the hollow conductive metal particles of the present invention may include: a core particle removal process, heating the conductive metal particles coated with a metal layer on the core particles containing a polymer resin to completely or partially remove the above-mentioned core particles; and an annealing process, heating the above-mentioned conductive metal particles to a temperature equal to or higher than the heating temperature of the above-mentioned core particle removal process.
[0016] In one embodiment, the method for preparing hollow conductive metal particles of the present invention is characterized in that, before the core particle removal process, it may further include a metal coating forming process of covering the core particles containing the polymer resin with a metal layer to form a metal coating.
[0017] In one embodiment, the method for preparing the hollow conductive metal particles of the present invention is characterized in that, after the annealing process, it may further include a process of covering and forming an additional metal layer on the metal layer.
[0018] In one embodiment, the polymer resin may include at least one of polymethyl methacrylate resin, polyacrylonitrile, polystyrene resin, acrylonitrile-styrene-butadiene resin, vinyl resin, polycarbonate resin, polyacetal resin, polysulfone resin, polyphenylene ether resin, polyester resin, polyolefin resin and polyurethane resin.
[0019] In one embodiment, the shape of the core particles can be spherical, plate-like, fibrous or irregular.
[0020] In one embodiment, the coefficient of variation (CV) of the particle size distribution of the core particles calculated by the following formula 1 may be 40% or less.
[0021] Coefficient of variation (CV, %) = (particle size standard deviation / average particle size) × 100% - Formula 1
[0022] In one embodiment, the heating temperature in the core particle removal process may be set to a temperature equal to or higher than a thermal decomposition temperature, at which the polymer chains of the polymer resin of the core particles inside the conductive metal particles are broken due to heat, causing the resin to vaporize.
[0023] In one embodiment, during the core particle removal process, the vaporized resin may be discharged to the outside of the metal layer through the holes formed in the metal layer.
[0024] In one embodiment, after the core particle removal process, core material remains inside the metal layer, and the mass of the core material may be less than 90 mass % relative to the mass of the core particles before the core particle removal process.
[0025] In one embodiment, the heating temperature of the annealing process can be set within a temperature range that is equal to or higher than the temperature at which the recrystallization texture of the metal layer is formed and is equal to or lower than the annealing temperature at which the area ratio of the region where the metal layer exists on the entire surface area of the conductive metal particles after the annealing process reaches more than 80%.
[0026] In one embodiment, in the core particle removal process, the heating temperature may be set in a range of 250° C. to 600° C., and the heating time may be set in a range of 30 minutes to 3 hours.
[0027] In one embodiment, when the metal layer is a nickel-containing metal layer, the heating temperature of the annealing process may be set within a range of 600° C. to 800° C., and the heating time may be set within a range of 20 minutes to 3 hours.
[0028] Effects of the Invention
[0029] According to the present invention, hollow metal particles having flexible characteristics that can increase the contact area with a connection target object and improve electrical conductivity can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 and Figure 2 FIG. 1 is a diagram showing the deformed shape of the hollow metal particles having soft characteristics according to the present invention after being subjected to external pressure.
[0031] Figures 3 to 6 The figure shows the deformation shape of the hollow metal particles which have not been subjected to the softening process of the present invention after being subjected to external pressure.
[0032] Figure 7 A diagram showing a hollow metal particle in which the metal layer is broken while the core particle is not completely decomposed.
[0033] Figure 8 FIG. 1 is a diagram showing hollow metal particles annealed at a temperature exceeding the temperature range of the annealing process of the present invention.
[0034] Fig. 9 This is a diagram showing the deformed shape after the pressure is applied to a single hollow metal particle having soft characteristics of the present invention with a predetermined force.
[0035] Fig.10 The diagram shows the deformed shape after the pressurization when a predetermined force is applied to a single hollow metal particle that has not been subjected to the softening process of the present invention.
[0036] Fig.11 This is a graph showing the change in resistance under compression of the hollow conductive metal particles having flexibility of the present invention and the conventional conductive metal particles having core particles but not having flexibility. DETAILED DESCRIPTION
[0037] Hereinafter, the hollow conductive metal particles having soft characteristics and the preparation method thereof of the present invention will be described in more detail.
[0038] <Conductive Metal Particles>
[0039] The conductive metal particles of the present invention have a conductive layer including a metal layer, and all or part of the core particles used in the preparation process described below are removed from the inside of the conductive metal particles, thereby forming a hollow conductive metal particle having a cavity on the inner side adjacent to the conductive layer.
[0040] In the interior of the conductive metal particle of the present invention, all of the core particles used in the preparation process described below are removed, so that substantially no residual solid material exists in the conductive layer of the conductive metal particle.
[0041] Alternatively, in the conductive metal particles of the present invention, even after the thermal decomposition process in the core particle removal process and the annealing process of the present invention to be described below, a part of the material of the above-mentioned core particle and / or a part of the thermal decomposition product are not completely removed, and still remain in a solid state, these residual solid materials inside the particles can exist in the conductive metal particles in a state that does not support the conductive layer. That is, in the conductive metal particles of the present invention, when the conductive layer is pressed by a force applied from the outside of the conductive metal particles and the conductive metal particles are deformed at a predetermined deformation rate, the solid materials inside the particles can exist in the particles in a form that does not support the conductive layer in a direction that resists its deformation. Below, as described above, even after the thermal decomposition process in the core particle removal process and the annealing process of the present invention, a part of the material of the above-mentioned core particle and / or a part of the thermal decomposition product are not completely removed, and the material that still remains in a solid state inside the conductive metal particles is referred to as "solid materials inside the particles".
[0042] For example, in the case where the conductive metal particles are pressurized and deformed at a deformation rate of 20%, when the conductive layer is deformed, the solid material inside the particles may exist in the form of a support structure that does not exist inside the particles to support the conductive layer to resist its deformation. Here, the deformation rate can be measured as the length change rate of the particles before and after the particles are deformed in the compressive direction, and the deformation rate can be appropriately selected according to the connection environment of the applicable conductive metal particles. In other words, in the present invention, when there is solid material inside the particles inside the conductive metal particles, its maximum particle size or length can be equal to or less than a predetermined ratio of the maximum particle size of the conductive metal particles. Preferably, the maximum particle size or length of the solid material inside the particles can be less than 90% of the maximum particle size of the conductive metal particles, more preferably, less than 80%, less than 60%, less than 40%, less than 20%, less than 10%, less than 5%, less than 3%, less than 1%, less than 0.1%.
[0043] In addition, in the present invention, as the pyrolysis product of the material of the core particles, a small amount of carbon material formed after the carbonization of the core material may sometimes remain inside the conductive layer. The particles in this state also form a cavity on the inner side adjacent to the conductive layer, and the remaining carbon material only occupies a part of the inner space. Therefore, they also belong to the hollow conductive metal particles of the present invention.
[0044] In the conductive metal particles of the present invention, when the particle interior solid material exists, the particle interior solid material may have any shape, and may exist in a form freely moving inside the particle or in a form attached to a portion of the inside of the particle.
[0045] The metal layer of the present invention may include at least one selected from the group consisting of copper, silver, gold, indium, nickel and alloys thereof, and preferably, when considering the manufacturing cost, may be nickel or a nickel alloy.
[0046] The conductive metal particles of the present invention have a soft property so that the metal layer will not break or be damaged when being pressed by an external force within a predetermined range. Preferably, the conductive metal particles of the present invention have a soft property such that the force applied when the metal layer reaches a deformation rate of 20% without breaking or being damaged is 0.5 mN to 20 mN. Therefore, the conductive metal particles of the present invention can increase the contact area with the connection object, and the metal layer will not break or be damaged when being pressed by the conductive connection object. As a result, the resistance with the connection object can be reduced when electricity is applied.
[0047] The size of the conductive metal particles of the present invention is not particularly limited, and for example, the average particle size may be 0.01 μm or more and 1,000 μm or less, preferably 0.1 μm or more and 500 μm or less, and more preferably 0.5 μm or more and 300 μm or less. Alternatively, the size of the conductive metal particles of the present invention may be within the above range plus the thickness range of the conductive layer below.
[0048] In addition, the thickness of the conductive layer of the conductive metal particles of the present invention is not particularly limited, and preferably, it can be 0.002 μm or more and 50 μm or less, preferably, it can be 0.02 μm or more and 50 μm or less, more preferably, it can be 0.1 μm or more and 20 μm or less, or it can be 0.15 μm or more and 15 μm or less.
[0049] <Method for preparing conductive metal particles>
[0050] The method for preparing the conductive metal particles of the present invention includes a core particle removal process and an annealing process, and may also include a metal coating formation process and / or an additional coating formation process. Each process will be described in detail below.
[0051] <Metal coating formation process>
[0052] The metal coating forming process of the present invention is a process for forming a metal coating on core particles.
[0053] The core particles of the present invention form a metal coating on their surfaces through this process, and the core particles are completely or partially removed by performing a core particle removal process described below after this process, so that the metal coating still remains as the above-mentioned metal layer.
[0054] For this reason, the core particles of the present invention are preferably polymer resin particles containing a polymer resin, and as the above-mentioned polymer resin, a known existing polymer resin capable of thermal decomposition can be used. Preferably, the above-mentioned polymer resin can be polymethyl methacrylate resin, polyacrylonitrile, polystyrene resin, acrylonitrile-styrene-butadiene resin, vinyl resin, polycarbonate resin, polyacetal resin, polysulfone resin, polyphenylene ether resin, polyester resin, polyolefin resin (for example, polyethylene, polypropylene, polybutylene, etc.) or polyurethane resin, and they can be used alone or in combination.
[0055] The shape of the core particles of the present invention is not particularly limited, for example, it can be spherical, plate-like, fibrous or irregular, etc. In addition, as the core particles, hollow particles with cavities formed inside the particles can be used, or porous particles with multiple holes formed on the surface can be used, for example, hollow spherical particles, porous spherical particles, etc. can be used. However, in the present invention, the core particles are not limited thereto, and particles that do not have cavities inside or are not porous can be used.
[0056] The particle size distribution of the core particles of the present invention is not limited, but from the perspective of the size uniformity of the conductive metal particles, it is preferred to use particles with a narrower particle size distribution whose coefficient of variation (CV, Coefficient of variation) % value calculated by the following formula 1 is preferably 20% or less.
[0057] Coefficient of variation (CV, %) = (particle size standard deviation / average particle size) × 100% - Formula 1
[0058] In general, in the case of non-hollow particles, it is easier to prepare particles with a narrow particle size distribution. In the present invention, even if non-hollow core particles are used, hollow conductive metal particles can be prepared through the core removal process and annealing process to be described below, and as a result, hollow conductive metal particles with a narrow particle size distribution can be prepared more easily.
[0059] However, according to the present invention, due to the excellent softness, a good electrical connection can be provided to the object to be connected, so even if core particles with a wide particle size distribution are used, a good electrical connection with the object to be connected can be achieved due to the excellent softness. For example, even if core particles with a wide particle size distribution having a CV value of 33% or less, or even 40% or less, or 50% or less are used, the hollow conductive metal particles prepared according to the present invention can still achieve a good electrical connection with the object to be connected due to their excellent softness.
[0060] The size of the core particles of the present invention is not particularly limited, and for example, the average particle diameter may be 0.01 μm or more and 1,000 μm or less, preferably 0.1 μm or more and 500 μm or less, and more preferably 0.5 μm or more and 300 μm or less.
[0061] For applications of connection with electronic circuits and the like, spherical core particles having an average particle diameter of 0.5 μm or more and 1,000 μm or less are preferably used, and more preferably 1 μm or more and 300 μm or less are used.
[0062] In one embodiment, the metal coating may be formed on the surface of the core particle by a plating process, such as an electroless plating process. Alternatively, the metal coating may be formed on the surface of the core particle by a known coating process for forming a metal layer, such as an evaporation method, a sputtering method, etc.
[0063] When a plating process is used for coating metal, the metal coating formation process may include a known plating process, and may include a surface etching process (surface modification process) for removing particulate impurities and increasing surface roughness, a sensitization process for adsorbing ionic substances (Sn, etc.) with reducing power on the material surface as a process for forming catalyst nuclei (Pd, Ag, etc.) required for the initial precipitation of the electroless plating process, an activation process for the reduction reaction of gold plating by attaching catalyst nuclei, an acceleration process for improving reactivity, and the like, a surface treatment process required, a process for dissolving noble metal ions in a reactor and then putting them into a plating solution together with a reducing agent for plating, etc. In one embodiment, a process that does not use expensive noble metal ions may also be selected.
[0064] <Core Removal Process>
[0065] This process is a process of removing all or part of the core particles in the core particles formed with the metal coating by a thermal decomposition process, thereby preparing hollow metal particles with a metal layer. In the present invention, by removing all or part of the core particles, the deformation rebound resistance that may be generated by the core when external pressure is applied to the conductive metal particles can be eliminated or reduced. In the present invention, the hollow metal particles as the result of the core removal process refer to particles that form a cavity inside adjacent to the metal coating because the core particles supporting the metal coating are completely or partially removed by the core removal process. Not only are the core particles completely removed, but the entire interior of the metal coating forms a cavity. In addition, even if the core particles are partially removed, the material or thermal decomposition product of the core particles remains, which can eliminate or reduce the deformation rebound resistance when the cavity is formed inside adjacent to the metal coating. Therefore, the above particles are also called hollow metal particles. For example, even when the core particles are thermally decomposed due to the thermal decomposition process of the core particle removal process, as will be described below, and are gasified and discharged to the outside of the metal layer, there is a case where a small amount of carbon material formed by carbonizing the core material as a thermal decomposition product of the core particle material remains inside the metal coating, and the particles in this state still belong to the hollow conductive metal particles of the present invention.
[0066] In this process, as will be described below, in order to thermally decompose the core particles, the conductive metal particles are heated for a predetermined heating time at a predetermined heating temperature set according to the thermal decomposition temperature of the core particles. For example, in this process, the thermal decomposition process can be performed by using a furnace (Furnace) set with a heating temperature and a heating time set according to the thermal decomposition temperature of the core particles. At this time, in order to prevent the particles from agglomerating with each other during the heating process to the greatest extent, it is preferred to use a rotary type (Rotary type) or air floating type (Air floating type) furnace, etc.
[0067] In this process, heating is preferably performed in an inert gas atmosphere such as argon or nitrogen.
[0068] Generally, the behavior of polymer resins changes with temperature. Depending on the polymer characteristics, molecular weight and molecular structure of the polymer resin, the glass transition temperature (Tg) of the polymer varies. If crystals are present, the crystallization temperature (Tc) and melting point (Tm) vary. The thermal decomposition process in this process refers to a process in which the polymer resin is heated for a predetermined time at a temperature equal to or higher than the thermal behavior of the polymer resin, so that the polymer chains of the polymer resin are cut by heat, and the resin is vaporized by breaking the unit molecular weight, monomer and / or molecular unit, that is, thereby reducing the original weight of the polymer resin compared to before heating. That is, in the present invention, the thermal decomposition temperature of the polymer resin is the temperature at which the polymer resin is vaporized and reduced in weight by thermal decomposition due to heating, and the thermal decomposition temperature can be determined by measuring the weight change using a TGA (Thermal Gravity Analysis) device while heating the polymer resin. This thermal decomposition process is easier to achieve in thermoplastic resins, but is not limited to this. Even for thermosetting resins such as epoxy resins, polymer resins will also gasify after thermal decomposition, thereby reducing the original weight of the polymer resin compared to before heating. According to this process, the polymer resin of the core particles is gasified at a high temperature equal to or higher than the pyrolysis temperature due to the cutting of the polymer chain, and the resin on the surface of the core particles is gradually thermally decomposed, and the gas after thermal decomposition passes through the metal coating, so that the core particles are gradually reduced and / or removed. At this time, the gas can be discharged to the outside through the micropores formed in the metal coating, and these micropores that enable the gas to be discharged can exist at least in the core removal process. That is, when the coating is formed on the core particles in the metal coating forming process, there may be micropores or cracks in the metal coating, and through these micropores, the internal gas can be discharged to the outside of the particle in the thermal decomposition process. Or, due to the pressure caused by the internal gas generated in the thermal decomposition process, micropores can be formed at some locations of the metal coating formed in the metal coating forming process with a thinner thickness, so that the internal gas can be discharged to the outside of the particle. For this reason, in the metal coating formation process, it is preferred to form the metal coating with a thickness that allows internal gas generated by thermal decomposition in the core removal process to be discharged to the outside, that is, to form the metal coating with a thickness that has formed or can form micropores that allow internal gas to be discharged to the outside in the core removal process. Here, micropores refer to channels that allow internal gas to be discharged to the outside of the particles, and their shapes are not limited.
[0069] In this process, a small amount of carbonized carbon material as a product of thermal decomposition of the core material may remain inside the metal coating. Alternatively, in this process, some core particles may remain without thermal decomposition, so that a portion of the core material remains inside the metal layer.
[0070] The heating temperature of this process may vary depending on the type of polymer resin, as described above, as long as it is equal to or higher than the thermal decomposition temperature of the polymer resin at which the polymer chains constituting the core particles are cut due to heat and the resin is vaporized by breaking the unit molecular weight, monomer and / or molecular unit.
[0071] Generally speaking, polymer resin begins to thermally decompose at 250°C to 600°C, and the weight of the resin decreases due to thermal decomposition. Therefore, the heating temperature of the core particle removal process of the present invention is in the range of 250°C to 800°C, preferably, it can be in the range of 250°C to 600°C.
[0072] In the present invention, a TGA (thermogravimetric analyzer) is used to analyze the resin weight loss behavior of the polymer resin according to the heating temperature to measure the thermal decomposition temperature at which the polymer resin is gasified and the weight is reduced, and the heating temperature can be set to a temperature equal to or higher than the above-mentioned thermal decomposition temperature. For example, the heating temperature can be set as the X-axis value, and the weight of the conductive particles containing the core of the polymer resin can be set as the Y-axis value. In the weight change curve measured during the heating process, the location with the steepest slope is used as the thermal decomposition temperature reference value, and the heating temperature is set based on the reference value. For example, the above-mentioned reference value itself can be set as the heating temperature of the core removal process, or the heating temperature can be set within a predetermined range of variation above and below the above-mentioned reference value, such as, but not limited to, 80%, 70%, 50%, 30%, 10%, 5%, etc. of the reference value. In addition, when using TGA to measure weight change, the heating temperature rise rate can be set to any temperature per unit time, preferably, set to 100°C per minute, 50°C per minute, 30°C per minute, 15°C per minute, 5°C per minute, 3°C per minute, etc. for measurement.
[0073] In addition, in the present process, the temperature may be gradually increased before reaching the above-mentioned heating temperature. Thermal decomposition of the polymer resin at a low temperature requires a very long time, and thermal decomposition of the polymer resin at a high temperature may cause serious damage to the surface of the metal coating due to rapid generation of decomposition gas. Therefore, in the present process, it is preferred to gradually increase the temperature to the above-mentioned heating temperature to prevent damage to the metal coating.
[0074] In this process, the kernel is thermally decomposed and converted into gas, and the gas is discharged through the micropores formed in the metal coating. At this time, the surface of the kernel particles in contact with the metal coating first undergoes thermal decomposition, so that the density of the core particle surface decreases. In this process, as the heating time passes, the mass of the kernel gradually decreases, and finally hollow metal particles in which there is substantially no kernel inside the metal coating can be produced. However, as mentioned above, in the kernel removal process of the present invention, heating can be terminated under the state that a part of the kernel remains and a cavity is formed between the metal coating and the kernel. The kernel remaining as above can be further thermally decomposed in the annealing process described below.
[0075] If the heating temperature of this process is a high temperature that is too high than the thermal decomposition temperature of the polymer resin of the kernel, the thermal decomposition and gasification speed of the polymer resin are too fast, thereby the metal coating may be broken in the process in which the thermal decomposition gas is discharged to the outside of the metal coating. Alternatively, if the heating temperature of this process is too low or the heating time is too short, the thermal decomposition of the kernel is insufficient, and too much kernel material remains. As a result, in the process of being heated to a higher temperature in the annealing process described below, due to the rapid thermal decomposition of the kernel, the gas pressure in the metal layer may become too high, causing the metal coating to be destroyed. Therefore, in this process, it is preferred to set the heating temperature and time of the kernel particles so that the metal coating is not destroyed in the kernel removal process and the annealing process.
[0076] Although the core particles can be 100% thermally decomposed by this process, in the present invention, since the annealing process is subsequently performed in a higher heating temperature environment after the thermal decomposition of the core particles in this process, the core particles do not have to be 100% thermally decomposed. However, if there are too many thermal decomposition residues of the core particles in this process, it may cause rapid gasification and increase of gas pressure inside the metal layer due to the higher heating temperature environment in the subsequent annealing process, resulting in damage to the metal layer ( Figure 7 ), therefore, it is preferred that the mass ratio of the thermal decomposition residue of the core particles is equal to or lower than a predetermined range.
[0077] Therefore, the heating time of this process should at least last until the mass of the residual core material after the thermal decomposition of the core by this process is reduced, so as to prevent the metal coating from being damaged due to the rapid thermal decomposition of the residual core in the subsequent annealing process. To this end, the heating time of this process can at least last until the total mass of the core particles and their thermal decomposition products after this process relative to the mass of the core particles before this process is reduced to less than 90%, preferably reduced to less than 50%, more preferably reduced to less than 10%, less than 5%, less than 3%, and even more preferably reduced to less than 1%, less than 0.1%, less than 0.01%. The upper limit of the heating time of this process is not particularly limited, but if the core is thermally decomposed and discharged in a manner that meets the above-mentioned benchmark, there is no need to continue heating for a long time, so the upper limit of the heating time can be set within the range that meets the above-mentioned benchmark.
[0078] As described above, in the present process, by removing all or part of the core particles, the deformation rebound resistance that may be generated when the core particles exist in their original size can be removed or reduced.
[0079] In one embodiment, when polymethyl methacrylate (PMMA) resin is used as the polymer resin, the heating temperature is set to 250°C to 600°C, preferably to 380°C to 500°C, and the heating time is set to 30 minutes to 3 hours, thereby completely or partially removing the core particles by thermally decomposing the core particles.
[0080] Through this process, the conductive metal particles become hollow conductive metal particles in which all or part of the core particles configured to support the metal layer inside do not exist inside the conductive metal particles.
[0081] <Annealing process>
[0082] This process is a process for preparing the hollow conductive metal particles with soft properties of the present invention by annealing the hollow metal particles prepared by the core removal process. The purpose of the annealing process is to reduce the hardness and strength of the metal by stabilizing the stress and structure of the metal coating, thereby improving the formability. In the present invention, by annealing the hollow metal particles prepared in the core removal process, not only the metal structure is stabilized, but also the formable hollow metal particles with soft properties are prepared.
[0083] For this reason, in the present process, the conductive metal particles are heated at a heating temperature in a range equal to or higher than the heating temperature of the core removal process and equal to or lower than the melting point of the metal layer.
[0084] In this process, heating is preferably performed in an inert gas atmosphere such as argon or nitrogen.
[0085] In the present invention, the heating temperature for annealing the metal can be set according to the material of the metal layer. According to one embodiment of the present invention, when the metal layer is nickel, it is known that after the heat treatment process, a recrystallized structure is formed at a recrystallization temperature of about 600°C and a collective structure is formed at 680°C (Journal of Heat Treatment Engineering, Vol. 21, No. 3, 2008).
[0086] In the present invention, the hardness is reduced by forming a recrystallized structure of the nickel metal layer, thereby obtaining the ductility characteristics of the nickel metal layer.
[0087] In the present invention, when the heating temperature of the hollow nickel particles in the annealing process is 600°C or more and less than 850°C, hollow nickel particles with soft properties can be prepared. More preferably, when the heating temperature of the annealing process is 625°C or more, 650°C or more and 750°C or less, 725°C or less, hollow nickel particles with stable soft properties can be prepared. When annealing is performed at a heating temperature lower than 600°C, the soft properties are reduced, so more hollow nickel particles are broken during pressurization. Therefore, it is preferred to perform annealing at a temperature of 600°C or more, which is a temperature at which a recrystallized structure is formed. Figures 3 to 6 The figure shows the particle shape of hollow nickel particles prepared by annealing at a heating temperature below 600°C after pressurization. As shown in the figure, the effect of the soft property is very poor, so the particles do not show ductile deformation under the action of external force, but appear in a broken shape. On the other hand, Figure 8 This is a diagram showing the shape of nickel particles prepared by annealing at a heating temperature of 850°C or higher. At a heating temperature of 850°C or higher, self-deformation occurs sequentially from the fragile portion due to the deviation in the thickness of the metal layer, so that the continuity of the surface is interrupted, and the shape in which the continuity of the nickel metal layer is severely damaged appears in the remaining area except for the thick surface area of the agglomeration. These conductive particles with severely damaged continuity will cause a significant increase in the contact resistance with the object to be connected. Therefore, in this process, it is preferable to set the heating temperature of the annealed hollow nickel particles to be lower than 850°C.
[0088] As described above, the heating temperature of the annealing process of the present invention is preferably set within a range of above the temperature at which the recrystallized structure of the metal layer is formed and below the temperature at which the continuity of the metal layer is not damaged after the annealing process. In the present invention, not damaging the continuity of the metal layer means that the area where the metal layer exists accounts for 80% or more of the total surface area of the conductive metal particles, preferably 90% or more, 95% or more, and more preferably 99% or more, 99.9% or more.
[0089] In addition, the heating time of the annealing process of the present invention is preferably set within a range of heating time that forms a recrystallized structure of the metal layer when heated within the above-mentioned heating temperature range and within a range of heating time that does not damage the continuity of the metal layer after the annealing process.
[0090] In one embodiment, when polymethyl methacrylate (PMMA) resin is used as the polymer resin and the metal coating is a nickel-containing metal layer, the metal layer is made soft by an annealing process at a heating temperature of 600°C to 800°C and a heating time of 20 minutes to 3 hours, preferably, a heating time of 30 minutes to 1 hour.
[0091] According to this process, the metal layer undergoes crystal changes that improve its ductility and electrical conductivity.
[0092] In addition, when the metal coating is formed in the metal coating forming process, impurities may be included. According to the present process, these impurities are decomposed and removed, so that the metal content of the metal layer is increased to improve the conductive properties. For example, when a nickel metal layer is covered by electroless plating, impurities other than the conductive metal contained in the reducing agent (sodium hypophosphite, dimethyldiamine boron, sodium borohydride, etc.) and the sensitizer (tin chloride, etc.) during the electroless plating process will damage the conductive properties of pure nickel, and these impurities can be decomposed and removed by the annealing process, so that the metal content of pure nickel is increased, and finally the conductive properties are improved.
[0093] In addition, according to the present process, even if core materials and / or thermal decomposition products remain inside the metal layer after the core removal process, they can be further decomposed and / or burned.
[0094] In addition, in the present invention, the conductive metal particles have a soft property through the annealing process, so that the above-mentioned metal layer will not be broken or damaged when being squeezed by an external force within a predetermined range, preferably, the conductive metal particles have a soft property of 0.5mN to 20mN when the above-mentioned metal layer reaches a deformation rate of 20% without being broken or damaged. Therefore, the conductive metal particles of the present invention can increase the contact area with the connection object, and the metal layer will not be broken or damaged when being pressed by the conductive connection object, and as a result, when electricity is applied, the resistance with the connection object can be reduced.
[0095] The thickness of the conductive layer of the conductive metal particles of the present invention is not particularly limited, and may preferably be 0.002 μm to 50 μm, preferably 0.02 μm to 50 μm, more preferably 0.1 μm to 20 μm, or 0.15 μm to 15 μm.
[0096] When the hollow conductive metal particles with soft properties of the present invention are placed between connection objects and pressurized and / or heated, the particles can deform without breaking or being damaged, and can deform freely to adapt to the surface properties and shape of the connection objects. Figure 1 and Figure 2 As shown, the hollow conductive metal particles with soft properties of the present invention can be deformed without destroying the particles. Therefore, according to the conductive metal particles of the present invention, the contact area and / or the number of contact points with the connection object can be increased, and as a result, the contact resistance between the conductive metal particles and the connection object can be reduced, thereby improving conductivity.
[0097] <Additional coating formation process>
[0098] In one embodiment, the present invention may further include an additional coating formation process of forming an additional conductive layer on the above-mentioned metal layer to enhance the elasticity, resilience and / or support force of the metal layer of the above-mentioned conductive metal particles.
[0099] In one embodiment, the conductive layer can be further thickened by additionally covering a metal layer of the same material as the already formed metal layer, thereby improving the elasticity of the conductive layer and reducing the resistance. Alternatively, a metal layer such as copper, silver, gold or indium, which is inherently soft, can be additionally covered on the already formed metal layer to improve the elasticity, deformability, conductivity and other properties of the conductive layer.
[0100] In one embodiment, the additional metal coating can be formed on the surface of the conductive metal particles by a plating process, for example, the additional metal coating can be formed by an electroless plating process. Alternatively, the coating can also be formed on the surface of the core particles by a known coating process for forming a conductive layer, for example, an evaporation method, a sputtering method, etc. can be used.
[0101] According to the present invention, a metal coating having functions such as conductivity and / or electron shielding is formed on core particles having various shapes and various compositions, and then a hollow conductive metal having soft characteristics can be prepared through a decomposition and annealing process of the core. According to the present invention, when the conductive metal particles are interposed between connection objects, the contact area with the connection object can be increased, and as a result, the contact resistance can be reduced, and the conductivity can be improved.
[0102] Since the conductive metal particles prepared according to the present invention are hollow metal particles with soft characteristics, their shape changes according to the pressurized surface during use. Therefore, when the conductive metal particles of the present invention are used as conductive materials in the form of anisotropic conductive films, heat-sealed connectors, or upper and lower adhesive tapes, even if there are some particles of larger size in the particles, the particles deform without breaking when under pressure, and are compressed to a size equivalent to the distance between the terminals, the thickness of the film or the coating to deform. Therefore, when the conductive metal particles of the present invention are used, the contact area of the pressed part is increased, the contact resistance characteristics are improved, and the protruding shape of the large particles is eliminated, so that a large number of particles participate in the connection between the terminals, resulting in good connection conductivity, so that a product with a film or coating with low surface roughness can be obtained.
[0103] The hollow conductive metal particles with soft properties of the present invention can be used to conduct electricity by contacting with a connection object, for example, suitable for use as anisotropic conductive film (ACF), heat-sealed connectors, display panels or other conductive materials for connecting circuit boards connected to electrodes of conductive materials, etc.
[0104] Example
[0105] Hereinafter, the process for preparing hollow conductive metal particles having ductility characteristics of the present invention will be described in more detail by way of examples. However, the scope of the present invention is not limited to the following examples.
[0106] [Example 1]
[0107] The electroless plating adopts the following pretreatment and electroless plating process, and the core particles used are PMMA 20 μm spherical particles with a narrow particle size distribution and a CV% value of the particle size distribution of less than 20%.
[0108] Electroless plating pre-treatment process
[0109] As a pretreatment for electroless plating, an etching process (surface modification process) (PT01-01, Pretreatment 01-01 process) is performed to remove impurities and give surface roughness. According to the conditions of the polymer resin particle powder preparation process, impurities exist in the particle powder, and these impurities must be removed in order to obtain uniform plating quality. For this purpose, impurities can be removed by using MEK aqueous solution, sodium hydroxide aqueous solution, ethanol aqueous solution, hydrochloric acid, sulfuric acid aqueous solution, chromic acid aqueous solution, etc., and different chemical substances can be used or mixed according to the state of the core powder.
[0110] In Example 1, 4 g of PMMA powder was washed 2 to 3 times with an 80% ethanol aqueous solution and physically filtered to remove impurities.
[0111] Next, a process of increasing the surface roughness is performed to ensure that the coating adheres evenly to the particle surface. As a process of increasing the roughness, 7 g of potassium permanganate (KMnO4) is dissolved in 100 ml of 80°C distilled water, followed by dissolving 6 g of sodium hydroxide (NaOH), adding PMMA powder, and stirring the mixture for 10 minutes. It is then washed several times with distilled water and filtered through filter paper to increase the surface roughness, thereby obtaining a PMMA powder for the core with a rough surface that subsequently allows nickel to be easily reduced and attached.
[0112] After that, the PMMA powder was stirred in 100 ml of 2% ammonium hydroxide (NH4OH) aqueous solution for 10 minutes, then washed several times with distilled water and filtered through filter paper to neutralize the fine and rough surface of the core powder, and then washed several times and filtered to obtain a neutralized core powder with a pH of 5 to 6. (PT01-2 process)
[0113] Then 2g of tin chloride (SnCl2) was dissolved in 100ml of distilled water at 50°C, and the core powder with increased roughness and enhanced adhesion after the previous pretreatment was stirred for 10 minutes, then washed several times with distilled water, physically filtered, and subjected to an activation process to increase activity (PT02-01 process) so that a chemical plating reaction occurred smoothly on its surface.
[0114] The activated core powder is dissolved in 100 ml of distilled water at 55°C, in which 0.1 g of palladium chloride (PdCl2) is dissolved, and stirred for 10 minutes to form palladium (Pd, Palladium) particles on the surface of the core powder. (PT02-02 process)
[0115] Then, in order to activate the reaction of the Pd fine particles generated on the surface of the core powder, 10% hydrochloric acid (HCl) was added to 100 ml of distilled water at 50° C., the core powder was added, stirred for 10 minutes, washed with distilled water several times, and physically filtered to prepare a powder (PT02-03) with a Pd catalyst attached to the surface. Thus, all pretreatments of the core powder were completed.
[0116] Electroless plating process
[0117] In the present invention, in order to form a coating on the surface of the core powder that has been surface-treated in the above-mentioned pretreatment process, nickel chloride or nickel sulfide can be used, and as a reducing agent, aqueous solutions of sodium hypophosphite, dimethylamine boron (DMAB), dimethylamine borane, hydrazine, etc. can be used, or two or more of them can be mixed and used.
[0118] In addition, in the plating process of the present invention, stabilizers and dispersants can be used to carry out effective electroless nickel plating deposition. There is no particular restriction on this, but for example, nonionic, cationic, water-soluble polymer materials can be used. As nonionic surfactants, polyoxyalkyl ether compounds such as polyethylene glycol, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, etc. can be used. As cationic surfactants, betaine surfactants such as alkyl dimethyl acetate betaine, alkyl dimethyl carboxymethyl acetate betaine, alkyl dimethyl amino acetate betaine can be used. As water-soluble polymers, polyvinyl alcohol, polyvinyl pyrrolidone, hydroxyethyl cellulose, etc. can be used. In addition, compounds of group IV elements (i.e., selenium, thiourea, thiocyanate, etc.), unsaturated organic acids (i.e., maleic acid, itaconic acid, etc.), oxygen-containing anions (i.e., molybdate anions, etc.), hexadecyl trimethyl ammonium bromide (CTAB), etc. can also be used. As the complexing agent, citrates, glycolic acid, succinic acid, malic acid, gluconic acid, sodium acetate, sodium citrate, glycine, etc. can be used, and two or more of these can be used in combination.
[0119] In Example 1, the chemical substances exemplified above were selectively used to carry out an electroless reduction reaction as follows.
[0120] In this embodiment, in order to improve the dispersibility before entering the electroless reduction reaction, the core powder pretreated by the above-mentioned plating pretreatment process (PT01-01 to PT02-3) is placed in 100 ml of distilled water at 70°C to 75°C, 0.01 g of PVP and 0.01 g of CTAB are added, and stirred for 20 minutes to prepare a pretreated core powder solution.
[0121] Then, a solution of 1 mol of nickel sulfide and 1 mol of glycine was prepared in a 100 ml beaker, and 2 mol of sodium hypophosphite and 1 mol of hydrazine as a reducing agent and 1 mol of sodium hydroxide as a pH adjuster were separately prepared in a 100 ml beaker.
[0122] The prepared Ni aqueous solution and reducing solution were added in small amounts by a micro-rotary metering pump to a 100 ml core powder solution maintained at 70° C. to 75° C. and pre-treated while stirring the solution. In this embodiment, the addition was performed for 30 to 60 minutes and the reaction was performed for 90 to 120 minutes to induce Ni to stably adhere to the core powder to form a core, thereby achieving plating.
[0123] The conductive metal powder thus produced was washed several times with distilled water, physically filtered and dried, and finally conductive metal particles having a nickel plating layer of 0.200 μm to 0.450 μm were prepared.
[0124] Core Removal Process
[0125] The thermal decomposition process must be set differently according to the thermal decomposition behavior of the polymer resin. In this embodiment, the PMMA particles used are heated from room temperature, i.e., about 25°C, to 450°C in a nitrogen environment in a furnace equipped with a quartz tube that can create a N2 gas environment and can enter and exit the gas. After a 2-hour heating process and a 1-hour high-temperature thermal decomposition process, the core decomposes and becomes a gas, which escapes through the pores on the surface of the coating. The surface part of the core particles in contact with the coating is first decomposed, and the core resin in the nickel metal layer is substantially absent, thereby preparing hollow conductive metal particles plated with a nickel layer. The heating rate can be set to a final 2 minutes / °C to 15 minutes / °C, but in this embodiment, the heating rate is set to 3 minutes / °C to 5°C / minute. According to the performance and capacity of the furnace equipment, the heating rate conditions can be changed so that the coating surface is not seriously damaged.
[0126] Annealing process
[0127] After preparing the above hollow conductive metal particles, annealing is performed from 450°C to 725°C in the previously used furnace, heating for 30 minutes, holding for 30 minutes, annealing in a N2 atmosphere for a total of 1 hour, and then slowly and fully cooled in a N2 atmosphere, thereby preparing hollow nickel metal particles with soft characteristics. The heating rate can be set to a final 5 minutes / °C to 20 minutes / °C, but in this embodiment, the heating rate is set to 5 minutes / °C to 10°C / minute. Depending on the performance of the equipment, it may be extended for several hours to ensure sufficient annealing.
[0128] [Example 2]
[0129] The temperature of the annealing process in the process of Example 1 is set to 750° C., and annealing is performed in a N 2 atmosphere under the same heating and holding conditions as above, and the mixture is slowly and fully cooled in the N 2 atmosphere to prepare hollow nickel metal particles having soft characteristics.
[0130] [Example 3]
[0131] In order to increase the thickness of the plated layer in the process of Example 1, the annealing process is the same as that of Example 1, and Ag as a soft metal is additionally plated, thereby preparing hollow nickel / silver multilayer metal particles having soft characteristics.
[0132] [Example 4]
[0133] In order to increase the thickness of the plated layer in the process of Example 1, the annealing process is the same as that of Example 1, and Au as a soft metal is additionally plated, thereby preparing hollow nickel / gold multilayer metal particles with soft characteristics.
[0134] [Example 5]
[0135] In Example 5, about 1.5 g of hollow polyacrylonitrile (PAN) powder having a tap density (ASTM B527) of 0.2 g / cc to 0.4 g / cc was stirred with an 80% ethanol aqueous solution at 65°C for 50 minutes, washed 2 to 3 times with distilled water, and impurities were removed by physical filtration. Then, 6 g of sodium hydroxide (NaOH) was dissolved in 100 ml of distilled water, and the treated core powder was added and stirred for 10 to 30 minutes. After that, it was washed several times with distilled water and filtered with filter paper to enhance the adhesion so that the nickel on the surface can be smoothly reduced and attached. For PAN powder, a separate process such as surface etching using a strong solvent can be used to plate the surface, so this process is omitted.
[0136] Then, the above powder was added to 100 ml of distilled water at 60°C, and mixed with 2 g of stannous chloride (SnCl2), 50 ml of distilled water and 50 ml of 20% hydrochloric acid solution to make 100 ml of a mixed solution. After stirring for 60 minutes, the solution was washed several times with distilled water and physically filtered. The surface was activated to increase the activity, making it easy for chemical plating to occur.
[0137] In this example, the PAN powder subjected to the above pretreatment was added to 100 ml of distilled water at 70° C. to 75° C., and 0.01 g of PVP and 0.01 g of CTAB were added, followed by stirring for 20 minutes.
[0138] Then, a solution of 1 mol of nickel sulfide and 1 mol of glycine was prepared in a 100 ml beaker, and 2 mol of sodium hypophosphite and 1 mol of hydrazine as a reducing agent and 1 mol of sodium hydroxide as a pH adjuster were separately prepared in a 100 ml beaker.
[0139] The Ni salt aqueous solution prepared in this manner is induced to stably adhere and form nuclei, thereby achieving plating.
[0140] The conductive metal powder prepared as above was washed several times with distilled water, physically filtered and dried, and finally hollow conductive metal particles having a nickel plating layer of 0.200 μm to 2 μm and a nickel plating content of about 80% with PAN resin present inside were prepared. The hollow conductive particles prepared at this time have a hollow core, so the thermal decomposition time can be reduced, however, in order to compare the difference depending on the annealing process performed next, the thermal decomposition conditions were made the same.
[0141] After the conductive metal particles thus obtained are subjected to the core decomposition process of Example 1, the temperature of the annealing process of Example 1 is set to 650°C, the heating and holding conditions are the same as above, annealing is performed in a N2 atmosphere, and slow and sufficient cooling is performed in a N2 atmosphere to prepare hollow nickel metal particles with soft properties.
[0142] [Comparative Example 1]
[0143] Hollow nickel conductive particles without soft properties were prepared by performing only the core removal process in Example 1 without performing the annealing process.
[0144] [Comparative Example 2]
[0145] The temperature of the annealing process in the process of Example 1 was set to 550° C., and annealing was performed in a N 2 atmosphere under the same heating and holding conditions as above, and cooling was performed in the N 2 atmosphere to prepare hollow nickel conductive particles having soft characteristics.
[0146] In Comparative Example 2, the annealing temperature is lower than 600°C, and the softness effect is very low. Figures 3 to 6 As shown, when subjected to external force, the particles did not extend and deform but showed a broken shape. In Comparative Example 2, the particles were broken due to external force, resulting in a decrease in conductive properties and an increase in resistance.
[0147] [Comparative Example 3]
[0148] The temperature of the annealing process in the process of Comparative Example 1 was set to 850° C., and annealing was performed in a N 2 atmosphere under the same heating and holding conditions as above, and the particles were slowly and sufficiently cooled in the N 2 atmosphere to prepare hollow nickel conductive particles having soft characteristics.
[0149] When the annealing process temperature is above 850℃, due to the thickness deviation of the metal layer, self-deformation occurs from the weak part, and the surface continuity is interrupted ( Figure 8 ), so only the thicker nickel surface condenses and remains, and the remaining weak parts do not exist on the surface and become holes, showing the shape of serious damage or aggregation of the plating. These severely damaged conductive particles show a significant increase in resistance.
[0150] [Comparative Example 4]
[0151] The annealing process temperature was set to 550°C, annealing was performed in a N2 atmosphere under the same heating and holding conditions as described above, and cooling was performed in a N2 atmosphere to prepare hollow nickel conductive particles having soft properties, similar to the process of Example 5. Similar to Comparative Example 2, the particles were broken due to external force, resulting in a decrease in conductive properties and an increase in resistance.
[0152] Table 1
[0153]
[0154]
[0155] The resistance value (mΩ) is measured using a powder resistance analyzer made according to ASTM D991. 6g of conductive particles (adjusted according to density) are placed in the measuring instrument, a load of 10kgf is applied, and the value is measured after 1 minute of stabilization. In addition, SEM photos are used to confirm whether the particles are broken after pressure is applied.
[0156] As for the breaking strength, the microhardness tester of FISCHERSCOPE HM2000 was used for measurement, the measuring temperature was 25°C, and the measuring speed was 0.33 mN / sec. The force required was measured at the length of 10%, 20%, and 30% deformation of the entire particle size, and the embodiment and the comparative example were compared. Preferably, the force applied at 20% deformation rate is 0.5 mN to 20 mN or less, and particularly 1 mN to 15 mN or less.
[0157] The Comprehensive Assessment (CA) in Table 2 below based on the above characteristic values is a combination of the measured values of the three factors of electrical resistance, softness, and crushing after pressurization that are mainly considered in the characteristics of the conductive hollow metal particles, and quantified into a single value. This is to facilitate the comprehensive characteristic evaluation of products that need to meet multiple benchmark values at the same time and to form a single value. Its definition is as follows.
[0158] CA (comprehensive assessment) = (resistance characteristics) × weight 1 + (flexibility characteristics) × weight 2 + (no breakage after pressure) × weight 3 - formula 2
[0159] Referring to Table 2 below, in Formula 2, in order to facilitate the evaluation of the performance shown by each measurement value shown in the comparative example and the embodiment, it is divided into three levels: excellent, general, and poor, which are scored as 5 points, 3 points, and 1 point respectively. The weight of each factor is set according to the importance so that the performance can be judged by increasing the performance difference. In Table 2 below, the weight 1 and weight 3 of the required resistance characteristics and whether it is broken after pressure are set to 3 points respectively, and the weight 2 representing the softness characteristic of the force at a deformation rate of 20% is set to 5 points, which is a higher weight.
[0160] Table 2
[0161]
[0162]
[0163] As can be seen from Table 1 and Table 2, the hollow conductive metal particles according to Examples 1 to 5 of the present invention all have excellent performance in terms of resistance, softness, and crushing performance after pressurization.
[0164] Fig. 9 and Fig.10 This is a photograph of a conductive metal particle after compression when it was repeatedly pressed 5 times with a pressure of 3 mN using a Shimadzu MCT-510(E) model micro-compression testing machine.
[0165] Fig. 9 The hollow conductive metal particles with soft properties prepared in Example 1 are as follows Fig. 9 As shown in the photo, it deforms smoothly when pressurized, and the number of contact points and contact area with the pressurized object on the upper surface increase. Fig.10 The conductive metal particles prepared in Comparative Example 1 are shown. Fig.10 As shown in the photo, it is not easy to deform when pressure is applied, so the number of contact points and contact area with the pressurized object remain essentially unchanged.
[0166] Fig.11 The figure shows a comparison of the resistance change caused by compression between the hollow conductive metal particles having soft characteristics prepared in Example 1 and the conventional conductive metal particles having a core. Fig.11 As shown, compared with the existing conductive metal particles with a core, the hollow conductive metal particles according to the present invention have improved softness, the number of contact points and the contact area with the object to which the external force is applied are increased, the conductivity is improved, and there is a favorable effect that less force is required for compression deformation.
Claims
1. A hollow conductive metal particle with soft properties, It is characterized in that The surface includes a metal layer, and having a hollow particle structure, wherein the hollow particle structure has no fixed core particles near the inner side of the metal layer, and a cavity space exists near the inner side of the metal layer, When the conductive metal particles are pressurized and deformed at a deformation rate of 20%, there are no broken or damaged portions causing discontinuity of the metal layer.
2. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that When the conductive metal particles are pressed to deform at a deformation rate of 20% without being broken or damaged to cause discontinuity of the metal layer, the force applied to the conductive metal particles by the pressing is 0.5 mN to 20 mN.
3. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that The metal layer contains at least one selected from the group consisting of copper, silver, gold, indium, nickel and alloys thereof.
4. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that There is unfixed solid material inside the particles adjacent to the inner side of the metal layer, and the maximum particle size or length of the solid material inside the particles is less than 90% of the maximum particle size of the conductive metal particles.
5. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that There is unfixed solid material inside the particles adjacent to the inner side of the metal layer. When the conductive metal particles are pressurized and deformed at a deformation rate of 20%, the solid material inside the particles does not resist the deformation of the metal layer and exerts a supporting force on the metal layer.
6. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that There is an unfixed solid material inside the particle adjacent to the inner side of the metal layer, and the solid material inside the particle contains at least one of a polymer resin or a carbide of the polymer resin.
7. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that The particle diameter of the hollow metal particles is 0.01 μm or more and 1000 μm or less.
8. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that The thickness of the metal layer is not less than 0.002 μm and not more than 50 μm.
9. The hollow conductive metal particles having soft properties according to claim 1, It is characterized in that The above metal layer includes: first coating; and The second plating layer is formed on the first plating layer and contains at least one selected from the group consisting of copper, silver, gold, indium, nickel and alloys thereof.
10. A method for preparing hollow conductive metal particles, which is a method for preparing the hollow conductive metal particles according to any one of claims 1 to 9, wherein the method for preparing the hollow conductive metal particles is characterized in that: include: a core particle removal process, heating the conductive metal particles coated with a metal layer on the core particles containing the polymer resin to completely or partially remove the core particles; and The annealing process heats the conductive metal particles to a temperature equal to or higher than the heating temperature of the core particle removal process.
11. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that Before the core particle removal process, a metal coating forming process is further included in which a metal layer is covered on the core particles containing the polymer resin to form a metal coating.
12. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that After the annealing process, the method further includes a process of covering and forming an additional metal layer on the metal layer.
13. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that The polymer resin includes at least one of polymethyl methacrylate resin, polyacrylonitrile, polystyrene resin, acrylonitrile-styrene-butadiene resin, vinyl resin, polycarbonate resin, polyacetal resin, polysulfone resin, polyphenylene ether resin, polyester resin, polyolefin resin and polyurethane resin.
14. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that The shape of the core particles is spherical, plate-like, fibrous or irregular.
15. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that The coefficient of variation (CV) of the particle size distribution of the core particles calculated by the following formula 1 is 40% or less: Coefficient of variation (CV, %) = (particle size standard deviation / average particle size) × 100% - Formula 1 16. The method for preparing hollow conductive metal particles according to claim 10, It is characterized in that The heating temperature in the core particle removal process is set to a temperature equal to or higher than a thermal decomposition temperature at which polymer chains of the polymer resin of the core particles inside the conductive metal particles are broken by heat, causing the resin to gasify.
17. The method for preparing the hollow conductive metal particles according to claim 16, It is characterized in that In the core particle removal process, the vaporized resin is discharged to the outside of the metal layer through the holes formed in the metal layer.
18. The method for preparing hollow conductive metal particles according to claim 10, It is characterized in that After the core particle removal process, core material remains inside the metal layer, and the mass of the core material is less than 90 mass % relative to the mass of the core particles before the core particle removal process.
19. The method for preparing the hollow conductive metal particles according to claim 10, It is characterized in that The heating temperature of the annealing process is set within a temperature range equal to or higher than the temperature at which the recrystallized texture of the metal layer is formed and equal to or lower than the annealing temperature at which the area ratio of the region where the metal layer exists on the entire surface area of the conductive metal particles after the annealing process reaches 80% or more.
20. The method for preparing hollow conductive metal particles according to claim 10, It is characterized in that In the above core particle removal process, the heating temperature is set in the range of 250° C. to 600° C., and the heating time is set in the range of 30 minutes to 3 hours.
21. The method for preparing hollow conductive metal particles according to claim 10, It is characterized in that When the metal layer is a nickel-containing metal layer, the heating temperature of the annealing process is set in the range of 600° C. to 800° C., and the heating time is set in the range of 20 minutes to 3 hours.