Novel duplex stainless steel
By adjusting the element composition and heat treatment process of duplex stainless steel, the coverage of quenched nitrides in ferrite grain boundaries is reduced and the formation of σ phase is avoided, which solves the problem of insufficient strength and corrosion resistance of duplex stainless steel in high pressure environments, and achieves the realization of High strength and durability improvement.
Patent Information
- Application Number
- CN202380033683.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-12
- Filing Date
- 2023-04-11
- Publication Date
- 2024-12-06
AI Technical Summary
Existing duplex stainless steels are prone to insufficient strength and corrosion resistance in high pressure environments, especially in the welding process, which may form σ phase and cause cracks, and the increase in weight leads to an increase in failure risk.
By adjusting the element composition and heat treatment process, a duplex stainless steel with high Cr content, W content and N content is prepared to ensure low coverage of quenched nitride in the ferrite grain boundary, avoid the formation of σ phase, and thus improve corrosion resistance and strength.
The high strength and corrosion resistance of duplex stainless steel in high pressure environments are achieved, the σ phase content of the heat-affected zone after welding is reduced, and the durability and impact toughness of the material are improved.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a duplex stainless steel with high Cr content, W content and N content. Background Art
[0002] Today, oil wells are being run at increasing pressures, and there are plans to develop wells with pressures of 20 kpsi. Offshore, long liner pipes, also called umbilicals, typically connect surface and subsea equipment. These umbilicals contain pipes for hydraulic and chemical injection into the seafloor, as well as signal lines for electrical and fiber optic signals and power. The umbilical pipes consist of long pipes that may be welded together.
[0003] Super duplex stainless steels with PRE greater than 40, i.e. austenitic-ferritic iron-chromium-nickel alloys with added molybdenum, have been used because these steels will provide adequate pitting resistance and mechanical strength for conventional subsea wells. However, for deeper wells, the pressure will increase significantly, which means that the umbilicals must be able to withstand higher internal pressures. This in turn means that the wall thickness of the umbilicals must be increased in order to withstand the higher pressures. As a result, these pipes will face the problem of increased weight leading to an increased probability of failure, because today's duplex stainless steels are not strong enough to carry their own weight when the wall thickness is increased to meet the higher pressure requirements. In addition, in some future applications, today's duplex stainless steels may not have sufficient corrosion resistance and there may be problems with the formation of sigma phases during welding, especially in the heat-affected zone. This will cause very large problems when manufacturing umbilicals, as these pipes may contain a large number of weld joints that can form cracks.
[0004] Therefore, there is a need for a new duplex stainless steel that will have high strength and high corrosion resistance both as stainless steel itself and when used for welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] The present disclosure is further illustrated by the following non-limiting drawings:
[0006] Figure 1A 0.05 mm for material 7 is shown 2 Photos of LOM in representative sites;
[0007] Figure 1B Shows the Figure 1A Same but also shows 0.05 mm 2 LOM photographs of 10 randomly oriented test lines in a representative site;
[0008] Figure 2A 0.05 mm for material 8 is shown 2 Photos of LOM in representative sites;
[0009] Figure 2B Shows the Figure 2A Same but also shows 0.05 mm 2 LOM photographs of 10 randomly oriented test lines in a representative site;
[0010] Figure 3A 0.05 mm for material 13 is shown 2 Photos of LOM in representative sites;
[0011] Figure 3B Shows the Figure 3A Same but also shows 0.05 mm 2 LOM photographs of 10 randomly oriented test lines in a representative site;
[0012] Figure 4A 0.05 mm of material 14 is shown 2 Photos of LOM in representative sites;
[0013] Figure 4B Shows the Figure 4A Same but also shows 0.05 mm 2 LOM photographs of 10 randomly oriented test lines in a representative site;
[0014] Figure 5A 0.05 mm for material 9 is shown 2 Photos of LOM in representative sites;
[0015] Figure 5B Shows the Figure 5A Same but also shows 0.05 mm 2 LOM photograph of 10 randomly oriented test lines in a representative site. DETAILED DESCRIPTION
[0016] The present disclosure provides a duplex stainless steel having a combination of high strength and excellent corrosion resistance because the duplex stainless steel in its final form has low coverage of quenched-in nitrides in the ferrite grain boundaries and is substantially free of any sigma phase in the steel itself and in the heat affected zone when exposed to welding. Low coverage of quenched-in nitrides in the ferrite grain boundaries will increase corrosion resistance and impact resistance. In addition, low levels of sigma phase will increase corrosion resistance. Both of these properties are important for the durability of the product when in service, such as when used in a tube in an umbilical. The term "final form" means that the duplex stainless steel of the present invention has been exposed to the metallurgical processes necessary for use in different applications. Therefore, the duplex stainless steel of the present invention, as defined below, will contain little or substantially no sigma phase in the duplex stainless steel itself and in the heat affected zone (HAZ) after welding, and in addition, will have low coverage of quenched-in nitrides in the ferrite grain boundaries after solution annealing and quenching.
[0017] Therefore, the present disclosure relates to a duplex stainless steel having the element ranges disclosed below.For the duplex stainless steel of the present invention, the inventors have carefully adjusted the elements to be used and the ranges of these elements to obtain a duplex stainless steel having the properties mentioned above or below.
[0018] Thus, the duplex stainless steel of the present invention therefore comprises the following elements (in wt %):
[0019] C max 0.030;
[0020] Si max 0.30;
[0021] Mn 0.20 to 2.50;
[0022] P max 0.030;
[0023] S max 0.030;
[0024] Cr28.5 to 30.5;
[0025] Ni6.0 to 8.0;
[0026] Mo0.70 to 3.00;
[0027] W2.00 to 4.40;
[0028] Cu max 0.50;
[0029] N0.30 to 0.55;
[0030] The balance is Fe and unavoidable impurities;
[0031] The ferrite content is 40 volume % to 60 volume %;
[0032] The duplex stainless steel meets the following requirements:
[0033] a. [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5, wherein the values of [Cr], [Mo] and [W] are in weight %; and
[0034] b) In the solution annealed state, the coverage of quenched nitrides in the ferrite grain boundaries is less than 10%.
[0035] Therefore, in other words, the duplex stainless steel of the present invention has low coverage of quenched nitrides in the ferrite grain boundaries after solution annealing followed by quenching. The coverage of quenched nitrides in the ferrite grain boundaries was measured according to the method described in Example 4. In addition, the duplex stainless steel of the present invention will resist the formation of sigma phase in the heat affected zone (HAZ) due to its composition and will therefore be substantially free of any sigma phase.
[0036] In the present disclosure, the term "solution annealed state" means a state obtained after heat treating the duplex stainless steel of the present invention for the purpose of solution annealing, cooling from the solution annealing temperature to a temperature of about 900°C to about 1000°C, and then quenching. In addition, in the present disclosure, the term "solution annealed" is intended to include heat treatment and cooling from the solution annealing temperature to a temperature between about 900°C and about 1000°C.
[0037] In this disclosure, the term "quench nitride" refers to nitrides formed at ferrite grain boundaries when steel is rapidly cooled, and will precipitate in the ferrite grain boundaries because the elements do not have time to migrate between phases. The coverage of quench nitrides in ferrite grain boundaries is measured according to the method described in the Examples.
[0038] Therefore, the inventors have found that in order to obtain the properties of the duplex stainless steel of the present invention, it is important to balance the elements that affect the formation of the σ phase during welding, because the σ phase has a negative impact on the strength. Therefore, the inventors have found that if the following conditions are met:
[0039] [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5 (Formula 1),
[0040] Where the values are expressed in wt %, the σ phase content of the duplex stainless steel of the present invention will be low, i.e., when it is cooled from the solution annealing temperature to room temperature at a cooling rate of 40°C / min, the σ phase content will be less than 0.2% by volume, as shown in the Examples, Table 2. This in turn means that the content of σ phase in the HAZ after welding will be low or substantially zero. Therefore, this low content of σ phase means that the strength and impact toughness of the duplex stainless steel when it is used as a base metal (e.g., in the form of a tube or tubular body) or as a welding material will be high. In addition, since the brittleness is reduced due to the low content of σ phase in the heat affected zone, the impact toughness and strength will be increased.
[0041] According to the present disclosure, Formula 1 may also satisfy the following: 40 < [Cr] + 4.0*[Mo] + 2.0*[W] < 42.
[0042] The ferrite content of the duplex stainless steel of the present invention is between 40 volume % and 60 volume %, and the rest is basically composed of austenite. If the ferrite content is too low, the mechanical strength will be too low, and if the ferrite content is too high, the corrosion performance will deteriorate. For example, if the ferrite content is too high, the resistance to hydrogen induced cracking will deteriorate. According to an embodiment, the ferrite content is at least 44 volume %, and the rest is basically austenite. Phase balance is important in duplex stainless steel because it helps to obtain optimal mechanical properties and corrosion resistance. In addition, the ferrite content of the duplex stainless steel of the present invention has been adjusted so that the phase balance in the heat affected zone is still within an acceptable range. This is important because the ferrite content in the heat affected zone tends to increase, which will have a negative impact on mechanical properties and corrosion resistance.
[0043] During solution annealing and subsequent quenching, as described above, the quench nitrides formed in the ferrite grain boundaries will have a negative impact on corrosion resistance and mechanical properties. Therefore, it is important to avoid the formation of these quench nitrides. The inventors of the present invention have found that the duplex stainless steel of the present invention has a specific element range as defined above or below, and in the solution annealed state, the coverage of the quench nitrides in the ferrite grain boundaries is low (less than 10%). Therefore, according to the present disclosure, the low coverage of the quench nitrides in the ferrite grain boundaries means that the percentage of ferrite grain boundaries covered by quench nitrides is less than 10%. In the case of typical expected grain sizes in the finished product of the duplex stainless steel of the present invention, a quench nitride coverage of the ferrite grain boundaries of 10% will correspond to an extremely low fraction of quench nitrides in the material as a whole. Therefore, less than 10% of the ferrite grain boundaries covered by quench nitrides are considered to be low coverage of quench nitrides.
[0044] The terms "weight %" and "wt %" are used interchangeably herein.
[0045] The terms "HAZ" or "heat affected zone" are used interchangeably and are unmelted areas of metal where material properties or microstructural changes occur due to exposure to the heat generated by welding. Thus, the HAZ is the area between the weld and the unaffected base metal. In the duplex steel of the present invention, the selected element ranges and conditions for balancing specific elements will significantly reduce sigma phase formation in the HAZ.
[0046] The advantages of the duplex stainless steel of the present invention and the selection of the element range of the duplex stainless steel make the duplex stainless steel of the present invention have unexpected advantages, which will be described in more detail below. It should be noted that the inventors have adjusted the composition for the selected elements and the ranges of these elements to obtain duplex stainless steels with the desired properties discussed herein. However, the present disclosure is not limited to the exemplary embodiments discussed, but can be varied within the scope of the appended claims. Unless otherwise explicitly disclosed, the upper and lower limits of individual constituent elements can be freely combined within the widest limits described in the claims. In addition, when a range is disclosed in the present disclosure, unless otherwise explicitly disclosed, the range includes the corresponding endpoint values of the range. Similarly, when an open range is disclosed, unless otherwise explicitly disclosed, the open range also includes the single endpoint values of the open range.
[0047] Chromium (Cr)
[0048] Chromium is an essential element, the range of which has been selected so that the duplex stainless steel of the present invention has good strength and corrosion resistance. In order to have good strength properties and corrosion resistance, the chromium content should be at least 28.5 wt%.
[0049] However, even though chromium is a beneficial element, its content should not be greater than 30.5 wt%, because high Cr content will increase the risk of sigma phase formation during cooling and in the HAZ during manufacturing. In addition, during solution annealing, the formation of quench nitrides will increase.
[0050] Furthermore, it has been found that in order to avoid the formation of sigma phase and to obtain maximum strength, it is important that the respective contents of chromium, molybdenum and tungsten are balanced. More specifically, the contents of chromium, molybdenum and tungsten are balanced so that the conditions of Formula 1 discussed above are met.
[0051] Therefore, the chromium content of the duplex stainless steel of the present invention is 28.5 wt % to 30.5 wt %. To further ensure that the above properties are obtained, according to the present disclosure, the chromium content can be 29.0 wt % to 30.5 wt %, such as 29.5 wt % to 30.5 wt %. According to the present disclosure, the chromium content can be 29.1 wt %, 29.2 wt %, 29.3 wt %, 29.4 wt % or 29.5 wt % to 29.6 wt %, 29.7 wt %, 29.8 wt %, 29.9 wt %, 30.0 wt %, 30.1 wt %, 30.2 wt %, 30.3 wt %, 30.4 wt % or 30.5 wt %.
[0052] Nickel (Ni)
[0053] Ni is used as an austenite stabilizing element. In order to obtain a ferrite content between 40 volume % and 60 volume %, the content of nickel should be at least 6.0 weight %. In addition, if the Ni content is too high, the austenite content will increase, resulting in reduced strength. However, since nickel is an expensive element, its content needs to be limited. According to the present disclosure, the maximum content of nickel is 8.0 weight %.
[0054] According to the present disclosure, the content of Ni can be less than 7.9 wt%, 7.8 wt%, 7.7 wt%, or 7.6 wt%. According to the present disclosure, the minimum amount of Ni can be 6.0 wt%. According to the present disclosure, the range can be between 6.0 wt% and 7.6 wt%.
[0055] Molybdenum (Mo)
[0056] Mo is an active element that improves strength and corrosion resistance in chloride environments and reducing acids.
[0057] However, excessive Mo content combined with high Cr content will increase the risk of σ phase formation. Molybdenum can sometimes be replaced by tungsten. It is generally accepted in the art that the replacement of molybdenum with tungsten can be carried out in a ratio of 2 wt. % W replacing 1 wt. % Mo. However, if the Mo content in the duplex stainless steel of the present invention is too low, excessive quenching nitrides will be formed in the ferrite grain boundaries during solution annealing and subsequent quenching.
[0058] Therefore, it is important to optimize the content of chromium, molybdenum and tungsten in duplex stainless steel to avoid the formation of sigma phase and obtain maximum strength. Therefore, the content of Mo should be in the range of at least 0.70 wt%, and the content of Mo should not be greater than 3.00 wt%. According to the present disclosure, the content of Mo can be at least 0.70 wt% to 2.00 wt%, such as at least 0.70 wt% to 1.70 wt%, such as at least 0.90 wt% to 1.70 wt%.
[0059] Tungsten (W)
[0060] W will improve corrosion resistance in chloride environments as well as pitting and crevice corrosion resistance. However, too high a W content combined with a high Cr content increases the risk of σ phase precipitation. Therefore, it is very important to balance the combined amounts of chromium, molybdenum and tungsten to avoid the formation of σ phase. More specifically, the contents of chromium, molybdenum and tungsten are balanced so that the conditions of Formula 1 discussed above are met.
[0061] Therefore, the content of W is 2.00 wt % to 4.40 wt %. According to the present disclosure, the content of W may be 2.50 wt % to 4.40 wt %, such as 3.00 wt % to 4.00 wt %.
[0062] Nitrogen (N)
[0063] Nitrogen is a very active element that increases the corrosion resistance and strength of duplex stainless steel. To achieve good results, at least 0.30 wt.% N should be added.
[0064] However, since the added N must be dissolved in the duplex stainless steel to increase strength and corrosion resistance, the N range must be carefully selected, since too high a N content increases the risk of chromium nitride precipitation, especially when the chromium content is also high. Therefore, the N content should be limited to a maximum of 0.55 wt%. Therefore, the nitrogen content is 0.30 wt% to 0.55 wt%.
[0065] According to the present disclosure, the content of N may be 0.35 wt % to 0.55 wt %, such as 0.38 wt % to 0.55 wt %, such as 0.38 wt % to 0.50 wt %.
[0066] Manganese (Mn)
[0067] In order to increase the solubility of N in steel, Mn is added. However, Mn may also form manganese sulfide, which becomes the starting point of pitting corrosion. Therefore, the content of Mn is greater than or equal to 0.20 wt % but less than or equal to 2.50 wt %. According to the present disclosure, the content of Mn may be 0.30 wt % to 2.00 wt %.
[0068] Silicon (Si)
[0069] Si is usually used as a deoxidizer in steel manufacturing. However, it is known that high silicon content can stabilize the σ phase. Therefore, the content of silicon should be limited to a maximum of 0.30 wt %. According to the present disclosure, the content of silicon can be 0.10 wt % to 0.30 wt %.
[0070] Carbon (C)
[0071] Carbon is an element that is difficult to completely avoid in duplex stainless steel. Pursuing extremely low carbon content will excessively increase manufacturing costs. Therefore, at least for cost reasons, carbon may be present in an amount of at least 0.005 wt%.
[0072] C strengthens stainless steel, but also promotes the formation of chromium carbides which are harmful to corrosion. Carbon also has limited solubility in both ferrite and austenite. Therefore, the carbon content should be limited to a maximum of 0.030% by weight, such as a maximum of 0.025% by weight.
[0073] Copper (Cu)
[0074] Cu can be added to improve resistance to certain corrosive environments such as acidic environments, and it also reduces sensitivity to stress corrosion cracking. In addition, Cu will increase strength and also reduce the formation of sigma phase.
[0075] However, Cu has a negative impact on nitrogen solubility, which increases the formation of chromium nitrides since less nitrogen is dissolved in the stainless steel. Therefore, if copper is added, it is very important to carefully adjust its content. Therefore, the content of Cu is limited to a maximum of 0.50 wt%, such as less than 0.50 wt%. According to one embodiment, Cu is added and the content of Cu is between 0.15 wt% and ≤ 0.50 wt%. According to an embodiment, the Cu content can be between 0.25 wt% and 0.45 wt%.
[0076] Sulfur (S)
[0077] Sulfur is a common impurity element in duplex stainless steel. The sulfur content should not be greater than 0.030 wt. % because hot workability may be affected above this range.
[0078] Phosphorus (P)
[0079] Phosphorus is also a common impurity element in duplex stainless steel. The phosphorus content should not be greater than 0.030 wt. % because it will affect hot workability above this range.
[0080] The balance of the duplex stainless steel of the present invention is iron (Fe) and unavoidable impurities. The unavoidable impurities are elements that are not intentionally added but may be in the steel of the present invention due to scrap and / or manufacturing processes used to obtain the duplex stainless steel. Examples of these elements are, but are not limited to, Co, V, Ti, Nb, Pb, Sn and Ce. The total content of these elements is less than 1.0 wt%.
[0081] In addition, the duplex stainless steel of the present invention may optionally contain one or more elements added to improve the manufacturing process. Examples of such manufacturing process improving elements are, but are not limited to, aluminum (Al), magnesium (Mg), calcium (Ca) and boron (B). Under the condition that the content of Al cannot be greater than 0.050 wt. % and under the condition that the content of B cannot be greater than 0.050 wt. %, the total content of these improving elements is less than 0.50 wt. %, such as less than 0.30 wt. %.
[0082] Furthermore, the duplex stainless steel of the present invention may comprise or consist of the elements mentioned herein within any ranges of the specific elements mentioned herein and meeting the requirements mentioned herein.
[0083] According to an embodiment, the present disclosure relates to an object comprising or consisting of a duplex stainless steel as defined above or below. According to an embodiment, the object is made of a duplex stainless steel as defined above or below. According to an embodiment, the object is in a solution annealed state.
[0084] Accordingly, the present disclosure relates to an object comprising a duplex stainless steel, wherein the duplex stainless steel comprises the following elements (in wt %):
[0085] C max 0.030;
[0086] Si max 0.30;
[0087] Mn 0.20 to 2.50;
[0088] P max 0.030;
[0089] S max 0.030;
[0090] Cr28.5 to 30.5;
[0091] Ni6.0 to 8.0;
[0092] Mo0.70 to 3.00;
[0093] W2.00 to 4.40;
[0094] Cu max 0.50;
[0095] N0.30 to 0.55;
[0096] The balance is Fe and unavoidable impurities;
[0097] The ferrite content is 40 volume % to 60 volume %;
[0098] The duplex stainless steel meets the following requirements:
[0099] a) [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5,
[0100] wherein the values of [Cr], [Mo] and [W] are in weight %; and
[0101] b) In the solution annealed state, the coverage of quenched nitrides in the ferrite grain boundaries is less than 10%.
[0102] The Rp0.2 of the object of the present invention measured at room temperature can be higher than 650 MPa (ISO 6892-1, 2019).
[0103] Therefore, the present disclosure also relates to an object comprising or consisting of a duplex stainless steel comprising the following elements (in wt. %):
[0104] C Max. 0.030 Si Max. 0.30 Mn 0.30 to 2.50 P Max. 0.030 S Max. 0.030 Cr 28.5 to 30.5 Ni 6.0 to 8.0 Mo 0.70 to 3.00 W 2.00 to 4.40 Cu Max. 0.50 N 0.30 to 0.55 Fe and unavoidable impurities margin
[0105] And meet the following conditions:
[0106] a) [Cr] + 4.0*[Mo] + 2.0*[W] < 42,
[0107] wherein the values of [Cr], [Mo] and [W] are in weight %; and wherein the ferrite content is 40 volume % to 60 volume %; and
[0108] b) wherein the coverage of quenched nitrides in the ferrite grain boundaries in the solution annealed condition is less than 10%; and
[0109] c) Where Rp0.2 at room temperature is higher than 650 MPa (ISO 6892-1, 2019).
[0110] The present disclosure also relates to an object comprising a duplex stainless steel, wherein the duplex stainless steel comprises the following elements (in wt %):
[0111] C Max. 0.030 Si Max. 0.30 Mn 0.20 to 2.50 P Max. 0.030 S Max. 0.030 Cr 28.5 to 30.5 Ni 6.0 to 8.0 Mo 0.70 to 3.00 W 2.00 to 4.40 Cu Max. 0.50 Al Max. 0.050 N 0.30 to 0.55 Fe and inevitable impurities margin
[0112] The ferrite content is 40 volume % to 60 volume %; and the following conditions are met:
[0113] a) [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5,
[0114] wherein the values of [Cr], [Mo] and [W] are in weight %; and
[0115] b) wherein the coverage of quenched nitrides in the ferrite grain boundaries in the solution annealed condition is less than 10%; and
[0116] c) wherein the object has an Rp0.2 measured at room temperature higher than 650 MPa (ISO 6892-1, 2019).
[0117] An Rp0.2 above 650 MPa (ISO 6892-1, 2019) at room temperature means that the duplex stainless steel objects of the present invention can be used in applications where the material is exposed to high internal pressures (such as may be found in new developments that have recently begun exploring at higher well pressures of 20 ksi) and yet still have a high strength sufficient to support its own weight.
[0118] According to an embodiment, the object is a tube or a tubular body, such as a seamless tube or a coil or one or more tubes welded together to form a long tube. According to other embodiments, the object is a longitudinally welded tube or a welded tubular body. According to an embodiment, the object is a hollow body or a billet. According to other embodiments, the object may be a strip or a wire.
[0119] The present disclosure also relates to a method of manufacturing a duplex stainless steel object such as a tube as defined above or below, wherein the method comprises the following steps:
[0120] - molten raw materials;
[0121] The melting can be performed by a high frequency induction furnace or an electric arc furnace.
[0122] - Casting;
[0123] - thermal processing;
[0124] The hot working may be performed by forging and / or rolling and / or extrusion.
[0125] - Cold working;
[0126] The cold working may be performed by rolling or pilger rolling.
[0127] - solution annealing, the solution annealing being carried out at a temperature ranging from about 1000°C to about 1200°C, such as from about 1050°C to about 1150°C;
[0128] - cool down;
[0129] The cooling may be performed at room temperature, and the cooling may be performed in air. The cooling is performed from the solution annealing temperature to a temperature of about 900°C to about 1000°C.
[0130] - Quenching;
[0131] Quenching can be done in water. Quenching should be done to avoid the formation of sigma phase.
[0132] - Optionally, further steps such as straightening, machining etc. may be performed.
[0133] The term "about" means a deviation of 10% from a numerical value.
[0134] List of projects to implement:
[0135] 1. A duplex stainless steel comprising the following elements (in wt%):
[0136] C max 0.030;
[0137] Si max 0.30;
[0138] Mn 0.20 to 2.50;
[0139] P max 0.030;
[0140] S max 0.030;
[0141] Cr28.5 to 30.5;
[0142] Ni6.0 to 8.0;
[0143] Mo0.70 to 3.00;
[0144] W2.00 to 4.40;
[0145] Cu max 0.50;
[0146] N0.30 to 0.55;
[0147] The balance is Fe and unavoidable impurities;
[0148] The ferrite content is 40 volume % to 60 volume %;
[0149] The duplex stainless steel meets the following requirements:
[0150] a) [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5, wherein the values of [Cr], [Mo] and [W] are in weight %; and
[0151] b) In the solution annealed state, the coverage of quenched nitrides in the ferrite grain boundaries is less than 10%.
[0152] 2. The duplex stainless steel according to item 1, wherein the Cr content is 29.0 wt % to 30.5 wt %.
[0153] 3. The duplex stainless steel according to item 1 or 2, wherein the Cr content is 29.5 wt % to 30.5 wt %.
[0154] 4. The duplex stainless steel according to any one of items 1 to 3, wherein the Ni content is 6.0 wt % to 7.6 wt %.
[0155] 5. The duplex stainless steel according to any one of items 1 to 4, wherein the content of Mo is at least 0.70 wt. % to 2.00 wt. %.
[0156] 6. The duplex stainless steel according to any one of items 1 to 5, wherein the content of W is 2.50 wt % to 4.40 wt %.
[0157] 7. The duplex stainless steel according to any one of items 1 to 6, wherein the content of W is 3.00 wt % to 4.00 wt %.
[0158] 8. The duplex stainless steel according to any one of items 1 to 7, wherein the content of Mn is 0.30 wt % to 2.00 wt %.
[0159] 9. The duplex stainless steel according to any one of items 1 to 8, wherein the Si content is 0.10 wt % to 0.30 wt %.
[0160] 10. The duplex stainless steel according to any one of items 1 to 9, wherein the Cu content is 0.15 wt % to 0.50 wt %.
[0161] 11. The duplex stainless steel according to any one of items 1 to 10, wherein the N content is 0.35 wt % to 0.55 wt %.
[0162] 12. The duplex stainless steel according to any one of items 1 to 11, wherein the N content is 0.38 wt % to 0.55 wt %.
[0163] 13. The duplex stainless steel according to any one of items 1 to 12, wherein the N content is 0.38 wt. % to 0.50 wt. %.
[0164] 14. An object comprising or consisting of the duplex stainless steel according to any one of items 1 to 13.
[0165] 15. The object according to item 14, wherein Rp0.2 of the object at room temperature is higher than 650 MPa (ISO6892-1, 2019).
[0166] According to an embodiment, the present disclosure also relates to a solution annealed object comprising or consisting of any one of features 1 to 15 or a combination thereof.
[0167] According to an embodiment, the present disclosure also relates to a treated duplex stainless steel comprising or consisting of any one or a combination of features 1 to 13. The duplex stainless steel has been treated as described above or below.
[0168] The present disclosure is further described by the following non-limiting examples.
[0169] Example
[0170] Example 1 - Sample preparation
[0171] The materials having the chemical compositions according to Table 1 were melted in a high-frequency induction furnace as 50 kg of material or 270 kg of material, and then cast into ingots using a mold.
[0172] After casting, the mold is removed and the ingot is heat treated by solution annealing and subsequent quenching. Chemical analysis samples are taken from each ingot. Chemical analysis is performed by using X-ray fluorescence spectrometry, spark atomic emission spectrometry and combustion techniques, as different elements require different methods to measure the content.
[0173] The obtained ingot is forged or hot-rolled into a billet. The obtained billet is machined into smaller billets as needed.
[0174] After hot working (rolling or forging), the billets are cold rolled into 7 to 10 mm samples and then solution annealed at a temperature between 1050°C and 1150°C, then cooled at room temperature to a temperature between 950°C and 1000°C and subsequently quenched with water.
[0175] Example 2 - σ Phase Measurement
[0176] The σ phase measurement results are shown in Table 2.
[0177] The samples were obtained after solution annealing and quenching. Then, in order to simulate the environment of the heat affected zone, the samples were heated to about 1100°C. The samples were cooled at a controlled rate of 40°C / min from about 1100°C to room temperature.
[0178] The fraction of σ phase formed during cooling was measured using SEM and the coverage of 0.4 mm 2 Ten image fields of the total area of the sample are evaluated by image analysis. Since this test simulates the real situation of welding operation, if there is no σ phase or a small amount of σ phase, the product can be welded with a small amount of σ phase formed in the HAZ. As previously mentioned, if no σ phase or a small amount of σ phase is found, corrosion resistance will be present, and impact toughness will be excellent.
[0179] Example 3 - Rp0.2 Measurement
[0180] Rp0.2 measured according to ISO 6892-1, 2019 at room temperature.
[0181] The results are shown in Table 2. The Rp0.2 of the stainless steel materials of the present invention is higher than 650 MPa, such as higher than 660 MPa.
[0182]
[0183] Example 4 - Measurement of coverage of quenched nitrides in ferrite grain boundaries
[0184] The coverage of quenched nitrides in the ferrite grain boundaries was measured in the solution annealed state. The samples were taken from Example 1. Standard optical microscope (LOM) micrographs taken at 500 times magnification and using a 0.05 mm 2 The intercept method of 10 randomly oriented test wires in a representative location was used to measure the percentage of ferrite grain boundaries covered by quenched nitride. The LOM specimens were prepared by surface polishing followed by electrolytic etching in HNO3 and NaOH. The percentage of ferrite grain boundaries covered by quenched nitride was calculated by dividing the number of intercepts between the test wire and ferrite grain boundaries covered by quenched nitride by the total number of intercepts between the test wire and ferrite grain boundaries. Figures 1A to 5B An example thereof is shown, and the results of these calculations are shown in Table 3.
[0185]
[0186] Example 5 – Ferrite Measurement
[0187] The amount of ferrite was measured using LOM and manual point counting according to ASTM E562. The remainder was essentially austenite. Ferrite was measured on cold rolled, solution annealed and quenched samples.
[0188]
[0189]
[0190]
Claims
1. A duplex stainless steel comprising the following elements in wt %: C max 0.030; Si max 0.30; Mn 0.20 to 2.50; P max 0.030; S max 0.030; Cr28.5 to 30.5; Ni6.0 to 8.0; Mo0.70 to 3.00; W2.00 to 4.40; Cu≤0.50; N0.30 to 0.55; The balance is Fe and unavoidable impurities; The ferrite content is 40 volume % to 60 volume %; The duplex stainless steel meets the following requirements: b. [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5, wherein the values of [Cr], [Mo] and [W] are in weight %; and c. In the solution annealed state, the coverage of quenched nitrides in the ferrite grain boundaries is less than 10%. 2 . The duplex stainless steel according to claim 1 , wherein the content of Cr is 29.0 wt % to 30.5 wt %.
3. The duplex stainless steel according to any one of claims 1 to 2, wherein the content of Ni is 6.0 wt% to 7.6 wt%.
4. The duplex stainless steel according to any one of claims 1 to 3, wherein the content of Mo is at least 0.70 wt. % to 2.00 wt. %.
5. The duplex stainless steel according to any one of claims 1 to 3, wherein the content of W is 2.50 wt% to 4.40 wt% or 3.00 wt% to 4.00 wt%.
6. The duplex stainless steel according to any one of claims 1 to 5, wherein the content of Mn is 0.30 wt% to 2.00 wt%.
7. The duplex stainless steel according to any one of claims 1 to 6, wherein the content of Si is 0.10 wt% to 0.30 wt%.
8. The duplex stainless steel according to any one of claims 1 to 7, wherein the content of Cu is 0.15 wt% to 0.50 wt%.
9. The duplex stainless steel according to any one of claims 1 to 8, wherein the N content is 0.35 wt% to 0.55 wt% or 0.38 wt% to 0.55 wt% or 0.38 wt% to 0.50 wt%.
10. An object comprising duplex stainless steel, wherein the duplex stainless steel comprises the following elements in wt %: C max 0.030; Si max 0.30; Mn 0.20 to 2.50; P max 0.030; S max 0.030; Cr28.5 to 30.5; Ni6.0 to 8.0; Mo0.70 to 3.00; W2.00 to 4.40; Cu≤0.50; N0.30 to 0.55; The balance is Fe and unavoidable impurities; The ferrite content is 40 volume % to 60 volume %; The duplex stainless steel meets the following requirements: a) [Cr] + 4.0*[Mo] + 2.0*[W] < 42.5 wherein the values of [Cr], [Mo] and [W] are in weight %; and b) In the solution annealed state, the coverage of quenched nitrides in the ferrite grain boundaries is less than 10%.
11. The object according to claim 10, wherein the object has an Rp0.2 higher than 650 MPa ISO 6892-1, 2019.
12. An object according to claims 10-11, wherein the object in the solution annealed condition will contain less than 0.2 volume % sigma phase after cooling from 1100°C to room temperature at 40°C / min.
13. The object of claims 10 to 12, wherein the object comprises an element within the range of any one of claims 2 to 9.
14. The object according to any one of claims 10 to 13, wherein the object is a tube, a sheet, a hollow body, a billet, a strip or a wire.
15. The object of any one of claims 10 to 14, wherein the object is a solution annealed object.
16. Use of an object according to any one of claims 10 to 15, in applications requiring high pressure resistance, such as applications with internal pressures above about 20 kpsi.
17. A method of manufacturing an object according to any one of claims 10 to 16, the method comprising the steps of: - melting; - Casting; - thermal processing; - Cold working; - solution annealing in a temperature range of about 1000°C to about 1200°C, such as about 1050°C to about 1150°C; - cooling from the solution annealing temperature to a temperature of about 900°C to about 1000°C; - Quenching.