Method for extracting vanadium from petroleum coke ash
The method addresses inefficiencies in existing vanadium extraction from petroleum coke ash by using sulfuric acid and sulfite salts at controlled temperatures and pH for high vanadium recovery rates, reducing energy and reagent use, and simplifying waste management.
Patent Information
- Application Number
- CN202380023116.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-26
- Filing Date
- 2023-03-17
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for extracting vanadium from petroleum coke ash are energy-intensive, require high amounts of concentrated acids and additional reagents, and are inefficient for both vanadium-poor and vanadium-rich ashes, necessitating additional concentration operations and equipment.
Leaching petroleum coke ash with a sulfuric acid solution at 20-50°C for 2 hours, using sodium sulfite, calcium sulfite, or ammonium sulfite as reducing agents to convert vanadium (+5) to vanadium (+4), followed by precipitation with soda ash or caustic soda at pH 6-8, omitting oxidative roasting and using less expensive reagents.
Achieves high extraction rates of 97-99.7% vanadium into solution, reducing energy and material costs, and simplifying waste disposal, while effectively processing both vanadium-poor and vanadium-rich ashes without additional concentration steps.
Smart Images

Figure BDA0005005167900000041
Abstract
Description
[0001] The invention relates to process chemistry and nonferrous metallurgy and can be used to extract vanadium from petroleum coke ash.
[0002] Traditional methods involve leaching vanadium directly from pre-treated petroleum coke or from the ash produced by the combustion of petroleum coke.
[0003] A method for extracting vanadium from petroleum coke (patent RU No. 2647725, IPC C22B 34 / 22, C22B 3 / 06, C22B 7 / 00, published on March 19, 2018, Bulletin No. 8), comprising crushing the petroleum coke to a particle size of 0.100 mm and leaching, wherein the leaching is carried out under the following conditions: using a mixture of concentrated sulfuric acid and nitric acid in a ratio of 1:1, at a temperature of 95°C to 105°C, with a mixture of petroleum coke and acid in a ratio of 1:3 to 3:1 for 1 to 2 hours.
[0004] The disadvantages of this process include high energy cost of maintaining the temperature of the mixture of petroleum coke and acid in the ratio of 1:3 to 3:1 at 95°C to 105°C for 1 to 2 hours and high material cost of large amounts of concentrated acid. Another disadvantage is that it is a great challenge to use the petroleum coke treated with concentrated acid as fuel for further combustion.
[0005] Another method for extracting vanadium and nickel from coke for demetallization of petroleum raw materials (patent RU No. 2685290, IPC C22B 34 / 22, C22B 7 / 00, C01G 31 / 00, C01G 53 / 10, published on April 17, 2019, Bulletin No. 11), comprising crushing a raw material containing an alkali metal salt, oxidative roasting, leaching by heating with water and extracting vanadium and nickel compounds in sequence, wherein the crushing is carried out with 0.1-0.3wt.% of manganese dioxide, crushed to particles with a size not exceeding 0.05mm; 8-10wt.% of sodium chloride and 0.5-1.0wt.% of sodium carbonate are used as alkali metal salts; ammonium nitrate solution is used for granulation before oxidative roasting; oxidative roasting is carried out in four stages according to temperature conditions:
[0006] 1) Heat and dry from 20℃ to 150-200℃,
[0007] 2) Pre-calcined from 150-200℃ to 650℃,
[0008] 3) Calcination at a constant temperature of 850°C,
[0009] 4) Cooling from 850°C to 120°C.
[0010] In the oxidant H 2 O 2In the presence of vanadium, vanadium and nickel compounds are extracted by leaching with water having a S:L ratio of 1:2.0-2.5 and a sulfuric acid solution having a S:L ratio of 1:1-2.5. The water and the acid leaching solution are mixed to extract vanadium and nickel compounds.
[0011] The disadvantages of this method include: high energy costs for maintaining the temperature, especially the calcination temperature of 850°C, large amounts of hydrogen peroxide (H 2 O 2 ) and the need to introduce a complex mixture of sodium chloride, manganese dioxide and nitrates into the charge prior to roasting.
[0012] As far as ash preparation is concerned, the method closest to the present invention is the method of extracting metals from refining residues (patent RU No. 2578891, IPC C22B 26 / 20, C22B 7 / 00, C22B 3 / 04, published on March 27, 2016, Bulletin No. 9). This method involves burning petroleum coke at a temperature of up to 900°C and using the heat generated in the energy field. Vanadium (+5) and molybdenum (+6) are extracted from the resulting ash by oxidative leaching using a caustic soda solution to which hydrogen peroxide is added and leaching nickel with sulfuric acid from the formed filter cake. Ammonium vanadate and ammonium polymolybdate are selectively precipitated from the alkaline production solution by adjusting the pH with an acid and adding ammonium sulfate. Nickel is precipitated in the form of hydroxide by neutralizing the sulfuric acid solution with magnesium oxide.
[0013] The disadvantages of this method include: high energy costs for maintaining temperature, large reagent consumption, complex waste liquor composition, and the need for additional equipment and space for its disposal. In addition, this method is relatively effective only when treating metal-rich ash and obtaining an alkaline solution rich in vanadium and molybdenum, because precipitation of ammonium vanadate and ammonium polymolybdate at an acceptable extraction rate is only feasible from the rich solution.
[0014] The object of the present invention is to provide a method for extracting vanadium from ash, which ensures that vanadium is extracted from both vanadium-poor ash and vanadium-rich ash at a high rate into solution, improves the performance of the method by omitting preliminary oxidation roasting and other additional vanadium oxidation operations, and reduces energy and material costs by extracting vanadium under optimal process conditions without the need for additional reagents and equipment.
[0015] This object is achieved by a method for extracting vanadium from petroleum coke ash, which method comprises leaching the petroleum coke ash and then extracting the vanadium from the production solution.
[0016] The novelty of the present invention is that the leaching is carried out using a sulfuric acid solution with a concentration of 20 to 50 g / l at a temperature of 20 to 50° C. for 2 hours. The leaching includes adding sodium sulfite, calcium sulfite, or ammonium sulfite in an amount of 80 to 140% of the sulfite ion content of the vanadium content in the ash; and the extraction of vanadium from the production solution includes precipitating vanadium hydroxide (+4) during the neutralization of the resulting solution with soda ash or caustic soda to a pH of 6 to 8.
[0017] Another novelty is that sodium sulfite salt having an active sulfite ion content of 57-63% is used as sodium sulfite.
[0018] Another novelty is that calcium sulfite salt having an active sulfite ion content of 40-66% is used as calcium sulfite.
[0019] Another novelty is that an ammonium sulfite-ammonium bisulfite solution having an active sulfite ion content of 12-40% is used as the ammonium sulfite.
[0020] To implement the method, the following materials were used:
[0021] Sodium sulfite, an inorganic compound, sodium salt of sulfurous acid, chemical formula Na2SO3, GOST 5644-75, used as a reducing agent for vanadium (+5), active sulfite ion content is 57-63%.
[0022] Calcium sulfite is an inorganic compound, the calcium salt of sulfurous acid, with the chemical formula CaSO 3 , a precipitate with an active sulfite ion content of 40-66%.
[0023] Ammonium sulfite, using ammonium sulfite-ammonium bisulfite technical solution (due to its instability in dry form), containing different proportions of qualified ammonium sulfite (NH 4 ) 2 SO 3 and ammonium bisulfite NH 4 HSO 3 , calculated as sulfite ion, the solution has a pH of 4.6-6.8 and an active sulfite ion content of 12-40%.
[0024] Commercial sulfuric acid according to GOST 2184-2013 2 SO 4 , used to prepare solutions when leaching vanadium.
[0025] Caustic soda Na in dry form or as a 20% solution according to GOST 5100-85 2 CO 3 , or caustic soda according to GOSTR55064-2012.
[0026] The method for extracting vanadium from petroleum coke ash of the present invention comprises: leaching the petroleum coke ash and then extracting vanadium from the production solution.
[0027] Leaching is carried out with a sulfuric acid solution with a concentration of 20-50 g / l (pH 0.7-0.8) at a temperature of 20°C to 50°C for 2 hours, during which sulfites: sodium sulfite or calcium sulfite or ammonium sulfite are added to the suspension as a reducing agent for vanadium (+5) to vanadium (+4).
[0028] The selected leaching conditions, i.e. a sulfuric acid concentration range of 20-50 g / l, ensure that vanadium is transferred to the solution in the form of stable and soluble vanadyl ions VO 2+, in which vanadium has an oxidation state of +4. Sulfuric acid concentrations above 50 g / l are excessive, while concentrations below 20 g / l may result in the presence of aggregated forms of vanadium (+5) in the solution, which may adversely affect the integrity of the subsequent extraction of vanadium from the sulfuric acid.
[0029] The leaching temperature of 20-50°C provides the required rate of vanadium reduction by sulfite ions on the one hand, and on the other hand provides sufficient solubility of sulfite ions to prevent the distillation of sulfur dioxide. The temperature range of the present invention can produce the maximum concentration of reducing agent-sulfite ions in the solution, and the loss of the side process enhanced with the increase of temperature is minimal.
[0030] In order to effectively consume the reducing agent - sodium sulfite, calcium sulfite or ammonium sulfite, it is recommended to introduce it into the process in an amount of 80%-140% of the sulfite ion content of the vanadium content in the ash. This amount is necessary and sufficient to achieve the amount required to extract the vanadium into solution. At lower amounts, the required completeness of vanadium (+5) recovery cannot be achieved, and the amount of vanadium extracted into solution will also be reduced. Due to the high content of sulfite ions, part of the reagent is not consumed by the ash. The excess material generated decomposes in an acidic environment to form sulfur dioxide, which is distilled into the gas phase and pollutes the environment.
[0031] Two hours of leaching are sufficient, during which the sodium sulfite, or calcium sulfite, or ammonium sulfite reacts with the vanadium (+5) and other components in the ash, ensuring that the sulfite ions are completely consumed and eliminating the leakage of unconsumed sulfur dioxide.
[0032] By using low soluble vanadium hydroxide V(OH) 4 Vanadium (+4) is extracted from the resulting production solution by precipitating it in the form of vanadium (+4). Maximum integrity of the vanadium precipitation can be achieved by neutralizing the solution to a pH of 6-8 with soda ash or caustic soda.
[0033] If the initial ash contains molybdenum and nickel, these metals are also transferred to the solution during the vanadium leaching process. Molybdenum is selectively extracted from the production solution by adsorption on a weakly basic anion exchanger according to conventional methods before the vanadium is deposited, and nickel is also deposited in the form of basic carbonates by raising the pH to 9-10 with soda according to conventional methods after the vanadium has been deposited.
[0034] Compared with the existing method of extracting vanadium from fuel ash or coke ash, the method of extracting vanadium from petroleum coke ash of the present invention can omit the operation of oxidative roasting of ash, leaching vanadium with soda or alkali solution in the presence of oxidant, hydrogen peroxide, and the complicated scheme of extracting vanadium from the alkali or soda solution used for leaching.
[0035] During the combustion of petroleum coke, depending on the degree of completeness of combustion, ash with different contents of vanadium and other components may be produced: inferior ash (where the content of useful components (metals) is not high, so when such ash is treated by conventional methods, additional vanadium concentration operations are required) and relatively rich ash (no additional concentration is required). The following table shows the typical composition. Sample No. 2 is the most representative component of inferior ash.
[0036] When the ash is leached with the presence of sodium sulfite or calcium sulfite or ammonium sulfite, high extraction rates of vanadium into solution are achieved from both vanadium-poor and vanadium-rich ashes. When the subsequent precipitation of vanadium is carried out under selected conditions, high vanadium precipitation rates are achieved for both lean and rich solutions (unlike the closest approach where it is difficult to precipitate ammonium vanadate from lean solutions without concentration). The resulting precipitate enriched in vanadium (+4) hydroxide can be processed to vanadium pentoxide by conventional methods.
[0037] The method is implemented using a specific implementation example, in which samples have different contents of vanadium and other components, the compositions of which are given in the table.
[0038] The content of main components in the ash sample
[0039] Example
[0040] Example 1: A 100 g portion of crushed petroleum coke ash sample No. 1 was mixed with 500 ml of a 50 g / l sulfuric acid solution in a reactor at a temperature of 30° C. During leaching, sodium sulfite containing 58.4% active sulfite ions was added to the suspension. The total consumption of sodium sulfite was 1.46 g (corresponding to 140% of the sulfite ions of the vanadium content in the ash sample, and the vanadium V content in the first sample portion was 0.61%).
[0041] Therefore, if a 100 g portion contains 0.61 g of vanadium, the amount of sulfite ions is 0.61 x 140 / 100 = 0.854 g. When the sulfite ion content in sodium sulfite is 58.4%, the amount of sodium sulfite is 0.854 x 100 / 58.4 = 1.46 g.
[0042] The process takes 2 hours. The calcined ash is added to the filtered solution after leaching with a vanadium content of 1.1 g / l until the solution reaches a pH of 8. The resulting vanadium hydroxide (+4) precipitate is filtered out and dried. The residual content of vanadium in the filtered solution is 0.03 g / l. The recovery rate in the precipitation stage is 97.3%. The yield of vanadium precipitation is 2.2 g, of which the vanadium content is 27.3%. After washing with sulfuric acid solution, the residual content of vanadium in the leached cake is 0.07%, corresponding to 88.5% of the vanadium extracted into the solution during the leaching process. The total extraction rate of vanadium is 86.1%.
[0043] Example 2: A 100 g portion of crushed petroleum coke ash sample No. 2 was mixed with 500 ml of a sulfuric acid solution with a concentration of 20 g / l in a reactor at a temperature of 20°C. During the leaching process, sodium sulfite with a sulfite ion content of 58.4% was added to the suspension. The total consumption of sodium sulfite was 10.1 g (corresponding to 140% of the sulfite ions of the vanadium content, which was equal to 4.22% in the second sample portion). The process took 2 hours. Under stirring, caustic soda was added to the filtered solution after leaching with a vanadium content of 8.23 g / l until the solution pH reached 7.6. The resulting vanadium hydroxide (+4) precipitate was filtered out and dried. The residual content of vanadium in the filtered solution was 0.03 g / l. The recovery rate of the precipitation stage was 99.6%. The yield of vanadium precipitate was 11.76 g, of which the vanadium content was 34.3%. The residual content of vanadium in the cake after ash leaching was 0.056%. The total extraction of vanadium to product was 98.0%.
[0044] Example 3: A 100 g portion of crushed petroleum coke ash No. 3 sample was mixed with 500 ml of a sulfuric acid solution with a concentration of 45 g / l at a temperature of 50°C. Sodium sulfite with a sulfite ion content of 58.4% was added to the suspension. The total consumption of sodium sulfite was 29 g (equivalent to 140% of the sulfite ions of the vanadium content in the ash, and the content of vanadium V in the third sample was 12.1%). The process took 2 hours. In the filtered solution after leaching with a vanadium content of 23.8 g / l, caustic soda was added under stirring until the solution pH reached 6. The resulting precipitate was filtered out and dried. The yield of vanadium was 26.7 g, and the vanadium content was 50.19%. The residual content of vanadium in the solution after precipitation was 0.064 g / l, and the extraction rate during precipitation was 99.7%. The residual content of vanadium in the cake after leaching was 0.21%. The extraction rate to the solution was 98.3%. The total extraction rate of vanadium to the product was 98.0%.
[0045] Example 4: A 100 g portion of crushed petroleum coke ash No. 3 sample was mixed with 500 ml of a sulfuric acid solution with a concentration of 45 g / l at a temperature of 50°C. Sodium sulfite with a sulfite ion content of 58.4% was added to the suspension. The total consumption of sodium sulfite was 18.1 g (corresponding to 87.6% of the vanadium content in the ash, and the content of vanadium V in the third sample portion was 12.1%). The process took 2 hours. Under stirring, caustic soda was added to the filtered solution after leaching with a vanadium content of 22.9 g / l until the solution pH reached 6. The resulting precipitate was filtered out and dried. The yield of vanadium was 23.0 g, and the vanadium content was 48.7%. The residual content of vanadium in the solution after precipitation was 0.072 g / l, and the extraction rate during precipitation was 99.7%. The residual content of vanadium in the cake after leaching was 0.64%. The extraction rate to the solution was 94.7%. The total extraction rate of vanadium to the product was 94.4%.
[0046] Example 5: A 100 g portion of a crushed petroleum coke ash sample No. 2 was mixed with 500 ml of a sulfuric acid solution having a concentration of 35 g / l in a reactor at a temperature of 20°C. During the leaching process, an ammonium sulfite solution having a sulfite ion concentration of 18% was added to the suspension. The total consumption of sulfite ions was 3.4 g (80% of the amount of vanadium in this portion), corresponding to an amount of 18.7 g of ammonium sulfite-ammonium bisulfite solution. The process took 2 hours. Under stirring, caustic soda was added to the filtered solution after leaching with a vanadium content of 8.04 g / l until the solution pH reached 7.6. The resulting vanadium hydroxide (+4) precipitate was filtered out and dried. The residual content of vanadium in the filtered solution was 0.03 g / L. The extraction rate during the precipitation process was 99.6%. The yield of the vanadium precipitate was 11.9 g, with a vanadium content of 33.9%. The residual content of vanadium in the cake after ash leaching was 0.2%. The total extraction of vanadium to product was 94.9%.
[0047] Example 6: A 100 g portion of crushed petroleum coke ash No. 2 sample was mixed with 500 ml of a 50 g / l sulfuric acid solution in a reactor at a temperature of 20°C. During the leaching process, an ammonium sulfite solution with a sulfite ion concentration of 18% was added to the suspension. The total consumption of sulfite ions was 5.9 g (140% of the vanadium content in the ash, 4.22% in the second sample portion), which was contained in 32.8 g of ammonium sulfite-ammonium bisulfite solution. The process took 2 hours. Under stirring, caustic soda was added to the filtered solution after leaching with a vanadium content of 8.23 g / l until the solution pH reached 7.6. The resulting vanadium hydroxide (+4) precipitate was filtered out and dried. The residual content of vanadium in the filtered solution was 0.03 g / L. The recovery during precipitation was 99.6%. The yield of vanadium precipitate was 12.3 g, with a vanadium content of 33.1%. The residual vanadium content in the cake after ash leaching was 0.12%. The total extraction rate of vanadium to product was 97.2%.
[0048] Example 7: A 100 g portion of crushed petroleum coke ash No. 2 sample was mixed with 500 ml of a 50 g / l sulfuric acid solution in a reactor at a temperature of 40°C. During the leaching process, calcium sulfite with a sulfite ion content of 52% was added to the suspension. The total consumption of sulfite ions was 5.06 g (120% of the vanadium content in the ash sample and 4.22% in the second sample portion), which was contained in 9.74 g of industrial calcium sulfite. The process took 2 hours. Under stirring, caustic soda was added to the filtered solution after leaching with a vanadium content of 8.15 g / l until the solution pH reached 6.6. The resulting vanadium hydroxide (+4) precipitate was filtered out and dried. The residual content of vanadium in the filtered solution was 0.03 g / L. The recovery during precipitation was 99.6%. The yield of vanadium precipitate was 12.6 g, with a vanadium content of 32.0%. The residual content of vanadium in the cake after ash leaching was 0.145%. The total extraction rate of vanadium from ash to sediment was 96.2%.
[0049] The above examples show that when the ash is leached in the presence of sodium sulfite or calcium sulfite or ammonium sulfite, high extraction rates of vanadium into solution are achieved from both vanadium-poor and vanadium-rich ashes. In the subsequent vanadium precipitation process under selected conditions, high vanadium precipitation is achieved in both lean and rich solutions. The resulting enriched vanadium hydroxide (+4) precipitate can be processed into vanadium pentoxide by conventional methods.
[0050] The method of extracting vanadium from ash of the present invention ensures that vanadium is extracted into solution at a high rate: the vanadium precipitation (extraction) rate is 97-99.7%, and the total amount of vanadium extracted into the precipitate from the petroleum coke ash is 86-98%. The performance of the method is improved (the total time spent on implementing the method is reduced) by omitting the preliminary oxidation roasting of vanadium and other additional oxidations. In addition, the method of extracting vanadium from petroleum coke ash of the present invention can significantly save material resources by eliminating the high consumption of expensive reagents (caustic soda, ammonium salts and hydrogen peroxide) and additional equipment, the ability to neutralize the resulting solution with cheap soda, and the ability to extract vanadium from rich and lean ash without compromising the efficiency of extracting vanadium. In addition, the problem of disposal of waste solution with uncomplicated composition is greatly simplified compared to the closest method.
Claims
1. A method for extracting vanadium from petroleum coke ash, the method comprising: include: Leaching the petroleum coke ash and then extracting vanadium from the production solution, characterized in that the leaching is carried out with a sulfuric acid solution with a concentration of 20 to 50 g / l at a temperature of 20 to 50° C. for 2 hours; the leaching process includes: adding sodium sulfite, or calcium sulfite, or ammonium sulfite, 80-140% of the sulfite ion content of the vanadium content in the ash, and the extraction of vanadium from the production solution includes: precipitating vanadium hydroxide (+4) during the process of neutralizing the resulting solution with soda ash or caustic soda to a pH of 6-8.
2. The method for extracting vanadium from petroleum coke ash according to claim 1, It is characterized in that Sodium sulfite salt with an active sulfite ion content of 57-63% is used as the sodium sulfite.
3. The method for extracting vanadium from petroleum coke ash according to claim 1, It is characterized in that Calcium sulfite salt with an active sulfite ion content of 40-66% is used as the calcium sulfite.
4. The method for extracting vanadium from petroleum coke ash according to claim 1, It is characterized in that An ammonium sulfite-ammonium bisulfite solution having an active sulfite ion content of 12-40% is used as the ammonium sulfite.