Acid-modified polyester resin, laminate, and biodegradable adhesive

By using acid-modified polyester resin as the adhesive layer between the polylactic acid resin layer and the PVA resin layer, the problem of insufficient adhesiveness between the two is solved, and the appearance and melt forming properties of the laminated body are improved. , realizes biodegradability and efficient multi-layer membrane forming process.

CN119095897APending Publication Date: 2024-12-06MITSUBISHI CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380030827.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

There is a lack of good adhesion between the polylactic acid-based resin layer and the PVA-based resin layer, and the existing biodegradable polyester-based resin is insufficient in the fluidity and melt forming properties of the multi-layer film forming, resulting in the appearance of the laminated body and Limited practicality.

Method used

Acid-modified polyester resin is used to graft α,β-unsaturated carboxylic acid or its anhydride in the aliphatic-aromatic polyester resin, and use a specific amount of free radical initiator during the grafting process. The melt flow rate and the change rate under the storage temperature are controlled to form an adhesive layer with excellent melt forming properties.

Benefits of technology

The efficient bonding between the polylactic acid-based resin layer and the PVA-based resin layer is achieved, the appearance and melt forming properties of the laminated body are improved, and the fluidity and storage stability of the multi-layer film are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005061974340000041
    Figure BDA0005061974340000041
  • Figure BDA0005061974340000051
    Figure BDA0005061974340000051
  • Figure BDA0005061974340000052
    Figure BDA0005061974340000052
Patent Text Reader

Abstract

One embodiment of the present invention relates to an acid-modified polyester resin obtained by grafting an alpha, beta-unsaturated carboxylic acid and / or an anhydride (X) thereof onto an aliphatic-aromatic polyester resin containing an aliphatic diol unit, an aliphatic dicarboxylic acid unit, and an aromatic dicarboxylic acid unit, the melt flow rate (210 DEG C, load of 2160 g) of the acid-modified polyester resin is 1.4-15 g / 10 min, and the content of the [alpha], [beta]-unsaturated carboxylic acid and / or the anhydride (X) thereof is 0.0001-0.8 parts by mass per 100 parts by mass of the aliphatic-aromatic polyester resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an acid-modified polyester resin, and more specifically, to an acid-modified polyester resin preferably used in an adhesive layer between a polyvinyl alcohol resin layer (hereinafter polyvinyl alcohol is referred to as "PVA") and a biodegradable resin layer such as polylactic acid. In addition, the present invention relates to a laminate having a layer containing the acid-modified polyester resin and a biodegradable adhesive containing the acid-modified polyester resin. Background Art

[0002] Plastics are widely used as packaging materials due to their excellent moldability, strength, water resistance, transparency, etc. Examples of plastics used in packaging materials include polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polystyrene and polyvinyl chloride; and aromatic polyester resins such as polyethylene terephthalate. However, these plastics lack biodegradability and may remain for a long time if discarded in the natural world after use, thereby damaging the landscape or causing environmental damage.

[0003] In contrast, in recent years, biodegradable resins that are biodegradable or hydrolyzed in soil and water and are useful for preventing environmental pollution have attracted much attention and are being put into practical use. Aliphatic polyester resins, cellulose acetate, modified starch, etc. are known as such biodegradable resins. As packaging materials, polylactic acid, adipic acid / terephthalic acid / 1,4-butanediol polycondensates, succinic acid / 1,4-butanediol / lactic acid polycondensates, etc. can be used from the perspective of excellent transparency, heat resistance, and strength.

[0004] However, aliphatic polyester resins such as polylactic acid do not have sufficient oxygen barrier properties and therefore cannot be used alone as packaging materials for contents such as food and chemicals that may deteriorate by oxidation.

[0005] Therefore, a laminate having a coating layer formed on at least one surface of a polylactic acid film, the coating layer being based on PVA having excellent gas barrier properties and also having biodegradability has been proposed (see, for example, Patent Document 1).

[0006] In addition, as a biodegradable laminate that can be co-extruded and further stretched by using a PVA-based resin that can be melt-molded, a biodegradable laminate has been proposed in which both sides of a gas barrier layer are sandwiched by aliphatic polyester layers having a melting point difference of 20° C. or less with the gas barrier layer, wherein the gas barrier layer has a PVA-based resin having a 1,2-diol structure in the side chain as a main component (for example, see Patent Document 2).

[0007] However, the surface properties of the polylactic acid resin layer and the PVA resin layer are significantly different, so the two layers lack adhesion and it is difficult to obtain practical interlayer bonding strength by directly laminating the two layers. For example, Patent Document 1 proposes surface activation treatments such as corona discharge treatment, flame treatment, and ozone treatment for polylactic acid films, and anchor coating treatments, which are still unsatisfactory and have room for improvement.

[0008] In Patent Document 2, the interlayer adhesion between the polylactic acid-based resin layer and the PVA-based resin layer is slightly improved by coextrusion lamination, but this is still insufficient for practical use.

[0009] Therefore, in order to obtain good interlayer adhesion between the polylactic acid resin layer and the PVA resin layer, it is necessary to provide an adhesive layer between the two layers. Furthermore, in order to utilize the biodegradability of the polylactic acid resin and the PVA resin, it is sought that the adhesive layer used in the laminate containing them is also biodegradable.

[0010] Under such circumstances, it has been proposed to use a polyester resin having a polar group obtained by grafting a biodegradable polyester resin with an α,β-unsaturated carboxylic acid or anhydride thereof as an adhesive layer (see, for example, Patent Document 3).

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Publication No. 2000-177072

[0014] Patent Document 2: Japanese Patent Application Publication No. 2009-196287

[0015] Patent Document 3: Japanese Patent Application Publication No. 2013-212682 Summary of the invention

[0016] Problem that the invention aims to solve

[0017] However, the biodegradable polyester resin proposed in Patent Document 3 may have poor fluidity and melt moldability during multilayer film formation, and may have poor appearance when formed into a laminate. Therefore, a first problem is to provide an acid-modified polyester resin having excellent melt moldability and capable of obtaining a laminate having excellent appearance when used as an adhesive layer of two layers in a laminate containing a PVA resin layer and a biodegradable resin layer.

[0018] In addition, in the technology of the above-mentioned Patent Document 3, the melt flow rate (MFR) of the resin may decrease over time during storage, and when used for multilayer film production, the fluidity of the resin in the extruder deteriorates, thereby sometimes deteriorating the melt moldability. Therefore, the second problem is to provide an acid-modified polyester resin in which the decrease in MFR during storage is suppressed and the melt moldability is excellent.

[0019] Solutions for solving problems

[0020] The present inventors conducted intensive studies on the above-mentioned subject.

[0021] The present inventors have found that the first problem can be solved by using an acid-modified polyester resin having a higher MFR than conventional resins and a specific MFR value, thereby completing the present invention.

[0022] The present inventors have conducted intensive studies on the second problem and have found that the problem can be solved by using an acid-modified polyester resin satisfying a specific formula among acid-modified polyester resins.

[0023] That is, the present invention relates to the following aspects 1 to 11.

[0024] A first aspect of the present invention is an acid-modified polyester resin, which is an aliphatic-aromatic polyester resin grafted with an α,β-unsaturated carboxylic acid and / or anhydride (X) thereof, wherein the aliphatic-aromatic polyester resin comprises an aliphatic diol unit, an aliphatic dicarboxylic acid unit, and an aromatic dicarboxylic acid unit.

[0025] The melt flow rate (210°C, load 2160g) of the acid-modified polyester resin is 1.4 to 15g / 10min, and the content of the α,β-unsaturated carboxylic acid and / or its anhydride (X) is 0.0001 to 0.8 parts by mass based on 100 parts by mass of the aliphatic-aromatic polyester resin.

[0026] A second aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of the first aspect,

[0027] The aliphatic diol unit and the aliphatic dicarboxylic acid unit contain 50 mol% or more in total.

[0028] A third aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of the first or second aspect,

[0029] Furthermore, a radical initiator (Y) is contained during grafting.

[0030] A fourth aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of the third aspect,

[0031] The content ratio (Y' / X) of the radical (Y') obtained from the radical initiator (Y) to the α,β-unsaturated carboxylic acid and / or its anhydride (X) is 0.5 to 5 in terms of molar ratio.

[0032] A fifth aspect of the present invention is an acid-modified polyester resin, characterized in that:

[0033] When the MFR change rate coefficient K is plotted for each storage temperature based on the following formula (II), the temperature dependence coefficient α obtained satisfies the following formula (III):

[0034] The MFR change rate coefficient K is calculated by plotting the change in MFR (melt flow rate) over time when the product is stored at a plurality of temperatures using the following formula (I).

[0035] MFR(t)=MFR(0)×e^(-K×t)…(I)

[0036] ln(K)=α / T+β…(II)

[0037] |α|<10000…(III)

[0038] (In the above formula (I), MFR(t) represents the MFR (210°C, 2160 g load) of the resin after t days from the start of storage, and MFR(0) represents the MFR (210°C, 2160 g load) of the resin at the start of storage. Furthermore, K is the MFR change rate coefficient, and t is the time (days) elapsed from the start of storage. In the above formula (II), T represents the temperature during storage (K), and β represents a constant term. In the above formulas (II) and (III), α represents the temperature dependence coefficient of the MFR change rate coefficient.)

[0039] A sixth aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of the fifth aspect,

[0040] It has at least one structural unit selected from the structural units represented by the following general formulae (1) to (3).

[0041]

[0042] [In formula (1), l is an integer from 2 to 8.]

[0043]

[0044] [In formula (2), m is an integer of 2 to 10.]

[0045]

[0046] [In formula (3), n is an integer from 2 to 9.]

[0047] A seventh aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of the sixth aspect,

[0048] The present invention contains at least one structural unit selected from the structural units represented by the above-mentioned general formulae (1) to (3) in a total amount of 50 mol% or more.

[0049] An eighth aspect of the present invention is an acid-modified polyester resin, wherein in the acid-modified polyester resin of any one of aspects 5 to 7, the acid-modified polyester resin is a polyester resin grafted with an α,β-unsaturated carboxylic acid and / or anhydride thereof.

[0050] A ninth aspect of the present invention is a biodegradable adhesive comprising the acid-modified polyester resin according to any one of the first to eighth aspects.

[0051] A tenth aspect of the present invention is a laminate having at least one layer containing the acid-modified polyester-based resin according to any one of aspects 1 to 8.

[0052] Aspect 11 of the present invention is a laminated body comprising an adhesive layer provided between a polyvinyl alcohol-based resin (B) layer and a biodegradable resin (C) layer,

[0053] The adhesive layer contains the acid-modified polyester resin according to any one of Embodiments 1 to 8.

[0054] Effects of the Invention

[0055] The acid-modified polyester resin of the present invention has excellent melt moldability, and when used as an adhesive layer of two layers in a laminate containing a PVA-based resin layer and a biodegradable resin layer, for example, a laminate having excellent appearance can be obtained.

[0056] The acid-modified polyester resin of the present invention has a suppressed decrease in MFR during storage and is excellent in melt moldability. The acid-modified polyester resin of the present invention is useful as an adhesive layer of two layers in a laminate containing a PVA-based resin layer and a biodegradable resin layer, for example. DETAILED DESCRIPTION

[0057] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to the following embodiment and can be implemented with various modifications within the scope of the gist thereof.

[0058] It should be noted that, in the present specification, parts and percentages based on mass have the same meanings as parts and percentages based on weight, respectively.

[0059] In this specification, when the expression "to" is used, it is used as an expression including the numerical values ​​or physical property values ​​before and after it. That is, "A to B" means A or more and B or less.

[0060] In addition, in this specification, "biodegradability" means satisfying the conditions specified in JIS K 6953-1:2011 (ISO 14855-1:2005).

[0061] The acid-modified polyester resin (A) of the present invention includes the following first embodiment.

[0062] An acid-modified polyester resin is an acid-modified polyester resin in which an α,β-unsaturated carboxylic acid and / or anhydride (X) is grafted onto an aliphatic-aromatic polyester resin, wherein the aliphatic-aromatic polyester resin comprises an aliphatic diol unit, an aliphatic dicarboxylic acid unit and an aromatic dicarboxylic acid unit.

[0063] The melt flow rate (210°C, load 2160g) of the acid-modified polyester resin is 1.4 to 15g / 10min, and the content of the α,β-unsaturated carboxylic acid and / or its anhydride (X) is 0.0001 to 0.8 parts by mass based on 100 parts by mass of the aliphatic-aromatic polyester resin.

[0064] Moreover, the acid-modified polyester resin (A) of the present invention includes the following second embodiment.

[0065] An acid-modified polyester resin, characterized in that a temperature dependence coefficient α obtained by plotting an MFR change rate coefficient K for each storage temperature based on the following formula (II) satisfies the following formula (III), wherein the MFR change rate coefficient K is calculated by plotting the change in MFR (melt flow rate) over time when stored at multiple temperatures using the following formula (I).

[0066] MFR(t)=MFR(0)×e^(-K×t)…(I)

[0067] ln(K)=α / T+β…(II)

[0068] |α|<10000…(III)

[0069] (In the above formula (I), MFR(t) represents the MFR (210°C, 2160 g load) of the resin after t days from the start of storage, and MFR(0) represents the MFR (210°C, 2160 g load) of the resin at the start of storage. Furthermore, K is the MFR change rate coefficient, and t is the time (days) elapsed from the start of storage. In the above formula (II), T represents the temperature during storage (K), and β represents a constant term. In the above formulas (II) and (III), α represents the temperature dependence coefficient of the MFR change rate coefficient.)

[0070] Hereinafter, the acid-modified polyester resin (A) according to the first embodiment and the second embodiment will be described respectively.

[0071] [Acid-modified polyester resin (A) according to the first aspect]

[0072] The acid-modified polyester resin (A) described in the first embodiment of the present invention is characterized in that it is an acid-modified polyester resin in which an α,β-unsaturated carboxylic acid and / or anhydride (X) is grafted onto an aliphatic-aromatic polyester resin, the aliphatic-aromatic polyester resin comprising an aliphatic diol unit, an aliphatic dicarboxylic acid unit and an aromatic dicarboxylic acid unit, the melt flow rate (210°C, load 2160g) of the acid-modified polyester resin is 1.4 to 15g / 10min, and the content of the α,β-unsaturated carboxylic acid and / or anhydride (X) is 0.0001 to 0.8 parts by mass relative to 100 parts by mass of the aliphatic-aromatic polyester resin.

[0073] The acid-modified polyester resin (A) described in the first embodiment of the present invention is an acid-modified polyester resin obtained by grafting α,β-unsaturated carboxylic acid and / or its anhydride (hereinafter, α,β-unsaturated carboxylic acid and / or its anhydride may be referred to as "α,β-unsaturated carboxylic acid") with an aliphatic-aromatic polyester resin.

[0074] The aliphatic-aromatic polyester resin contains an aliphatic diol unit, an aliphatic dicarboxylic acid unit, and an aromatic dicarboxylic acid unit. When the aliphatic-aromatic polyester resin contains the above-mentioned structural units, the biodegradability of the acid-modified polyester resin (A) is improved.

[0075] The total content of the aliphatic diol unit, the aliphatic dicarboxylic acid unit and the aromatic dicarboxylic acid unit in the acid-modified polyester resin (A) according to the first aspect of the present invention is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more.

[0076] Among them, the acid-modified polyester resin (A) according to the first aspect of the present invention preferably contains 50 mol % or more of an aliphatic diol unit and an aliphatic dicarboxylic acid unit.

[0077] The acid-modified polyester resin (A) according to the first embodiment of the present invention contains 50 mol% or more of aliphatic diol units and aliphatic dicarboxylic acid units in total, thereby improving biodegradability. The acid-modified polyester resin (A) according to the first embodiment of the present invention more preferably contains 70 mol% or more of aliphatic diol units and aliphatic dicarboxylic acid units in total, and further preferably 90 mol% or more.

[0078] Specifically, the aliphatic carboxylic acid unit is preferably an aliphatic carboxylic acid unit represented by the following general formula (1). In addition, the aliphatic diol unit is preferably an aliphatic diol unit represented by the following formula (2).

[0079]

[0080] [In formula (1), l is an integer from 2 to 8.]

[0081]

[0082] [In formula (2), m is an integer of 2 to 10.]

[0083] In the above formula (1), l is an integer of 2 to 8, and is preferably an integer of 3 to 5 from the viewpoint of moldability and flexibility.

[0084] In the above formula (2), m is an integer of 2 to 10, and is preferably an integer of 3 to 5 from the viewpoint of moldability and flexibility.

[0085] The acid-modified polyester resin (A) according to the first embodiment of the present invention is composed of structural units represented by aliphatic diol units, aliphatic dicarboxylic acid units and aromatic dicarboxylic acid units, and may have other structural units for the purpose of controlling heat resistance, strength, biodegradability and the like.

[0086] The acid-modified polyester resin (A) according to the first embodiment of the present invention having an aliphatic diol unit, an aliphatic dicarboxylic acid unit and an aromatic dicarboxylic acid unit can be obtained by polycondensing at least one selected from the group consisting of an aliphatic dicarboxylic acid, an aliphatic diol compound, a cyclic aliphatic diol compound, a cyclic aliphatic dicarboxylic acid, an aromatic dicarboxylic acid and other components by a known method, and then acid-modifying the polycondensed polyester resin.

[0087] Examples of the aliphatic dicarboxylic acid include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid, azelaic acid, and sebacic acid. Among them, adipic acid is preferred from the viewpoint of moldability and flexibility.

[0088] Examples of the aliphatic diol compound include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol. Among them, 1,4-butanediol is preferred from the viewpoint of moldability and flexibility.

[0089] Examples of the cyclic aliphatic diol compound include 1,3-cyclohexanediol and 1,4-cyclohexanediol. Among them, 1,4-cyclohexanediol is preferred from the viewpoint of moldability and flexibility.

[0090] Examples of the cycloaliphatic dicarboxylic acid include 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid. Among them, 1,4-cyclohexanedicarboxylic acid is preferred from the viewpoint of moldability and flexibility.

[0091] Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, and furandicarboxylic acid. Among them, terephthalic acid is preferred from the viewpoint of moldability. In addition, derivatives of aromatic dicarboxylic acids may be used.

[0092] In addition, as other components, specifically, there can be listed hydroxy acids such as 4-hydroxybutyric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid; dicarboxylic acids such as oxalic acid and malonic acid having an alkylene chain number of less than 2 and their derivatives; hydroxycarboxylic acids such as glycolic acid and lactic acid having an alkylene chain number of less than 2 and their derivatives; and other components that are well-known as copolymer components of polyester resins.

[0093] The acid-modified polyester resin (A) according to the first embodiment of the present invention is obtained by grafting the above-mentioned aliphatic-aromatic polyester resin (hereinafter sometimes referred to as raw material polyester resin (A')) with an α,β-unsaturated carboxylic acid and / or anhydride thereof. Such an acid-modified polyester resin (A) has excellent adhesiveness.

[0094] Specific examples of the α,β-unsaturated carboxylic acids (X) include α,β-unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid; α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, or anhydrides thereof. Preferably, anhydrides of α,β-unsaturated dicarboxylic acids are used.

[0095] In addition, these α,β-unsaturated carboxylic acids (X) are not limited to the case where one type is used alone, and two or more types may be used in combination.

[0096] The method for obtaining the acid-modified polyester resin (A) grafted with the α,β-unsaturated carboxylic acid (X) by grafting the α,β-unsaturated carboxylic acid (X) with the raw material polyester resin (A') is not particularly limited, and a known method can be used. It may be a thermal reaction only, but in order to improve the reactivity, it is preferred to use a free radical initiator (Y). In addition, the reaction method includes a solution reaction, a reaction in the form of a suspension, a reaction in a molten state without using a solvent (melting method), etc. Among them, the melting method is preferred.

[0097] Examples of commercially available products of the raw material polyester resin (A') include "Ecoflex" manufactured by BASF Corporation, which has a polycondensate of adipic acid / terephthalic acid / 1,4-butanediol as a main component.

[0098] The melting method will be described in detail below.

[0099] As the melting method, the following methods can be used: a method in which the raw material polyester resin (A'), α, β-unsaturated carboxylic acid (X) and free radical initiator (Y) are pre-mixed and then melt-kneaded in a kneader to react; a method in which the α, β-unsaturated carboxylic acid (X) and free radical initiator (Y) are added to the raw material polyester resin (A') in a molten state in a kneader, etc.

[0100] As a mixer used when mixing the raw materials in advance, for example, a Henschel mixer, a ribbon blender, etc. can be used, and as a kneading machine used for melt kneading, for example, a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader, a Brabender agitator, etc. can be used.

[0101] The temperature during melt kneading may be appropriately set within a temperature range not lower than the melting point of the raw material polyester resin (A') and not causing thermal degradation. Melt kneading is preferably performed at 100 to 250°C, more preferably 160 to 220°C.

[0102] When the grafting reaction is carried out using a kneader, the screw speed of the kneader is preferably 220 to 800 rpm. If the screw speed is within the above range, the MFR can be adjusted to the preferred range. The screw speed is more preferably 250 to 625 rpm, and even more preferably 350 to 550 rpm.

[0103] Furthermore, when a mixer is used to carry out the grafting reaction, the screw diameter (D) of the mixer is preferably 3 to 500 mm. If the screw diameter (D) is within the above range, thermal degradation of the resin can be suppressed and the production volume can be increased. The screw diameter (D) is more preferably 5 to 300 mm, the screw diameter (D) is further preferably 10 to 200 mm, and particularly preferably 15 to 100 mm.

[0104] It should be noted that the screw diameter (D) generally refers to the outer diameter of the screw.

[0105] In addition, the ratio (L / D) of the screw diameter (D) to the screw length (L) is preferably in the range of 10 to 200. When L / D is in the above range, thermal degradation of the resin can be suppressed and the production volume can be improved. L / D is more preferably 20 to 150, and even more preferably 25 to 100.

[0106] When the graft reaction is carried out using a kneading machine, the kneading section for carrying out kneading may be provided at only one location in the kneading machine, or may be provided at a plurality of locations.

[0107] In the first aspect of the present invention, the content of the α,β-unsaturated carboxylic acid (X) is 0.0001 to 0.8 parts by mass, preferably 0.001 to 0.6 parts by mass, and more preferably 0.02 to 0.45 parts by mass based on 100 parts by mass of the raw polyester resin (A′).

[0108] If the content of the α,β-unsaturated carboxylic acid (X) is 0.0001 parts by mass or more relative to 100 parts by mass of the raw polyester resin (A'), a sufficient amount of polar groups can be introduced into the aliphatic-aromatic polyester resin, and interlayer adhesion, especially adhesion to the PVA resin layer, can be sufficiently obtained. In addition, if the content of the α,β-unsaturated carboxylic acid (X) is 0.8 parts by mass or less relative to 100 parts by mass of the raw polyester resin (A'), the α,β-unsaturated carboxylic acid (X) that has not undergone a grafting reaction is unlikely to remain in the resin, and the appearance defects caused by this can be suppressed.

[0109] In the first aspect of the present invention, from the viewpoint of improving the graft reaction efficiency, it is preferred that a radical initiator (Y) is contained during grafting. That is, the acid-modified polyester resin according to the first aspect of the present invention contains a radical initiator (Y) during grafting.

[0110] The radical initiator (Y) is not particularly limited, and a known one can be used, and examples thereof include organic or inorganic peroxides such as tert-butyl hydroperoxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-bis(tert-butyloxy)hexane, 3,5,5-trimethylhexanoyl peroxide, tert-butyl perbenzoate, benzoyl peroxide, m-toluoyl peroxide, dicumyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, dibutyl peroxide, methyl ethyl ketone peroxide, potassium peroxide, and hydrogen peroxide; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(isobutylamide)diacid halide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and di-tert-butane; and diisopropylbenzene and the like.

[0111] These may be used alone or in combination of two or more.

[0112] In the first aspect of the present invention, the content of the radical initiator (Y) is preferably 0.00001 to 5.0 parts by mass, more preferably 0.0001 to 1.0 part by mass, and even more preferably 0.002 to 0.5 parts by mass based on 100 parts by mass of the raw polyester resin (A').

[0113] If the content of the radical initiator (Y) is 0.00001 parts by mass or more relative to 100 parts by mass of the raw material polyester resin (A'), the grafting reaction is sufficiently carried out, and the effect of the present invention is easily obtained. In addition, if the content of the radical initiator (Y) is 5.0 parts by mass or less, it is not easy to reduce the molecular weight due to the decomposition of the polyester resin, and insufficient adhesive strength caused by insufficient cohesive force can be suppressed.

[0114] In addition, the content ratio (Y' / X) of the free radical (Y') obtained from the free radical initiator (Y) to the α,β-unsaturated carboxylic acid and / or its anhydride (X) is preferably 0.5 to 5 in terms of molar ratio. By setting Y' / X in the range of 0.5 to 5, the α,β-unsaturated carboxylic acid (X) that has not undergone the grafting reaction is unlikely to remain in the resin, and the appearance defects caused by this can be suppressed. Y' / X is more preferably 0.6 to 4, further preferably 0.7 to 3, and particularly preferably 0.8 to 2.

[0115] In addition, the amount of the radical (Y') obtained from the radical initiator (Y) is set as the theoretical value of the radical that can be generated from the radical initiator (Y).

[0116] The acid-modified polyester resin (A) according to the first aspect of the present invention has an MFR of 1.4 to 15 g / 10 min.

[0117] If the MFR of the acid-modified polyester resin (A) according to the first embodiment of the present invention is less than 1.4 g / 10 min, the fluidity is reduced, and thus there is a tendency for the appearance to deteriorate during multilayer film formation. In addition, by setting the MFR of the acid-modified polyester resin (A) to 15 g / 10 min or less, it is possible to suppress the viscosity difference between the acid-modified polyester resin (A) and other resins from becoming large during multilayer film formation, and the appearance during multilayer film formation can be improved.

[0118] The smaller the molecular weight of the acid-modified polyester resin (A), the larger the MFR and the higher the fluidity. It is inferred that in the first embodiment of the present invention, the screw speed is controlled during the grafting reaction of the acid-modified polyester resin (A), and the shear in the extruder is controlled to reduce the molecular weight, thereby improving the fluidity of the acid-modified polyester resin (A) and obtaining the effect of the present invention.

[0119] From the viewpoint of appearance during multilayer film formation, the MFR is preferably 2 to 10 g / 10 min, more preferably 3 to 7 g / 10 min.

[0120] The method for measuring the above-mentioned MFR will be described in detail below.

[0121] Determination method

[0122] Use a melt index tester based on JIS K 7210-1:2014. Put 5g of the sample into a barrel set to 210°C and feed it within 30 seconds. After 4 minutes and 30 seconds from the time the sample is put in, carry a weight of 2160g, cut off the strands extruded 5 minutes after the sample is put in and discard them. Then, cut the strands 6 minutes, 7 minutes, and 8 minutes after the sample is put in, and collect a total of 3 strands. Measure the mass of the 3 strands collected and find the average value. Calculate MFR based on the average mass calculated using the following formula.

[0123] MFR (g / 10min) = W × 10

[0124] W: average mass of 3 strands (g)

[0125] 10: Factor used to convert grams per minute to grams per 10 minutes

[0126] In order to make the said MFR into a specific range, the following method is mentioned, for example.

[0127] (i) A method of adjusting the screw speed of the extruder during the graft reaction of the acid-modified polyester resin (A).

[0128] (ii) A method of adjusting the amount of the radical initiator (Y) used during the graft reaction of the acid-modified polyester resin (A).

[0129] Among them, method (i) is preferred from the viewpoint of efficiency of the graft reaction.

[0130] The weight average molecular weight of the acid-modified polyester resin (A) according to the first embodiment of the present invention is preferably 5,000 to 500,000, more preferably 50,000 to 400,000, further preferably 100,000 to 200,000, and particularly preferably 140,000 to 180,000. When the weight average molecular weight is 500,000 or less, the melt viscosity is suppressed from increasing, and melt molding is easy. In addition, when the weight average molecular weight is 5,000 or more, the molded product can be suppressed from becoming brittle.

[0131] It should be noted that the above weight average molecular weight is a weight average molecular weight converted based on a standard polystyrene molecular weight, and was determined by using two columns in series in a high performance liquid chromatograph (manufactured by Tosoh Corporation, “HLC-8320GPC”): TSKgel SuperMultipore HZ-M (exclusion limit molecular weight: 2×10 6 , theoretical plate number: 16,000 plates / plate, filler material: styrene-divinylbenzene copolymer, filler particle size: 4 μm).

[0132] [Acid-modified polyester resin (A) according to the second aspect]

[0133] The acid-modified polyester resin (A) described in the second embodiment of the present invention is characterized in that the temperature dependence coefficient α obtained when the MFR change rate coefficient K is plotted for each storage temperature based on the following formula (II) satisfies the following formula (III), wherein the MFR change rate coefficient K is calculated by plotting the time-dependent MFR change when stored at multiple temperatures using the following formula (I).

[0134] MFR(t)=MFR(0)×e^(-K×t)…(I)

[0135] ln(K)=α / T+β…(II)

[0136] |α|<10000…(III)

[0137] (In the above formula (I), MFR(t) represents the MFR (210°C, 2160 g load) of the resin after t days from the start of storage, MFR(0) represents the MFR (210°C, 2160 g load) of the resin at the start of storage, and e is the base of the natural logarithm. Furthermore, K is the MFR change rate coefficient, and t is the time (days) elapsed from the start of storage. In the above formula (II), ln represents the natural logarithm, T represents the temperature during storage (K), and β represents a constant term. In the above formulas (II) and (III), α represents the temperature dependence coefficient of the MFR change rate coefficient.)

[0138] When the acid-modified polyester resin (A) according to the second aspect of the present invention satisfies the above conditions, the temperature dependence of the crosslinking reaction during storage becomes small, and the variation in MFR due to the difference in storage temperature becomes small, thereby achieving excellent storage stability.

[0139] Here, the magnitude of |α| is an index of storage stability. If |α| is 10,000 or more, the temperature dependence of the crosslinking reaction during storage becomes large, and the variation of MFR due to the difference in storage temperature becomes large, and the storage stability decreases.

[0140] It is believed that if the uniformity of the grafting reaction of the acid-modified polyester resin (A) is reduced, the grafted polar group will be localized. It can be inferred that the polar group not only serves as the starting point of the cross-linking reaction, but also functions as a catalyst for hydrolysis. Therefore, if the polar group is localized, the terminal hydroxyl group generated by hydrolysis will immediately react with the adjacent polar group, thereby promoting the cross-linking reaction. It can be inferred that by uniformly modifying, the abnormal cross-linking reaction is suppressed, and thus the MFR reduction rate during high-temperature storage is reduced. Therefore, it can be inferred that, for example, when the acid-modified polyester resin (A) is manufactured, the fluidity of the resin is increased by increasing the temperature in the extruder during the grafting reaction, and the uniformity during kneading with the free radical initiator and the α, β-unsaturated carboxylic acid and / or its anhydride, and then the uniformity of the grafting reaction is improved, thereby suppressing the localization of the polar group, and thus the effect of the present invention can be obtained.

[0141] In the above formula (III), from the viewpoint of the fluidity of the resin after storage, the value of |α| is less than 10,000, preferably 7,000 or less, and more preferably 5,000 or less.

[0142] The method for determining the value of |α| based on the above-mentioned formula (I) to formula (II) will be described in detail below.

[0143] 10 g of the acid-modified polyester resin (A) is weighed and put into an aluminum bag, and then stored in a sealed state by heat sealing. The MFR at the beginning of storage is measured, and then the bag is stored at an arbitrary temperature, and the MFR after an arbitrary storage period is measured. Here, including the beginning of storage, more than 3 samples are measured at intervals of more than 7 days within 100 days, and the MFR of the resin after t days is set as MFR(t). Furthermore, MFR(t) and the elapsed time t are plotted based on formula (I), and the MFR change rate coefficient K is calculated by the least squares method. Regarding this K, it is calculated at more than 4 points at intervals of more than 5K among the storage temperatures of 273.15 to 373.15K. Based on formula (II), the storage temperature T and the MFR change rate coefficient K are plotted, and the temperature dependence coefficient α of the MFR change rate coefficient K is calculated by the least squares method.

[0144] [Method for measuring MFR]

[0145] Use a melt index tester in accordance with JIS K 7210-1:2014. Put 5g of the sample into a barrel set to 210°C and feed it within 30 seconds. After 4 minutes and 30 seconds from the time the sample is put in, carry a weight of 2160g, cut off the strands extruded 5 minutes after the sample is put in and discard them. Then, cut the strands 6 minutes, 7 minutes, and 8 minutes after the sample is put in, and collect a total of 3 strands. Measure the mass of the 3 strands collected and find the average value. Calculate MFR based on the average mass calculated using the following formula.

[0146] MFR (g / 10min) = W × 10

[0147] W: average mass of 3 strands (g)

[0148] 10: Factor used to convert grams per minute to grams per 10 minutes

[0149] In order to obtain the acid-modified polyester resin (A) satisfying the above formula (III), for example, the following method can be mentioned.

[0150] (i) A method of adjusting the ratio (Q / N (kg / (hr·rpm)) of the discharge amount (Q (kg / hr)) and the screw rotation speed (N (rpm)) during the grafting reaction.

[0151] (ii) A method of adjusting the set temperature of the extruder during the graft reaction.

[0152] Among them, method (i) is preferred from the viewpoint of production efficiency.

[0153] The acid-modified polyester resin (A) according to the second aspect of the present invention preferably has at least one structural unit selected from the structural units represented by the following general formulae (1) to (3).

[0154]

[0155] [In formula (1), l is an integer from 2 to 8.]

[0156]

[0157] [In formula (2), m is an integer of 2 to 10.]

[0158]

[0159] [In formula (3), n is an integer from 2 to 9.]

[0160] In the above formula (1), l is an integer of 2 to 8, and is preferably an integer of 3 to 5 from the viewpoint of moldability and flexibility.

[0161] In the above formula (2), m is an integer of 2 to 10, and is preferably an integer of 3 to 5 from the viewpoint of moldability and flexibility.

[0162] In the above formula (3), n is an integer of 2 to 9, and is preferably an integer of 3 to 5 from the viewpoint of moldability and flexibility.

[0163] From the viewpoint of biodegradability, the acid-modified polyester resin (A) described in the second embodiment of the present invention is more preferably composed of at least one structural unit selected from the structural units represented by the above-mentioned general formulas (1) to (3), and may have other structural units for the purpose of controlling heat resistance, strength, biodegradability, etc.

[0164] The total content of at least one structural unit selected from the structural units represented by the general formulae (1) to (3) is preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more.

[0165] When the acid-modified polyester resin (A) described in the second embodiment of the present invention has at least one structural unit selected from the structural units represented by the above general formulae (1) to (3), it can be obtained by polycondensing at least one selected from the group consisting of aliphatic dicarboxylic acids, aliphatic diol compounds, cyclic aliphatic diol compounds, cyclic aliphatic dicarboxylic acids and other components using a known method, and then acid-modifying.

[0166] Examples of the aliphatic dicarboxylic acid include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid, azelaic acid, and sebacic acid. Among them, adipic acid is preferred from the viewpoint of moldability and flexibility.

[0167] Examples of the aliphatic diol compound include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol. Among them, 1,4-butanediol is preferred from the viewpoint of moldability and flexibility.

[0168] Examples of the cyclic aliphatic diol compound include 1,3-cyclohexanediol and 1,4-cyclohexanediol. Among them, 1,4-cyclohexanediol is preferred from the viewpoint of moldability and flexibility.

[0169] Examples of the cycloaliphatic dicarboxylic acid include 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid. Among them, 1,4-cyclohexanedicarboxylic acid is preferred from the viewpoint of moldability and flexibility.

[0170] In addition, specific examples of other components include hydroxy acids such as 4-hydroxybutyric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid; aromatic dicarboxylic acids and derivatives such as terephthalic acid, isophthalic acid, and furandicarboxylic acid; dicarboxylic acids and derivatives thereof such as oxalic acid and malonic acid having an alkylene chain number of less than 2; hydroxycarboxylic acids and derivatives thereof such as glycolic acid and lactic acid having an alkylene chain number of less than 2; and other components known as copolymer components of polyester resins.

[0171] The weight average molecular weight of the acid-modified polyester resin (A) according to the second embodiment of the present invention is preferably 5,000 to 500,000, more preferably 50,000 to 400,000, further preferably 100,000 to 200,000, and particularly preferably 140,000 to 180,000. When the weight average molecular weight is 500,000 or less, the melt viscosity is not too high, and melt molding is easy. In addition, when the weight average molecular weight is 5,000 or more, it is possible to suppress the brittleness of the molded product.

[0172] It should be noted that the above weight average molecular weight is a weight average molecular weight converted based on a standard polystyrene molecular weight, and was determined by using two columns in series in a high performance liquid chromatograph (manufactured by Tosoh Corporation, “HLC-8320GPC”): TSKgel Super Multipore HZ-M (exclusion limit molecular weight: 2×10 6 , theoretical plate number: 16,000 plates / plate, filler material: styrene-divinylbenzene copolymer, filler particle size: 4 μm).

[0173] Regarding the acid-modified polyester resin (A) described in the second embodiment of the present invention, from the viewpoint of adhesion, an acid-modified polyester resin (A) in which an α,β-unsaturated carboxylic acid and / or anhydride thereof (hereinafter sometimes referred to as “α,β-unsaturated carboxylic acid”) is grafted onto the raw polyester resin (A′) is good.

[0174] Specific examples of the α,β-unsaturated carboxylic acids include α,β-unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid; α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, or anhydrides thereof. Preferably, anhydrides of α,β-unsaturated dicarboxylic acids are used.

[0175] In addition, these α, β-unsaturated carboxylic acids are not limited to the case where one type is used alone, and two or more types may be used in combination.

[0176] The method for obtaining the acid-modified polyester resin (A) grafted with the α,β-unsaturated carboxylic acid by grafting the α,β-unsaturated carboxylic acid with the raw material polyester resin (A') is not particularly limited, and a known method can be used. It may be a thermal reaction only, but in order to improve the reactivity, it is preferred to use a free radical initiator. In addition, the reaction method includes a solution reaction, a suspension reaction, a reaction in a molten state without using a solvent (melt method), etc. Among them, the melt method is preferred.

[0177] Examples of commercially available raw material polyester resins (A') include "Ecoflex" manufactured by BASF Corporation, which mainly comprises a polycondensate of adipic acid / terephthalic acid / 1,4-butanediol, and "BioPBS" manufactured by Mitsubishi Chemical Corporation, which mainly comprises a polycondensate of succinic acid / 1,4-butanediol.

[0178] The melting method will be described in detail below.

[0179] As the melt method, the following methods can be used: a method in which the raw material polyester resin (A'), α, β-unsaturated carboxylic acid and free radical initiator are pre-mixed and then melt-kneaded in a kneader to react; a method in which the α, β-unsaturated carboxylic acid and free radical initiator are added to the polyester resin (A') in a molten state in a kneader, etc.

[0180] As a mixer used when mixing the raw materials in advance, for example, a Henschel mixer, a ribbon blender, etc. can be used, and as a kneading machine used for melt kneading, for example, a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader, a Brabender agitator, etc. can be used.

[0181] In the second aspect of the present invention, the temperature setting during melt kneading can be appropriately set within a temperature range above the melting point of the raw material polyester resin (A') and where thermal degradation does not occur. The temperature setting during melt kneading is preferably 100 to 250°C, more preferably 160 to 220°C.

[0182] When the grafting reaction is carried out using a kneader, the screw speed N of the kneader is preferably 100 to 700 rpm. If the screw speed N is within the above range, the uniformity of the grafting reaction can be improved. The screw speed N is more preferably 200 to 600 rpm, and further preferably 300 to 500 rpm.

[0183] The discharge rate Q of the kneader during the grafting reaction is preferably 200 to 800 kg / hr. If the discharge rate Q is within the above range, the uniformity of the grafting reaction can be improved. The discharge rate Q is more preferably 300 to 700 kg / hr, and further preferably 400 to 600 kg / hr.

[0184] In addition, the ratio (Q / N) of the discharge amount Q to the screw speed N during the grafting reaction is preferably 1.20 or more. By making Q / N 1.20 or more, the uniformity of the grafting reaction can be improved. Q / N is preferably 1.21 or more, more preferably 1.22 or more, further preferably 1.23 or more, and particularly preferably 1.24 or more. In addition, from the viewpoint of manufacturing, Q / N is preferably 3.00 or less, more preferably 2.50 or less, further preferably 2.00 or less, and particularly preferably 1.50 or less.

[0185] When the graft reaction is carried out using a kneading machine, the kneading section for carrying out kneading may be provided at only one location in the kneading machine, or may be provided at a plurality of locations.

[0186] In the second embodiment of the present invention, the amount of α,β-unsaturated carboxylic acid is preferably 0.0001 to 5 parts by mass, more preferably 0.001 to 1 part by mass, and further preferably 0.02 to 0.45 parts by mass relative to 100 parts by mass of the raw material polyester resin (A'). If the amount is 0.0001 parts by mass or more, a sufficient amount of polar groups are introduced into the polyester resin (A'), and the interlayer adhesion, especially the adhesion to the PVA resin layer, can be fully obtained. In addition, if the amount is 5 parts by mass or less, the α,β-unsaturated carboxylic acid that has not undergone the grafting reaction is not easy to remain in the resin, which can suppress the appearance defects caused by this.

[0187] The free radical initiator is not particularly limited, and known substances can be used, and examples thereof include organic or inorganic peroxides such as tert-butyl hydroperoxide, isopropyl hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-bis(tert-butyloxy)hexane, 3,5,5-trimethylhexanoyl peroxide, tert-butyl perbenzoate, benzoyl peroxide, m-toluoyl peroxide, dicumyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, dibutyl peroxide, methyl ethyl ketone peroxide, potassium peroxide, and hydrogen peroxide; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(isobutylamide)diacid halide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and di-tert-butane; and diisopropylbenzene and the like.

[0188] These may be used alone or in combination of two or more.

[0189] The amount of the radical initiator is preferably 0.00001 to 5.0 parts by mass, more preferably 0.0001 to 1.0 part by mass, and even more preferably 0.002 to 0.5 parts by mass, based on 100 parts by mass of the raw polyester resin (A').

[0190] If the amount of the free radical initiator blended is 0.00001 parts by mass or more, the grafting reaction will proceed sufficiently and the effect of the present invention will be easily obtained. If the amount of the free radical initiator blended is 5.0 parts by mass or less, low molecular weight caused by decomposition of the polyester resin will not easily occur, and insufficient adhesive strength caused by insufficient cohesive force can be suppressed.

[0191] The acid-modified polyester resin according to the first and second aspects of the present invention can be suitably used as a biodegradable adhesive. That is, the biodegradable adhesive according to the first and second aspects of the present invention contains the acid-modified polyester resin of the present invention.

[0192] The acid-modified polyester resin (A) according to the first and second aspects of the present invention can be particularly suitably used as an adhesive composition for a laminate, for example, as an adhesive layer when laminating a PVA resin (B) layer and a biodegradable resin (C) layer having different surface properties.

[0193] Hereinafter, the PVA-based resin (B) layer and the biodegradable resin (C) layer constituting the laminate will be described.

[0194] [PVA-based resin (B) layer]

[0195] The PVA-based resin (B) layer is preferably used for a gas barrier layer of the laminate of the present invention described later, and particularly preferably assumes the gas barrier properties of the laminate of the present invention.

[0196] It is preferred that a PVA-based resin (B) layer is laminated on at least one surface of the biodegradable resin (C) layer described later via a layer (adhesive layer) containing the acid-modified polyester-based resin (A) of the present invention.

[0197] The PVA resin (B) layer used in the present invention is a layer having a PVA resin (B) as a main component, and preferably contains 70% by mass or more of the PVA resin (B), more preferably 80% by mass or more, and further preferably 90% by mass or more. The upper limit is 100% by mass. If the content is 70% by mass or more, gas barrier properties are fully obtained.

[0198] The PVA-based resin (B) used in the present invention is a resin mainly composed of vinyl alcohol structural units, obtained by saponifying a polyvinyl ester-based resin obtained by polymerizing a vinyl ester-based monomer, and is composed of vinyl alcohol structural units and vinyl ester structural units having equivalent degrees of saponification.

[0199] Examples of the vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate. In terms of economy, vinyl acetate is preferably used.

[0200] The average degree of polymerization (measured in accordance with JIS K6726-1994) of the PVA-based resin (B) used in the present invention is preferably 200 to 1800, more preferably 300 to 1500, and even more preferably 300 to 1000.

[0201] If the average degree of polymerization is 200 or more, the mechanical strength of the PVA resin (B) layer can be sufficiently obtained. In addition, if the average degree of polymerization is 1800 or less, when the PVA resin (B) layer is formed by hot melt molding, the fluidity can be suppressed from decreasing, and the moldability can be improved. In addition, the abnormal occurrence of shear heat release during molding can be suppressed, and the PVA resin (B) is not easily thermally decomposed.

[0202] The saponification degree (measured in accordance with JIS K6726-1994) of the PVA-based resin (B) used in the present invention is preferably 80 to 100 mol %, more preferably 90 to 99.9 mol %, and even more preferably 98 to 99.9 mol %.

[0203] When the saponification degree is 80 mol % or more, the gas barrier properties are improved.

[0204] In addition, in the present invention, as the PVA-based resin (B), there can be used a resin obtained by copolymerizing various monomers and saponifying them when manufacturing a polyvinyl ester-based resin; and various modified PVA-based resins obtained by introducing various functional groups into unmodified PVA by post-modification.

[0205] Examples of the monomers used in the copolymerization with the vinyl ester monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; α-olefins containing a hydroxyl group such as 3-butene-1-ol, 4-pentene-1-ol, 5-hexene-1-ol, and 3,4-dihydroxy-1-butene, and their derivatives such as acylates; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, their salts, their monoesters, or their dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; diacetone acrylamide, acrylamide , amides such as methacrylamide; olefin sulfonic acids or their salts such as ethylene sulfonic acid, allyl sulfonic acid, and methyl allyl sulfonic acid; vinyl compounds such as alkyl vinyl ethers, dimethyl allyl vinyl ketone, N-vinyl pyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, glycerol monoallyl ether, 3,4-diacetoxy-1-butene; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; vinylidene chloride, 1,4-diacetoxy-2-butene, vinyl carbonate, etc.

[0206] In addition, as modified PVA-based resins into which functional groups are introduced by post-modification, there can be listed: resins having an acetoacetyl group by reaction with diene ketone, resins having a polyoxyalkylene group by reaction with ethylene oxide, resins having a hydroxyalkyl group by reaction with epoxy compounds, or resins obtained by reacting aldehyde compounds having various functional groups with PVA, etc.

[0207] Regarding the content of the modified species in the modified PVA-based resin, i.e., the structural units derived from various monomers in the copolymer or the functional groups introduced through post-reaction, it is impossible to generalize because the properties vary significantly depending on the modified species. It is preferably in the range of 1 to 20 mol%, and more preferably in the range of 2 to 10 mol%.

[0208] Among these various modified PVA-based resins, in the present invention, for the method for producing the laminate of the present invention described later, from the viewpoint of easy melt molding, it is preferred to use a PVA-based resin comprising a structural unit having a 1,2-diol structure in the side chain represented by the following general formula (4) (hereinafter sometimes referred to as a "1,2-diol structural unit").

[0209]

[0210] It should be noted that R 1 ~R 4 Each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms.

[0211] Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl and tert-butyl groups. The alkyl group may have a functional group such as a halogen group, a hydroxyl group, an ester group, a carboxylic acid group or a sulfonic acid group as required.

[0212] In addition, X in the 1,2-diol structural unit represented by the general formula (4) represents a single bond or a bond chain.

[0213] Examples of the bond chain include -O-, -(CH 2 O) t -、-(OCH 2 ) t -、-(CH 2 O) t CH 2 -、-CO-、-COCO-、-CO(CH 2 ) t CO-、-CO(C 6 H 4 )CO-, -S-, -CS-, -SO-, -SO 2 -, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO 4 -、-Si(OR) 2 -、-OSi(OR) 2 -、-OSi(OR) 2 O-、-Ti(OR) 2 -、-OTi(OR) 2 -、-OTi(OR) 2 O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, etc. (R is independently an arbitrary substituent, representing a hydrogen atom, a linear alkyl group or a branched alkyl group having 1 to 6 carbon atoms, and t represents an integer of 1 to 5).

[0214] Among them, from the viewpoint of stability during production or use, the bond chain is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and particularly preferably a methylene group or -CH 2 OCH 2 -.

[0215] From the viewpoint of thermal stability and stability under high temperature or acidic conditions, X is most preferably a single bond.

[0216] Among the 1,2-diol structural units represented by the general formula (4), R 1 ~R 4 Each of them is a hydrogen atom and X is a single bond, and is a structural unit represented by the following general formula (4').

[0217]

[0218] Examples of a method for producing a PVA-based resin having a 1,2-diol structural unit in a side chain include the method described in paragraphs

[0026] to

[0034] of JP-A-2015-143356.

[0219] The content of the 1,2-diol structural unit contained in the PVA-based resin having the 1,2-diol structural unit in the side chain is preferably 1 to 20 mol%, more preferably 2 to 10 mol%, and further preferably 3 to 8 mol%. If the content is 1 mol% or more, the effect of the side chain 1,2-diol structure can be fully obtained, and if the content is 20 mol% or less, the reduction in gas barrier properties under high humidity can be suppressed.

[0220] It should be noted that the content of the 1,2-diol structural unit in the PVA-based resin can be determined by the amount of the substance obtained by completely saponifying the PVA-based resin. 1 The content can be determined from the H-NMR spectrum (solvent: DMSO-d6, internal standard: tetramethylsilane). Specifically, the content can be calculated based on the peak areas of hydroxyl protons, methine protons and methylene protons in the 1,2-diol structural unit, methylene protons in the main chain, and protons of hydroxyl groups connected to the main chain.

[0221] In addition, the PVA resin (B) used in the present invention may be one type or a mixture of two or more types. When the PVA resin (B) is a mixture of two or more types, a combination of the above-mentioned unmodified PVAs may be used; a combination of unmodified PVA and a PVA resin having a structural unit represented by the general formula (4); a combination of PVA resins having a structural unit represented by the general formula (4) with different degrees of saponification, polymerization, and modification; a combination of unmodified PVA or a PVA resin having a structural unit represented by the general formula (4) and other modified PVA resins, etc.

[0222] In addition, the PVA-based resin (B) layer used in the present invention may also contain, in addition to the PVA-based resin (B), a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, an antistatic agent, a flame retardant, a plasticizer, a lubricant, a filler, a lubricant, and a crystal nucleating agent.

[0223] [Biodegradable resin (C) layer]

[0224] Next, the biodegradable resin (C) layer preferably used in the outer layer of the laminate of the present invention described later is described. The biodegradable resin (C) layer is a layer with a biodegradable resin (C) as a main component, preferably containing 70% by mass or more of the biodegradable resin (C), more preferably containing 80% by mass or more, and further preferably containing 90% by mass or more. The upper limit is 100% by mass.

[0225] Examples of the biodegradable resin (C) include polylactic acid (C1), polycondensates of adipic acid / terephthalic acid / 1,4-butanediol (polybutylene adipate-terephthalate (C2)), polycondensates of succinic acid / 1,4-butanediol / lactic acid, aliphatic polyesters such as polyglycolic acid; modified starch; casein plastic; cellulose, etc., and these may be used alone or in combination of two or more.

[0226] Among them, polylactic acid (C1) and polybutylene adipate-terephthalate (C2) are preferred from the viewpoint of strength. Furthermore, a mixture (C3) of polylactic acid (C1) and polybutylene adipate-terephthalate (C2) is preferred from the viewpoint of adhesiveness and strength.

[0227] The polylactic acid (C1) is an aliphatic polyester resin having a lactic acid structural unit as a main component, and is a polymer made from L-lactic acid, D-lactic acid, or L-lactide, D-lactide, or DL-lactide which are cyclic dimers thereof.

[0228] The polylactic acid (C1) used in the present invention is preferably a homopolymer of these lactic acids, and may contain copolymer components other than lactic acids as long as the amount is such that the properties are not impaired, for example, 10 mol% or less.

[0229] Examples of the copolymer component include aliphatic hydroxycarboxylic acids such as glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, and 6-hydroxycaproic acid; lactones such as caprolactone; aliphatic diols such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, and 1,4-butanediol; and aliphatic dibasic acids such as succinic acid, oxalic acid, malonic acid, glutaric acid, and adipic acid.

[0230] In addition, about the content ratio of L-lactic acid component and D-lactic acid component in polylactic acid (C1) (mass of L-lactic acid component / mass of D-lactic acid component), it is preferably used 95 / 5 or more, more preferably 99 / 1 or more, and further preferably 99.8 / 0.2 or more. There is the following tendency: the larger the value, the higher the melting point, and the heat resistance is improved, and conversely, the smaller the value, the lower the melting point, and the heat resistance is insufficient.

[0231] Specifically, in the case of a homopolymer of polylactic acid (C1), the melting point of the one with a content ratio of 95 / 5 is 152°C, the melting point of the one with a content ratio of 99 / 1 is 171°C, and the melting point of the one with a content ratio of 99.8 / 0.2 is 175°C.

[0232] In addition, the weight average molecular weight of the polylactic acid (C1) used in the present invention is preferably 20,000 to 1,000,000, more preferably 30,000 to 300,000, and further preferably 40,000 to 200,000. If the weight average molecular weight is 1,000,000 or less, the melt viscosity during hot melt molding can be suppressed from becoming too high, and good film forming properties can be obtained. In addition, if the weight average molecular weight is 20,000 or more, the mechanical strength of the obtained laminate can be fully obtained.

[0233] The weight average molecular weight can be determined by size exclusion chromatography (GPC, gel permeation chromatography) in the form of polystyrene equivalents according to ISO 16014-1:2012 and ISO 16014-3:2012 using tetrahydrofuran as eluent and a column (polystyrene gel) heated to 40°C.

[0234] Examples of commercially available products of the polylactic acid (C1) include “Ingeo” manufactured by Nature Works, “Lacea” manufactured by Mitsui Chemicals, Inc., “REVODE” manufactured by Zhejiang Hisun Biomaterials Co., Ltd., and “VYLOECOL” manufactured by Toyobo Co., Ltd.

[0235] Polybutylene adipate-terephthalate (C2) is obtained by polycondensing adipic acid, terephthalic acid, and 1,4-butanediol.

[0236] The content of adipic acid in the polybutylene adipate-terephthalate (C2) is preferably 10 to 50 mol%, more preferably 15 to 40 mol%.

[0237] The content of terephthalic acid in the polybutylene adipate-terephthalate (C2) is preferably 5 to 45 mol%, more preferably 8 to 35 mol%.

[0238] The content of 1,4-butanediol in the polybutylene adipate-terephthalate (C2) is preferably 5 to 45 mol%, more preferably 10 to 30 mol%.

[0239] When the content of each component is within the above range, workability and corrosion resistance are improved.

[0240] The weight average molecular weight of polybutylene adipate-terephthalate (C2) is preferably 3,000 to 1,000,000, more preferably 20,000 to 600,000, and even more preferably 50,000 to 400,000.

[0241] The weight average molecular weight can be determined by size exclusion chromatography (GPC, gel permeation chromatography) in the form of polystyrene equivalents according to ISO 16014-1:2012 and ISO 16014-3:2012 using tetrahydrofuran as eluent and a column (polystyrene gel) heated to 40°C.

[0242] When the weight average molecular weight is 3,000 or more, production is easy, and when the weight average molecular weight is 1,000,000 or less, melt viscosity is reduced and moldability is improved.

[0243] The polybutylene adipate-terephthalate (C2) may contain other copolymer components in addition to adipic acid, terephthalic acid and 1,4-butanediol.

[0244] As other copolymer components, there can be listed dihydroxy compounds such as diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol and polytetrahydrofuran (poly-THF); glycolic acid, D-lactic acid, L-lactic acid, D,L-lactic acid, 6-hydroxycaproic acid, and cyclic derivatives thereof, such as glycolide (1,4-dioxane-2,5-dione), D-dilactide, and L-dilactide (3,6-dimethyl-1,4-dioxane-2,5-dione); hydroxycarboxylic acids such as p-hydroxybenzoic acid and oligomers and polymers of p-hydroxybenzoic acid, and the like.

[0245] The content of the other copolymer components is about 0.1 to 30 mol% of the entire polybutylene adipate-terephthalate (C2).

[0246] In addition, a mixture (C3) of polylactic acid (C1) and polybutylene adipate-terephthalate (C2) can also be used.

[0247] As a mixing ratio, polylactic acid / polybutylene adipate-butylene terephthalate (mass ratio) is preferably 10 / 90 to 90 / 10, and more preferably 20 / 80 to 60 / 40.

[0248] In addition, the biodegradable resin (C) layer used in the present invention may contain, in addition to the biodegradable resin (C), a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, an antistatic agent, a flame retardant, a plasticizer, a lubricant, a filler, a lubricant, a crystal nucleating agent, etc.

[0249] [Laminated body]

[0250] The laminate of the present invention has at least one layer containing the acid-modified polyester resin (A) of the present invention (hereinafter sometimes referred to as “acid-modified polyester resin (A) layer”).

[0251] The acid-modified polyester resin (A) layer is a layer containing the acid-modified polyester resin (A) as a main component, and preferably contains 70% by mass or more of the acid-modified polyester resin (A), more preferably 80% by mass or more, and further preferably 90% by mass or more. The upper limit is 100% by mass.

[0252] The acid-modified polyester resin (A) layer used in the present invention may contain, in addition to the acid-modified polyester resin (A) described in the first embodiment or the second embodiment of the present invention, a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, an antistatic agent, a flame retardant, a plasticizer, a lubricant, a filler lubricant, a crystal nucleating agent, etc.

[0253] The laminate of the present invention preferably has a biodegradable resin (C) layer as a layer other than the acid-modified polyester resin (A) layer.

[0254] Among them, in the laminate of the present invention, it is preferred that a PVA-based resin (B) layer be used as the gas barrier layer, and a biodegradable resin (C) layer be used as the outer layer.

[0255] In addition, the laminate of the present invention is preferably a laminate having an adhesive layer provided between the PVA-based resin (B) layer and the biodegradable resin (C) layer, wherein the adhesive layer contains the acid-modified polyester-based resin (A) of the present invention. The laminate preferably has a layer structure of 3 to 15 layers, more preferably 3 to 7 layers, and particularly preferably 5 to 7 layers.

[0256] The structure of the laminate of the present invention is not particularly limited. When the biodegradable resin (C) layer is c, the PVA resin (B) layer is b, and the acid-modified polyester resin (A) layer (adhesive layer) is a, it can be any combination of c / a / b, c / a / b / a / c, c / b / a / b / a / b / c, etc. It should be noted that when there are multiple biodegradable resin (C) layers in the laminate, the multiple biodegradable resin (C) layers can be the same layer or different layers. The case where there are multiple PVA resin (B) layers in the laminate is the same as the case where there are multiple acid-modified polyester resin (A) layers.

[0257] It should be noted that, in order to prevent the gas barrier performance of the PVA-based resin (B) layer from being reduced due to moisture absorption, it is preferred that a biodegradable resin (C) layer be provided in the portion of the PVA-based resin (B) layer that comes into contact with the outside air or contents containing moisture.

[0258] The thickness of the laminate of the present invention is preferably in the range of 1 to 30,000 μm, more preferably 3 to 13,000 μm, and even more preferably 10 to 3,000 μm.

[0259] As the thickness of each layer constituting the laminate, the thickness of the acid-modified polyester resin (A) layer (adhesive layer) is preferably 0.1 to 500 μm, more preferably 0.15 to 250 μm, and particularly preferably 0.5 to 50 μm. If the thickness of the acid-modified polyester resin (A) layer is 500 μm or less, the appearance becomes good. In addition, if the thickness of the acid-modified polyester resin (A) layer is 0.1 μm or more, the decrease in adhesive force can be suppressed.

[0260] In addition, the thickness of the PVA-based resin (B) layer is preferably 0.1 to 1,000 μm, more preferably 0.3 to 500 μm, and even more preferably 1 to 100 μm. If the thickness of the PVA-based resin (B) layer is 1,000 μm or less, it is possible to suppress the laminate from becoming hard and brittle. In addition, if the thickness of the PVA-based resin (B) layer is 0.1 μm or more, the gas barrier properties are improved.

[0261] In addition, the thickness of the biodegradable resin (C) layer is preferably 0.4 to 14,000 μm, more preferably 1 to 6,000 μm, and particularly preferably 4 to 1,400 μm. If the thickness of the biodegradable resin (C) layer is 14,000 μm or less, it is possible to prevent the laminate from becoming too hard. In addition, if the thickness of the biodegradable resin (C) layer is 0.4 μm or more, it is possible to prevent the laminate from becoming brittle.

[0262] In addition, regarding the thickness ratio of the biodegradable resin (C) layer to the PVA-based resin (B) layer (thickness of the biodegradable resin (C) layer / thickness of the PVA-based resin (B) layer), when there are a plurality of layers, the ratio of the total values ​​of their thicknesses is preferably 1 to 100, more preferably 2.5 to 50. If the ratio is 100 or less, the barrier properties are improved, and if the ratio is 1 or more, it is possible to suppress the laminate from becoming hard and brittle.

[0263] In addition, the thickness ratio of the laminate of the present invention to the acid-modified polyester resin (A) layer (adhesive layer) (thickness of the acid-modified polyester resin (A) layer / thickness of the laminate of the present invention) is preferably 0.005 to 0.5, more preferably 0.01 to 0.3, when there are a plurality of acid-modified polyester resin (A) layers (adhesive layers). When the ratio is 0.5 or less, the appearance is improved, and when the ratio is 0.005 or more, the adhesive force is improved.

[0264] In addition, the laminate produced using the acid-modified polyester resin according to the first embodiment of the present invention preferably has a uniform thickness. Specifically, the coefficient of variation of the thickness of the laminate is preferably 0.5 or less. By setting the coefficient of variation of the thickness of the laminate to 0.5 or less, it is possible to suppress poor appearance after stretching. The coefficient of variation of the thickness of the laminate is more preferably 0.3 or less, further preferably 0.2 or less, and particularly preferably 0.1 or less.

[0265] The coefficient of variation of the thickness of the laminate can be measured by the method described in the examples below. In addition, as a method for setting the coefficient of variation of the thickness of the laminate to be within the above range, for example, a method for adjusting the fluidity of the resin of each layer, a method for adjusting the pressure when the resin of each layer merges can be listed.

[0266] The laminate of the present invention can be produced by a conventionally known molding method, and specifically, a melt molding method or a molding method of molding from a solution state can be used.

[0267] For example, as a melt molding method, there can be listed: a method of sequentially or simultaneously melt-extruding and laminating an acid-modified polyester resin (A) and a PVA-based resin (B) on a film or sheet of a biodegradable resin (C); conversely, a method of sequentially or simultaneously melt-extruding and laminating an acid-modified polyester resin (A) and a biodegradable resin (C) on a film or sheet of a PVA-based resin (B); or a method of co-extruding a biodegradable resin (C), an acid-modified polyester resin (A) and a PVA-based resin (B).

[0268] In addition, as a molding method from a solution state, there can be listed a method in which a solution obtained by dissolving an acid-modified polyester resin (A) in a good solvent is applied to a solution of a film or sheet of a biodegradable resin (C), and after drying, the solution is coated with an aqueous solution of a PVA resin (B).

[0269] Among them, from the viewpoint that a laminate having excellent interlayer adhesion can be obtained by manufacturing in one process, a melt molding method is preferred, and a coextrusion method is particularly preferred. Furthermore, when the melt molding method is used, a PVA resin having a 1,2-diol structural unit in the side chain is preferably used as the PVA resin (B).

[0270] Specific examples of the coextrusion method include an inflation method, a T-die method, a multi-manifold die method, a feed block method, and a multi-slot die method. As the shape of the die, a T-die, a round die, and the like can be used.

[0271] The melt molding temperature during melt extrusion is preferably in the range of 190 to 250°C, more preferably 200 to 230°C.

[0272] The laminate of the present invention may be further subjected to a heat-stretching treatment. By the stretching treatment, improvement in strength and improvement in gas barrier properties can be expected.

[0273] In particular, in the laminate of the present invention, when a PVA-based resin having a 1,2-diol structural unit in a side chain is used as the PVA-based resin (B), stretchability becomes good.

[0274] It should be noted that, for the above-mentioned stretching treatment and the like, a known stretching method can be adopted.

[0275] Specifically, examples include uniaxial stretching and biaxial stretching in which the two edges of a multilayer structure sheet are held and expanded; mold forming methods such as deep drawing, vacuum forming, compressed air forming, and vacuum compressed air forming in which a multilayer structure sheet is stretched using a mold; and methods for processing preformed multilayer structures such as parisons using tube stretching and stretch blow molding.

[0276] When the stretching method is intended to produce a film or sheet-shaped product, it is preferable to use a uniaxial stretching method or a biaxial stretching method.

[0277] In addition, in the case of mold forming methods such as deep drawing, vacuum forming, pressure forming, vacuum pressure forming, etc., it is preferred to use a hot air oven, a heater oven, or a combination of the two to uniformly heat the laminate, and stretch it using a chuck, a plug, a vacuum force, a pressure force, etc.

[0278] When the purpose is to form a molded product such as a cup or tray with a drawing ratio (depth of the molded product (mm) / maximum diameter of the molded product (mm)) usually in the range of 0.1 to 3, it is preferred to adopt a mold forming method using a mold for stretching, such as deep drawing, vacuum forming, pressure forming, vacuum pressure forming, etc.

[0279] In the laminate of the present invention thus obtained, for example, strong adhesion exists between any of the biodegradable resin (C) layer and the acid-modified polyester resin (A) layer, and between the PVA resin (B) layer and the acid-modified polyester resin (A) layer.

[0280] In addition, the acid-modified polyester resin (A) of the present invention has excellent biodegradability. Furthermore, the biodegradable resin (C) and the PVA resin (B) are both biodegradable, so the laminate of the present invention having at least one layer of the acid-modified polyester resin (A) also has excellent biodegradability.

[0281] The laminate of the present invention is biodegradable and can therefore be directly disposed of in compost, and can be suitably used in, for example, coffee capsules (coffee bean containers for capsule coffee manufacturers), shrink films, and other food / beverage containers.

[0282] Furthermore, when the laminate of the present invention has a PVA-based resin (B) layer, the PVA-based resin (B) layer may be dissolved in water and removed, and only the remaining water-insoluble resin may be reused.

[0283] Example

[0284] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not limited to the description of the Examples unless it exceeds the gist of the present invention.

[0285] In addition, in an example, "part" and "%" are a mass basis.

[0286] <Test Example 1>

[0287] [Example 1-1]

[0288] [Preparation of acid-modified polyester resin (A)]

[0289] As a raw material polyester resin (A'), 100 parts of adipic acid / terephthalic acid / 1,4-butanediol polycondensate ("Ecoflex C1200" manufactured by BASF), 0.35 parts of maleic anhydride (X), and 0.25 parts of 2,5-dimethyl-2,5-bis(tert-butyloxy)hexane ("PERHEXA 25B" manufactured by NOF Corporation) as a free radical initiator (Y) were dry-blended, melt-kneaded by a twin-screw extruder under the following conditions, extruded into strands and water-cooled, and then cut by a pelletizer to obtain cylindrical pellets of the acid-modified polyester resin (A).

[0290] The content ratio (Y' / X) of the free radical (Y') obtained from the free radical initiator (Y) to the maleic anhydride (X) was 0.96 in terms of molar ratio.

[0291] Twin screw extruder

[0292] Screw diameter (D): 15mm

[0293] Mixing department: one

[0294] Screw length (L) / screw diameter (D): 60

[0295] Screw speed: 650rpm

[0296] Screen: 90 / 90 mesh

[0297] Processing temperature: C1 / C2 / C3 / C4 / C5 / C6 / H = 30 / 160 / 160 / 160 / 160 / 160 / 200°C (C1 to C6 represent the barrels, H represents the head.)

[0298] [Determination of MFR]

[0299] The MFR of the acid-modified polyester resin (A) obtained above was measured by the above-mentioned MFR measurement method.

[0300] [Preparation of PVA-based resin (B)]

[0301] Into a reaction vessel equipped with a reflux condenser, a dropping funnel, and a stirrer, 68.0 parts of vinyl acetate, 23.8 parts of methanol, 8.2 parts of 3,4-diacetoxy-1-butene, and 0.3 mol% (relative to the amount of vinyl acetate charged) of azobisisobutyronitrile were added, and the temperature was raised under a nitrogen stream while stirring to start polymerization. When the polymerization rate of vinyl acetate reached 90%, meta-dinitrobenzene was added to terminate the polymerization, and then unreacted vinyl acetate monomer was removed from the system by blowing methanol vapor to obtain a methanol solution of a copolymer.

[0302] Next, the methanol solution was further diluted with methanol to adjust the concentration to 45%, and then put into a kneader, and a 2% methanol solution of sodium hydroxide was added at a ratio of 10.5 mmol to 1 mol of the total amount of the vinyl acetate structural unit and the 3,4-diacetoxy-1-butene structural unit in the copolymer to perform saponification while maintaining the solution temperature at 35° C. As the saponification proceeded, saponified products precipitated, and when they became granular, they were filtered out, washed thoroughly with methanol, and dried in a hot air dryer to prepare a PVA-based resin (B) having a 1,2-diol structural unit in a side chain represented by the general formula (4′).

[0303] The saponification degree of the obtained PVA-based resin (B) was 99.2 mol % when analyzed by the alkali consumption required for the hydrolysis of residual vinyl acetate and 3,4-diacetoxy-1-butene.

[0304] The average degree of polymerization of the PVA-based resin (B) was 450 when analyzed in accordance with JIS K 6726-1994.

[0305] In addition, the content of 1,2-diol structural units is determined by using 1 When the integrated value measured by H-NMR (300 MHz proton NMR, d6-DMSO solution, internal standard substance; tetramethylsilane, 50° C.) was calculated, it was 6 mol %.

[0306] [Production of laminated body]

[0307] Using polylactic acid (C1) ("Ingeo4032D" manufactured by Nature Works), PVA resin (B), and acid-modified polyester resin (A), a laminate having a three-layer structure of polylactic acid (C1) layer / acid-modified polyester resin (A) layer / PVA resin (B) layer / acid-modified polyester resin (A) layer / polylactic acid (C1) layer was prepared using a three-layer, five-layer multilayer film-making apparatus equipped with three extruders and a 45 cm wide T-die. The thickness of the obtained laminate was 100 μm, the thickness of each layer was 30 μm / 10 μm / 20 μm / 10 μm / 30 μm, and the width of the obtained laminate was 38 cm.

[0308] In addition, the setting temperature of each extruder and roll is as follows.

[0309] Set temperature

[0310] (C1 to C4 represent the barrels, H represents the head, J represents the joint, FD1, 2 represents the front die, and D1 to 3 represent the die.)

[0311] Polylactic acid (C1): C1 / C2 / C3 / C4 / H / J=180 / 190 / 200 / 200 / 200 / 200℃

[0312] PVA resin (B): C1 / C2 / C3 / C4 / H / J=180 / 200 / 210 / 210 / 210 / 210°C

[0313] Acid-modified polyester resin (A): C1 / C2 / H / J=180 / 200 / 210 / 210°C

[0314] Die head: FD1 / FD2 / D1 / D2 / D3=200 / 200 / 200 / 200 / 200℃

[0315] Roller: 60℃

[0316] [Evaluation of the appearance of laminated body]

[0317] The laminated body obtained above was visually observed and evaluated based on the following criteria.

[0318] A (good): No flow marks, good appearance

[0319] B (bad): flow marks occur, poor appearance

[0320] [Evaluation of uniformity of thickness of laminated body]

[0321] The thickness uniformity in the TD direction of the laminate obtained above was evaluated according to the following procedure.

[0322] A dot was made in the center of the laminate in the TD direction, and 17 points were made at intervals of 1 cm from this point toward one end of the end. 17 points were also made from the point in the center toward the end on the opposite side, and 35 points were made for the entire laminate. The thickness of the laminate at each point was measured using a film thickness meter, and the average value and standard deviation were calculated to calculate the coefficient of variation (=standard deviation / average value). The results are shown in Table 2.

[0323] [Example 1-2] to [Example 1-4]

[0324] In the preparation of the acid-modified polyester resin (A) of Example 1-1, the screw speed of the extruder was changed as shown in Table 1. The acid-modified polyester resin (A) was prepared in the same manner as in Example 1-1, and a laminate was prepared. The appearance and thickness uniformity of the obtained laminate were evaluated in the same manner as in Example 1-1. The results are shown in Tables 1 and 2.

[0325] [Comparative Example 1-1] to [Comparative Example 1-2]

[0326] In the preparation of the acid-modified polyester resin (A) of Example 1-1, the screw speed of the extruder was changed as shown in Table 1. The acid-modified polyester resin (A) was prepared in the same manner as in Example 1-1, and a laminate was prepared. The appearance of the obtained laminate was evaluated in the same manner as in Example 1-1. The results are shown in Tables 1 and 2.

[0327] [Table 1]

[0328] Table 1

[0329]

[0330] [Table 2]

[0331] Table 2

[0332] Coefficient of variation of thickness of laminate Example 1-1 0.30 Example 1-2 0.24 Examples 1-3 0.09 Examples 1-4 0.32

[0333] The laminates of Examples 1-1 to 1-4 were excellent in appearance. On the other hand, the laminates of Comparative Examples 1-1 and 1-2 obtained using a polyester resin having a low MFR were poor in appearance.

[0334] In addition, since the coefficient of variation of the thickness of the laminated bodies of Examples 1-1 to 1-4 was sufficiently low at 0.32 or less, it is presumed that a good appearance can be obtained even when the laminated body is subjected to a stretching treatment.

[0335] <Test Example 2>

[0336] [Example 2-1]

[0337] (Preparation of acid-modified polyester resin (A))

[0338] As a raw material polyester resin (A'), 100 parts of adipic acid / terephthalic acid / 1,4-butanediol polycondensate ("Ecoflex C1200" manufactured by BASF), 0.35 parts of maleic anhydride, and 0.25 parts of 2,5-dimethyl-2,5-bis(tert-butyloxy)hexane ("PERHEXA25B" manufactured by NOF Corporation) as a free radical initiator were dry-blended, melt-kneaded by a twin-screw extruder under the following conditions, extruded into strands and water-cooled, and then cut by a pelletizer to obtain cylindrical pellets of acid-modified polyester resin (A). It should be noted that the resin temperature during kneading is the value shown in Table 5.

[0339] Twin screw extruder

[0340] Diameter (D): 69mm,

[0341] Mixing department: one

[0342] Screw length (L) / diameter (D): 42

[0343] Screen: 20 / 110 / 20 mesh

[0344] Discharge (Q): 500kg / hr

[0345] Screw speed (N): 400rpm

[0346] Processing temperature: C1 / C2 / C3 / C4 / C5 / C6 / C7 / C8 / C9 / C10 / C11=30 / 30 / 30 / 30 / 30 / 160 / 160 / 160 / 160 / 160 / 160℃ (C1~C11 represent barrel.)

[0347] The |α| of the acid-modified polyester resin (A) obtained above was calculated based on formula (I) to formula (II). The results are shown in Tables 3 and 5.

[0348] [Table 3]

[0349] Table 3

[0350]

[0351] [Storage stability evaluation]

[0352] The acid-modified polyester resin (A) obtained above was stored at 40° C. for 2 months and evaluated based on the following criteria.

[0353] A (good): |α| is less than 10000, and the storage stability is good

[0354] B (bad): |α| is 10000 or more, storage stability is poor

[0355] [Preparation of PVA-based resin (B)]

[0356] Into a reaction vessel equipped with a reflux condenser, a dropping funnel, and a stirrer, 68.0 parts of vinyl acetate, 23.8 parts of methanol, 8.2 parts of 3,4-diacetoxy-1-butene, and 0.3 mol% (relative to the amount of vinyl acetate charged) of azobisisobutyronitrile were added, and the temperature was raised under a nitrogen stream while stirring to start polymerization. When the polymerization rate of vinyl acetate reached 90%, meta-dinitrobenzene was added to terminate the polymerization, and then unreacted vinyl acetate monomer was removed from the system by blowing methanol vapor to obtain a methanol solution of a copolymer.

[0357] Next, the methanol solution was further diluted with methanol to adjust the concentration to 45%, and then put into a kneader, and a 2% methanol solution of sodium hydroxide was added at a ratio of 10.5 mmol to 1 mol of the total amount of the vinyl acetate structural unit and the 3,4-diacetoxy-1-butene structural unit in the copolymer to perform saponification while maintaining the solution temperature at 35° C. As the saponification proceeded, saponified products precipitated, and when they became granular, they were filtered out, washed thoroughly with methanol, and dried in a hot air dryer to prepare a PVA-based resin (B) having a 1,2-diol structural unit in a side chain represented by the general formula (4′).

[0358] The saponification degree of the obtained PVA-based resin (B) was 99.2 mol % when analyzed by the alkali consumption required for the hydrolysis of residual vinyl acetate and 3,4-diacetoxy-1-butene.

[0359] The average degree of polymerization of the PVA-based resin (B) was 450 when analyzed in accordance with JIS K 6726-1994.

[0360] In addition, the content of 1,2-diol structural units is determined by using 1 When the integrated value measured by H-NMR (300 MHz proton NMR, d6-DMSO solution, internal standard substance; tetramethylsilane, 50° C.) was calculated, it was 6 mol %.

[0361] [Production of laminated body]

[0362] Using polylactic acid (C1) ("Ingeo4032D" manufactured by Nature Works), PVA resin (B), and acid-modified polyester resin (A), a three-type five-layer multilayer film-forming device equipped with three extruders was used to prepare a three-type five-layer laminate having a polylactic acid (C1) layer / acid-modified polyester resin (A) layer / PVA resin (B) layer / acid-modified polyester resin (A) layer / polylactic acid (C1) layer. The thickness of the obtained laminate was 100 μm, and the thickness of each layer was 30 μm / 10 μm / 20 μm / 10 μm / 30 μm.

[0363] In addition, the setting temperature of each extruder and roll is as follows.

[0364] Set temperature

[0365] (C1 to C4 represent the barrels, H represents the head, J represents the joint, FD1, 2 represents the front die, and D1 to 3 represent the die.)

[0366] Polylactic acid (C1): C1 / C2 / C3 / C4 / H / J=180 / 190 / 200 / 200 / 200 / 200℃

[0367] PVA resin (B): C1 / C2 / C3 / C4 / H / J=180 / 200 / 210 / 210 / 210 / 210°C

[0368] Acid-modified polyester resin (A): C1 / C2 / H / J=180 / 200 / 210 / 210°C

[0369] Die head: FD1 / FD2 / D1 / D2 / D3=200 / 200 / 200 / 200 / 200℃

[0370] Roller: 60℃

[0371] [Evaluation of the appearance of laminated body]

[0372] The laminated body obtained above was visually observed and evaluated based on the following criteria.

[0373] A (good): No flow marks, good appearance

[0374] B (bad): flow marks occur, poor appearance

[0375] [Comparative Example 2-1]

[0376] In the preparation of the acid-modified polyester resin (A) of Example 2-1, the discharge amount (Q) during the grafting reaction was changed to 300 kg / hr, and the screw speed (N) was changed to 264 rpm. The acid-modified polyester resin (A) was prepared in the same manner as in Example 2-1 to prepare a laminate. It should be noted that the ratio (Q / N (kg / (hr·rpm)) of the discharge amount (Q (kg / hr)) during the grafting reaction to the screw speed (N (rpm)) and the temperature of the resin are as shown in Table 5. |α| is calculated according to the above formula (I) to formula (II). The results are shown in Table 4. Using the obtained acid-modified polyester resin, the storage stability was evaluated in the same manner as in Example 2-1, and the appearance of the obtained laminate was evaluated. The results are shown in Table 5.

[0377] [Table 4]

[0378] Table 4

[0379]

[0380] [Table 5]

[0381] Table 5

[0382]

[0383] The resin composition of Example 2-1 was excellent in storage stability. In addition, the laminate of Example 2-1 had a good appearance and therefore excellent melt moldability.

[0384] On the other hand, the resin composition of Comparative Example 2-1 obtained by using a polyester resin that did not satisfy |α|<10000 suffered from resin degradation and was inferior in storage stability.

[0385] The present invention is described in detail and with reference to specific embodiments, but it is self-evident to those skilled in the art that various changes and modifications can be made without exceeding the subject matter and scope of the present invention. This application is based on Japanese patent applications (Japanese patent application 2022-051108) filed on March 28, 2022 and Japanese patent applications (Japanese patent application 2022-051567) filed on March 28, 2022, and the contents thereof are incorporated herein by reference.

[0386] Industrial Applicability

[0387] The acid-modified polyester-based resin (A) of the present invention can be suitably used as an adhesive layer between a PVA-based resin (B) layer and a biodegradable resin (C) layer.

[0388] The obtained laminate is biodegradable and can be directly disposed of in compost, and can be suitably used in, for example, coffee capsules (coffee bean containers used by capsule coffee manufacturers), shrink films, and other food / beverage containers.

Claims

1. An acid-modified polyester resin, which is an aliphatic-aromatic polyester resin grafted with an α,β-unsaturated carboxylic acid and / or anhydride (X), wherein the aliphatic-aromatic polyester resin comprises an aliphatic diol unit, an aliphatic dicarboxylic acid unit and an aromatic dicarboxylic acid unit, The melt flow rate (210° C., load 2160 g) of the acid-modified polyester resin is 1.4 to 15 g / 10 min, and the content of the α,β-unsaturated carboxylic acid and / or its anhydride (X) is 0.0001 to 0.8 parts by mass based on 100 parts by mass of the aliphatic-aromatic polyester resin. 2 . The acid-modified polyester resin according to claim 1 , comprising 50 mol % or more of the aliphatic diol unit and the aliphatic dicarboxylic acid unit in total. 3 . The acid-modified polyester resin according to claim 1 , further comprising a radical initiator (Y) during grafting.

4. The acid-modified polyester resin according to claim 3, wherein The content ratio (Y' / X) of the free radical (Y') obtained from the free radical initiator (Y) to the α,β-unsaturated carboxylic acid and / or its anhydride (X) is 0.5 to 5 in terms of molar ratio.

5. An acid-modified polyester resin, characterized in that: When the MFR change rate coefficient K is plotted for each storage temperature based on the following formula (II), the temperature dependence coefficient α obtained satisfies the following formula (III): The MFR change rate coefficient K is calculated by plotting the change in MFR (melt flow rate) over time when the product is stored at a plurality of temperatures using the following formula (I): MFR(t)=MFR(0)×e^(-K×t)…(I) ln(K)=α / T+β…(II) |a| <10000…(III) In the above formula (I), MFR(t) represents the MFR (210°C, 2160 g load) of the resin after t days from storage, MFR(0) represents the MFR (210°C, 2160 g load) of the resin at the beginning of storage, K represents the MFR change rate coefficient, t represents the time (days) elapsed from storage, In the above formula (II), T represents the storage temperature (K), β represents a constant term, In the above formula (II) and formula (III), α represents the temperature dependency coefficient of the MFR change rate coefficient.

6. The acid-modified polyester resin according to claim 5, which has at least one structural unit selected from the structural units represented by the following general formulae (1) to (3): In formula (1), l is an integer from 2 to 8, In formula (2), m is an integer from 2 to 10, In formula (3), n is an integer of 2 to 9. 7 . The acid-modified polyester resin according to claim 6 , which has a total of 50 mol % or more of at least one structural unit selected from the structural units represented by the general formulae (1) to (3). 8 . The acid-modified polyester resin according to claim 5 , wherein an α,β-unsaturated carboxylic acid and / or anhydride thereof is grafted onto the polyester resin. 9 . A biodegradable adhesive comprising the acid-modified polyester resin according to claim 1 . 10 . A laminate comprising at least one layer comprising the acid-modified polyester resin according to claim 1 .

11. A laminated body comprising an adhesive layer provided between a polyvinyl alcohol-based resin (B) layer and a biodegradable resin (C) layer, The adhesive layer contains the acid-modified polyester resin according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polylactic acid gas barrier film

    JP2000177072A

  • Biodegradable laminate

    JP2009196287A

  • Biodegradable laminate

    JP2013212682A

  • Drilling fluid modifier and drilling fluid using the same

    JP2015143356A

  • Semiconductor device and semiconductor storage

    JP2022051108A