Separator for rechargeable lithium battery and rechargeable lithium battery including same
A MOF-coated separator for lithium batteries addresses the explosion risk by capturing gases during thermal runaway, enhancing safety through effective gas adsorption.
Patent Information
- Application Number
- CN202280094527.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2022-06-03
- Publication Date
- 2024-12-06
AI Technical Summary
Rechargeable lithium batteries face a high risk of explosion due to rapid gas generation during thermal runaway conditions, which existing methods to reduce gas production are ineffective once a short circuit occurs.
A separator for lithium batteries is coated with a metal organic framework (MOF) such as ZIF-8 or Fe-BTC, or a combination thereof, which captures gas through adsorption reactions, reducing the risk of explosion by trapping increasing gas volumes.
The MOF-coated separator effectively captures rapidly generated gases, significantly reducing the risk of lithium battery explosions during thermal runaway situations.
Smart Images

Figure CN119096394A_ABST
Abstract
Description
Technical Field
[0001] Disclosed are a separator for a rechargeable lithium battery and a rechargeable lithium battery including the same. Background Art
[0002] Rechargeable lithium batteries have attracted attention as power sources for driving medium to large devices such as hybrid vehicles and battery vehicles, as well as small devices such as mobile phones, notebook computers, and smartphones.
[0003] When these rechargeable lithium batteries are exposed to misuse conditions such as overcharging and extreme conditions such as heat exposure, the rechargeable lithium batteries may explode due to a sharp increase in the amount of gas generated therein while thermal runaway occurs.
[0004] Methods of reducing the amount of gas generated by coating the surface of the active material or adding film-forming additives to the electrolyte are known to some extent. However, when a rechargeable lithium battery enters a thermal runaway situation due to a short circuit, this method is no longer effective. Summary of the invention
[0005] [Technical issues]
[0006] Embodiments are provided to suppress a rapid increase in the amount of gas generated in a rechargeable lithium battery when the rechargeable lithium battery enters a thermal runaway condition.
[0007] [Technical problem solving method]
[0008] In an embodiment, a separator for a rechargeable lithium battery includes: a substrate; and a coating; a metal organic framework (MOF) located on one or both surfaces of the substrate and including ZIF-8, Fe-BTC, or a combination thereof.
[0009] Another embodiment provides a rechargeable lithium battery including the separator for a rechargeable lithium battery.
[0010] [Beneficial Effects]
[0011] In the separator for a rechargeable lithium battery of this embodiment, the metal organic framework structure, which is ZIF-8, Fe-BTC, or a combination thereof, is a material that can effectively capture gas through an adsorption reaction.
[0012] Accordingly, a rechargeable lithium battery including a separator coated with a metal organic framework structure (which is ZIF-8, Fe-BTC or a combination thereof) on one or both surfaces has a significantly reduced risk of explosion even when a thermal runaway situation occurs and the amount of gas generated therein increases rapidly, because the metal organic framework captures the rapidly increasing gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Various examples of the shape (pattern) of the coating layer formed according to the embodiment are explained.
[0014] Figure 2 is a perspective view of a pouch-type rechargeable battery according to an embodiment.
[0015] Figure 3 For along Figure 2 A vertical cross-sectional view taken along line II in the direction of the arrow.
[0016] Figure 4 For along Figure 2 A horizontal cross-sectional view taken along line II-II in the direction of the arrow. DETAILED DESCRIPTION
[0017] Hereinafter, specific embodiments will be described in detail so that those skilled in the art can easily implement them. However, the present disclosure may be implemented in many different forms and is not to be construed as limited to the example embodiments set forth herein.
[0018] The terms used herein are for describing the embodiments only and are not intended to limit the present disclosure. A singular expression includes a plural expression unless the context clearly indicates otherwise.
[0019] "Combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like, of the components.
[0020] It should be understood that terms such as “comprises,” “includes,” or “has” are intended to indicate the presence of implemented features, quantities, steps, elements, or a combination thereof, but do not exclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or a combination thereof.
[0021] In the drawings, the thickness of layers, films, panels, regions, etc., are exaggerated for clarity, and the same reference numerals represent the same elements throughout the specification. It will be understood that when an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, it can be directly on the other element, or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0022] The "layer" includes not only a shape formed on the entire surface when viewed from a plan view but also a shape formed on a partial surface.
[0023] "Particle size" or "average particle size" can be measured by methods well known to those skilled in the art, for example, by a particle size analyzer, or by a transmission electron microscope or a scanning electron microscope. Alternatively, the average particle size value can be obtained by measuring using a dynamic light scattering method, performing data analysis, counting the number of particles in each particle size range, and calculating therefrom. Unless otherwise defined, the average particle size may refer to the diameter (D ) of particles of a particle size having a cumulative volume of 50% by volume. 50 ).
[0024] The "thickness" can be measured by a photograph taken with a thickness gauge or an optical microscope (such as a scanning electron microscope). In addition, the "area" can be measured by a photograph taken with an optical microscope (such as a scanning electron microscope).
[0025] [Separator for rechargeable lithium battery]
[0026] In an embodiment, a separator for a rechargeable lithium battery includes: a substrate; and a coating layer on one or both surfaces of the substrate and including a metal organic framework (MOF) of ZIF-8, Fe-BTC, or a combination thereof.
[0027] Metal organic frameworks are materials that can effectively capture gas through adsorption reactions. In particular, a rechargeable lithium battery including a separator coated with a metal organic framework structure (which is ZIF-8, Fe-BTC or a combination thereof) on one or both surfaces has a significantly reduced risk of explosion even when a thermal runaway situation occurs and the amount of gas generated therein increases rapidly, because the metal organic framework captures the rapidly increasing gas.
[0028] Hereinafter, a separator for a rechargeable lithium battery according to an embodiment will be described in detail.
[0029] The structure of a metal-organic framework
[0030] The metal organic framework is a material in which metal ions or metal clusters are connected by organic ligands, and is a coordination polymer. The metal organic framework has a cage that becomes an empty space therein by forming a three-dimensional structure. As a result, the metal organic framework can undergo an adsorption reaction through the cage and trap the gas in the cage.
[0031] On the other hand, zeolite, a crystalline aluminum silicate mineral, has a poor gas capture effect compared to metal organic frameworks. Gas adsorption reaction is a reaction in which gas molecules are adsorbed on the cage surface inside the material structure. In general, the larger the specific surface area, the more gas molecules can be adsorbed. According to the results of several previous studies comparing the specific surface area of zeolite and representative materials with the specific surface area of metal organic frameworks, metal organic frameworks have been reported to have a larger specific surface area than zeolites. Accordingly, metal organic frameworks can have a larger surface area for gas adsorption than zeolites. In particular, in rechargeable lithium batteries using nickel-based positive electrode active materials containing 90% or more Ni as positive electrode active materials, metal organic frameworks exhibit very excellent gas capture effects, while zeolites exhibit very poor gas capture effects. This fact is confirmed in the evaluation examples described later.
[0032] The structural and compositional features of the metal organic framework can be effectively used in the formation charge and discharge and thermal runaway conditions of rechargeable lithium batteries. Specifically, when the sheet for a rechargeable lithium battery according to an embodiment is arranged inside the rechargeable lithium battery, the increase in battery volume and the increase in internal pressure can be prevented by capturing the gas generated inside the rechargeable lithium battery during the first cycle charge and discharge (i.e., formation charge and discharge). In addition, even when the rechargeable lithium battery enters a thermal runaway condition in which a short circuit occurs due to overcharging, heat exposure, etc., the metal organic framework can effectively collect the rapidly increasing gas components (e.g., H2, CO, CO2, etc.) inside the rechargeable lithium battery, so that the possibility of explosion of the rechargeable lithium battery is significantly reduced.
[0033] In particular, in the separator for a rechargeable lithium battery of the embodiment, the metal organic framework may include ZIF-8, Fe-BTC or a combination thereof, and each structure is as follows:
[0034] [Chemical formula 1]
[0035]
[0036] ZIF-8 is represented by Chemical Formula 1, the coordination metal is Zn, and the linker is 2-methylimidazole. ZIF-8 has a diameter of 0.66 cm 3 / g pore volume and 1300m 2 / g~1800m 2 / g BET specific surface area.
[0037] [Chemical formula 2]
[0038]
[0039] Fe-BTC is represented by chemical formula 2, the coordination metal is Fe, and the linker is 1,3,5-benzenetricarboxylic acid. Fe-BTC has a carbon content of 0.9 g / cm 3 The pore volume and 1300m 2 / g~1600m 2 / g BET specific surface area.
[0040] According to the evaluation examples described below, ZIF-8 and Fe-BTC have remarkably excellent gas capture effects not only compared with zeolite but also compared with other metal organic frameworks (eg, ZIF-67, etc.).
[0041] Previous studies on metal organic frameworks known to date have shown that cations increase the polarity of metal organic frameworks, thereby enhancing the physical adsorption of gas molecules, and that anions increase chemical adsorption through coordination bonds of unshared electron pairs.
[0042] In this regard, it is speculated that the gas capture effects of ZIF-8 and Fe-BTC are significantly better than not only zeolites but also other metal-organic frameworks because the synergistic effect of physical adsorption and chemical adsorption of gas components (e.g., H2, CO, CO2, etc.) generated by rechargeable lithium batteries is maximized due to the molecular structure.
[0043] Additional components of coating
[0044] In addition to the metal organic framework structure, which is ZIF-8, Fe-BTC, or a combination thereof, the coating may further include a binder.
[0045] The binder may be a particle-type binder and is used to bind the metal organic framework structures (which are ZIF-8, Fe-BTC or a combination thereof) to each other or to a substrate.
[0046] The particle type binder may include polyvinylidene fluoride (PVdF), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer, ethylene vinyl acetate (EVA), hydroxyethyl cellulose (HEC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), ethylene-acrylic acid copolymer, acrylonitrile, vinyl acetate derivatives, polyethylene glycol, acrylic rubber or a combination thereof. Polyvinylidene fluoride can improve the bonding strength between metal organic framework structures (which are ZIF-8, Fe-BTC or a combination thereof) and the bonding strength between them and the substrate. In an embodiment, the particle size of the particle type binder is not limited, and a particle type binder with a particle size commonly used in the art can be used.
[0047] The weight ratio of the binder to the metal organic framework in the coating layer may be 0.3:9.7 to 5:5, specifically 0.4:9.6 to 5:5, and more specifically 0.4:9.6 to 4:6. Within this range, the dispersibility of the binder and the metal organic framework in the coating solution, the bonding strength between the metal organic frameworks, and the bonding strength between the metal organic framework and the substrate can be well ensured.
[0048] Meanwhile, in order to ensure heat resistance or mechanical strength, inorganic filler particles and / or a binder may be further included in the interior, upper portion and / or lower portion of the coating. For example, an additional coating layer including inorganic filler particles and / or a binder may be included in a single layer or multilayer structure on the top and / or bottom of the coating layer.
[0049] Specifically, the inorganic filler particles can be metal oxides, semi-metal oxides or a combination thereof.
[0050] Specifically, the inorganic filler particles may be one or more selected from alumina (Al2O3), boehmite, BaSO4, MgO, Mg(OH)2, clay, silica (SiO2) and (TiO2). Alumina, silica, etc. have a small particle size, so it is easy to prepare a dispersion.
[0051] For example, the inorganic filler particles may be Al2O3, SiO2, TiO2, SnO2, CeO2, NiO, CaO, ZnO, MgO, ZrO2, Y2O3, SrTiO3, BaTiO3, MgF2, Mg(OH)2, or a combination thereof. The inorganic filler particles may have a spherical shape, a plate shape, a fibrous shape, etc., but are not limited thereto, and any form available in the art may be used.
[0052] The plate-like inorganic filler particles include, for example, alumina and boehmite. In this case, the reduction in the separator area at high temperatures can be further suppressed, a relatively large degree of porosity can be ensured, and the characteristics when evaluating lithium battery permeability can be improved.
[0053] When the inorganic filler particles are in the form of flakes or fibers, the inorganic filler particles may have an aspect ratio of about 1:5 to 1:100. For example, the aspect ratio may be about 1:10 to 1:100. For example, the aspect ratio may be about 1:5 to 1:50. For example, the aspect ratio may be about 1:10 to 1:50.
[0054] The length ratio of the major axis to the minor axis on the flat surface of the flaky inorganic filler particles may be 1 to 3. For example, the length ratio of the major axis to the minor axis on the flat surface may be 1 to 2. For example, the length ratio of the major axis to the minor axis on the flat surface may be about 1. The aspect ratio and the length ratio of the major axis to the minor axis may be measured by a scanning electron microscope (SEM). Within the range of the aspect ratio and the length ratio of the major axis to the minor axis, the shrinkage of the separator may be suppressed, a relatively improved porosity may be ensured, and the permeation characteristics of the lithium battery may be improved.
[0055] When the inorganic filler particles are plate-shaped, the flat surface of the inorganic filler particles has an average angle of 0 to 30° with one surface of the porous substrate. For example, the average angle of the flat surface of the inorganic filler particles with one surface of the porous substrate can converge to 0°. In other words, the flat surface of the inorganic filler particles can be parallel to one surface of the porous substrate. For example, when the average angle of the flat surface of the inorganic filler particles with one surface of the porous substrate is within this range, the porous substrate can effectively suppress thermal shrinkage, thereby providing a diaphragm with a reduced shrinkage rate.
[0056] At the same time, the binder may include a polymer binder of a particle or solution type. Examples of polymer binders may include polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymers or combinations thereof. When a separator additionally coated with a polymer binder is used, a physical crosslinking phenomenon occurs between the polymer binder and the binder present in each positive electrode and negative electrode, thereby improving the bonding strength between the separator and the electrode.
[0057] Coating thickness and area
[0058] The thickness ratio of the coating layer to the substrate (coating thickness / substrate thickness) on each surface of the substrate of the diaphragm may be 1 / 1000 to 5. For example, the thickness ratio of the coating layer to the substrate (coating thickness / substrate thickness) on each surface of the substrate of the diaphragm may be greater than or equal to 1 / 1000, greater than or equal to 1 / 100, or greater than or equal to 1 / 10, and less than or equal to 5, less than or equal to 4.2, less than or equal to 4, less than or equal to 3, less than or equal to 2, or less than or equal to 1.
[0059] Specifically, the thickness of the coating on each surface of the substrate of the diaphragm may be greater than or equal to 50 nm. Although the thickness ratio of the coating on each surface of the substrate of the diaphragm to the substrate (coating thickness / substrate thickness) is less than 1 / 1000, when the coating has a thickness of less than 50 nm, the gas capture effect of the metal organic framework may not be obvious. In contrast, although the thickness ratio of the coating on each surface of the substrate of the diaphragm to the substrate (coating thickness / substrate thickness) is greater than 5, when the thickness of the coating is greater than 30 μm, the gas capture effect tends to be saturated.
[0060] Specifically, the thickness of the coating on each surface of the substrate of the diaphragm may be greater than or equal to 50 nm, greater than or equal to 100 nm, greater than or equal to 500 nm, greater than or equal to 1 μm, greater than or equal to 5 μm, or greater than or equal to 10 μm. In this article, since the thickness of the coating on each surface of the substrate of the diaphragm is closer to greater than or equal to 10 μm, the metal organic framework can increase the gas capture effect.
[0061] In addition, the thickness of the coating on each surface of the substrate of the diaphragm may be less than or equal to 30 μm or less than or equal to 20 μm. The gas capture effect when the thickness of the coating on each surface of the substrate of the diaphragm ranges from 10 μm to 20 μm may be equivalent to the gas capture effect when the thickness of the coating on each surface of the substrate of the diaphragm ranges from greater than 20 μm to less than or equal to 30 μm. Accordingly, considering economic feasibility, the thickness of the coating may be less than or equal to 20 μm.
[0062] On the other hand, the larger the membrane is, the larger the area of each surface of the substrate is, and the better the gas capture effect is. In this regard, the coating may be applied to the entire surface of the substrate, wherein the coating may be present on one surface or both surfaces of the substrate. In particular, when the coating is present on both entire surfaces of the substrate, the gas capture effect may be more excellent than when the coating is present on only one surface of the substrate.
[0063] For reference, if the binder is included in the coating, the thickness and area of the coating include the thickness and area due to the binder. In this article, "thickness" can be measured by a photograph taken with a thickness gauge or an optical microscope (such as a scanning electron microscope). For example, the thickness of the coating in the diaphragm can be measured by cutting the diaphragm in the thickness direction and measuring the length between the lowest end and the highest end of the coating using a commercially available thickness gauge. Alternatively, the thickness of the coating can be obtained by taking an image of the cut surface of the diaphragm with an optical microscope (such as a scanning electron microscope) and calculating the length between the lowest end and the highest end of the coating shown on the image.
[0064] On the other hand, the "area" can be measured by a photograph taken with an optical microscope (such as a scanning electron microscope). For example, the area of the coating in the diaphragm can be obtained by taking an image of the diaphragm from the top with an optical microscope (such as a scanning electron microscope) and calculating the area of the coating shown in the image.
[0065] Coating shape (pattern)
[0066] The coating can be patterned. In this way, the gas diffusion area is enlarged in the patterned coating, thereby further enhancing the gas capture effect. Specifically, Figure 1Various shapes (patterns) of the positive electrode active material layer are illustrated. The coating may be patterned into a plurality of dots, lines, rings, or a combination thereof. However, the embodiment is not limited thereto, and may include a non-patterned coating, in which case an excellent gas capture effect may also be exhibited.
[0067] Method for forming a coating
[0068] The method for forming the coating layer may be any method available in the relevant technical field.
[0069] Specifically, a slurry-phase coating solution can be prepared by dispersing a metal organic framework (which is ZIF-8, Fe-BTC or a combination thereof) in an appropriate dispersion solvent, to which a binder can be added. Thereafter, the diaphragm of the embodiment can be completed by coating the coating solution on a substrate and then by processes such as drying and pressing.
[0070] The solvent is not particularly limited as long as it is a solvent capable of dispersing the metal organic framework structure (which is ZIF-8, Fe-BTC, or a combination thereof) and the binder, and may be, for example, methylpyrrolidone (NMP).
[0071] The total amount of solid content (i.e., metal organic framework structure (which is ZIF-8, Fe-BTC or a combination thereof) and binder) in the coating solution may be 0.5 wt % to 30 wt %. Within this range, the dispersibility of the coating solution is appropriately controlled so that it can be uniformly coated on the substrate.
[0072] The method for applying the coating solution on the above-mentioned substrate is not particularly limited, and any method available in the relevant technical field can be used. For example, methods such as printing, pressing, indentation, roller coating, scraping, brushing, dipping, spraying or flow coating can be used.
[0073] substrate
[0074] The substrate may be a porous substrate. The above-mentioned porous substrate may be a porous film including polyolefin. Since polyolefin is a material that can achieve a shutdown effect and an excellent short circuit prevention effect, a porous substrate including polyolefin can improve battery stability. In addition, a porous substrate including polyolefin can improve the coating performance of a coating solution applied thereon, and can reduce the thickness of the resulting coating. Accordingly, when a porous substrate including polyolefin is used, the total thickness of the separator including the porous substrate and the coating formed thereon becomes thinner, so that the proportion of the electrode active material in the battery is relatively increased, and the capacity per unit volume of the battery can be increased.
[0075] Meanwhile, the above-mentioned film may be a single-layer film including polyolefin such as polyethylene or polypropylene, or a multilayer film including two or more layers of polyolefin in each layer.
[0076] Specifically, the material may be a laminate (a three-layer film of PP / PE / PP), in which a first layer including polypropylene, a second layer including polyethylene, and a third layer including polypropylene are laminated in sequence. Compared with a single-layer film including polyolefins (such as polyethylene or polypropylene) or a two-layer film including polyolefins in each layer, the three-layer film of PP / PE / PP has a high synergistic effect with a metal organic framework structure (which is ZIF-8, Fe-BTC, or a combination thereof). In addition, compared with a single-layer film including polyolefins (such as polyethylene or polypropylene) or a two-layer film including polyolefins in each layer, the three-layer film of PP / PE / PP has more excellent mechanical strength, and thus may have stronger shrinkage resistance and deformation resistance, and in particular, it is presumed that the diffusion of gases generated at high temperatures into the metal organic framework has relatively little interference.
[0077] The thickness of the substrate mentioned above may be 1 μm to 100 μm, 1 μm to 30 μm, 3 μm to 20 μm, 3 μm to 15 μm or 3 μm to 12 μm. If the thickness of the substrate is less than 1 μm, it may be difficult to maintain the mechanical properties of the separator, and if the thickness of the substrate is greater than 100 μm, the internal resistance of the lithium battery may increase.
[0078] The porosity of the composition may be 5% to 95%. If the porosity is less than 5%, the internal resistance of the lithium battery may increase, and if the porosity is greater than 95%, it may be difficult to maintain the mechanical properties of the porous substrate.
[0079] The pore size of the above materials may be 0.01 μm to 50 μm. For example, the pore size of the porous substrate in the separator may be 0.01 μm to 20 μm. For example, the pore size of the porous substrate in the separator may be 0.01 μm to 10 μm. If the pore size of the porous substrate is less than 0.01 μm, the internal resistance of the lithium battery may increase, and if the pore size of the porous substrate is greater than 50 μm, it may be difficult to maintain the mechanical properties of the porous substrate.
[0080] [Rechargeable lithium battery]
[0081] In another embodiment, a rechargeable lithium battery is provided, which includes the sheet usable for a rechargeable lithium battery of the aforementioned embodiment.
[0082] A rechargeable lithium battery including an outer material having an inner surface coated with a metal-organic framework structure (which is ZIF-8, Fe-BTC, or a combination thereof) has a significantly reduced risk of explosion even when a thermal runaway condition occurs and the amount of gas generated therein increases rapidly because the metal-organic framework captures the rapidly increasing gas.
[0083] Hereinafter, a rechargeable lithium battery is described in detail without excluding any explanation overlapping with the above-mentioned contents.
[0084] Figure 2 is a perspective view of a pouch-type rechargeable battery according to an embodiment, Figure 3 For along Figure 2 A vertical cross-sectional view taken along line II in the direction of the arrow, and Figure 4 For along Figure 2 A horizontal cross-sectional view taken along the line II-II in the direction of the arrow in FIG. Herein, the rechargeable lithium battery according to the embodiment is described as an example in which a stacked electrode assembly is installed in a pouch-type case, but the present invention is not limited thereto and can be applied to batteries in which an electrode assembly of a stacked type, a wound type (core-wound type), a stacked and folded type, a Z-folded type, etc. is installed in a cylindrical, prismatic, coin-shaped, etc. case.
[0085] refer to Figure 2 to Figure 4 According to an embodiment, a pouch-type rechargeable battery 100 includes: an electrode assembly 10 having a separator 13 between a positive electrode 11 and a negative electrode 12; an external material 25 in which the electrode assembly 10 is accommodated; and a positive electrode terminal 21 and a negative electrode terminal 22, the positive electrode terminal 21 being electrically connected to the positive electrode 11, and the negative electrode terminal 22 being electrically connected to the negative electrode 12.
[0086] Meanwhile, the electrode assembly 10 may have a structure in which a plurality of square sheet-shaped positive electrodes 11 and a plurality of negative electrodes 12 are alternately stacked, with the separator 13 interposed therebetween. The embodiment is not limited thereto, and may have a structure in which one positive electrode 11 and one negative electrode 12 are stacked, with one separator 13 interposed therebetween. In addition, the electrode assembly may be formed into a structure in which a separator is interposed between a strip-shaped positive electrode and a negative electrode, and then wound.
[0087] In the electrode assembly 10 , the positive electrode uncoated region 11 a and the negative electrode uncoated region 12 a are provided at one end, and the positive electrode terminal 21 is attached to the positive electrode uncoated region 11 a by welding, and the negative electrode terminal 22 is attached to the negative electrode uncoated region 12 a by welding.
[0088] The positive electrode 11, the negative electrode 12, and the separator 13 may each be formed in a square sheet shape. The electrode assembly 10 may be received inside the exterior material 25 and sealed by a sealing portion 30 along the edge of the exterior material 25, but is not limited thereto.
[0089] The outer material 25 may include an upper outer material 25a and a lower outer material 25b. The upper outer material 25a and the lower outer material 25b may each have a multilayer structure. The structures of the upper outer material 25a and the lower outer material 25b are the same, and will be explained based on the upper outer material 25a as an example. The upper outer material 25a may have a configuration in which an outer resin layer, a metal layer, and an inner resin layer are stacked in sequence.
[0090] The sealing portion 30 may be located at the edge of the outer material 25, such as Figure 2 The insulating member 40 may be attached to each of the positive electrode terminal 21 and the negative electrode terminal 22 , but is not limited thereto.
[0091] Positive electrode
[0092] The positive electrode includes a current collector and a positive electrode active material layer on the current collector.
[0093] The positive electrode active material layer includes a positive electrode active material, and may further include a positive electrode binder and / or a conductive material.
[0094] As the positive electrode active material, a compound capable of reversibly intercalating and deintercalating lithium (lithiated intercalation compound) can be used. Examples of the positive electrode active material include compounds represented by any one of the following chemical formulas:
[0095] Li a A 1-b X b D2(0.90≤a≤1.8, 0≤b≤0.5);
[0096] Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05);
[0097] Li a E 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05);
[0098] Li a E 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05);
[0099] Lia Ni 1-b-c Co b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);
[0100] Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);
[0101] Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);
[0102] Li a Ni 1-b-c Mr b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α≤2);
[0103] Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);
[0104] Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);
[0105] Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);
[0106] Li a Ni b Coc Mn d G e O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1);
[0107] Li a NiG b O2(0.90≤a≤1.8,0.001≤b≤0.1);
[0108] Li a CoG b O2(0.90≤a≤1.8,0.001≤b≤0.1);
[0109] Li a Mn 1-b G b O2(0.90≤a≤1.8,0.001≤b≤0.1);
[0110] Li a Mn2G b O4(0.90≤a≤1.8,0.001≤b≤0.1);
[0111] Li a Mn 1-g G g PO4(0.90≤a≤1.8,0≤g≤0.5);
[0112] QO2;QS2;LiQS2;
[0113] V2O5;LiV2O5;
[0114] LiZO2;
[0115] LiNiVO4;
[0116] Li (3-f) J2(PO4)3(0≤f≤2);
[0117] Li (3-f) Fe2(PO4)3(0≤f≤2);
[0118] Li a FePO4(0.90≤a≤1.8).
[0119] In the above chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; and J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0120] The compound may have a coating on the surface, or may be mixed with another compound having a coating. The coating may include at least one coating element compound selected from the group consisting of an oxide of the coating element, a hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, and a hydroxycarbonate of the coating element. The compound for the coating may be amorphous or crystalline. The coating element included in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a combination thereof. The coating formation process may use a method that does not adversely affect the physical properties of the positive electrode active material, for example, spraying, dipping, and the like.
[0121] For example, the positive electrode may include a composite oxide of lithium and at least one metal selected from nickel, cobalt, manganese, and aluminum as a positive electrode active material.
[0122] The positive electrode active material may include, for example, a lithium nickel composite oxide represented by Chemical Formula 11.
[0123] [Chemical formula 11]
[0124] Li a11 Ni x11 M 11 y11 M 12 1-x11-y12 O2
[0125] In Chemical Formula 11, 0.9≤a11≤1.8, 0.3≤x11≤1, 0≤y11≤0.7, and M 11 and M 12 Independently selected from Al, B, Ce, Co, Cr, F, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W, Zr and combinations thereof.
[0126] In Chemical Formula 11, 0.4 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.6; 0.5 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.5; 0.6 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.4; 0.7 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.3; 0.8 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.2; or 0.9 ≤ x11 ≤ 1 and 0 ≤ y11 ≤ 0.1.
[0127] As a specific example, the second positive electrode active material may include a lithium nickel cobalt composite oxide represented by Chemical Formula 12.
[0128] [Chemical Formula 12]
[0129] Li a12 Ni x12 Co y12 M 13 1-x12-y12 O2
[0130] In Chemical Formula 12, 0.9 ≤ a12 ≤ 1.8, 0.3 ≤ x12 < 1, 0 < y12 ≤ 0.7, and M 13 is selected from Al, B, Ce, Cr, F, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W, Zr, and combinations thereof.
[0131] In Chemical Formula 12, 0.3 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.7; 0.4 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.6; 0.5 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.5; 0.6 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.4; 0.7 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.3; 0.8 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.2; or 0.9 ≤ x12 ≤ 0.99 and 0.01 ≤ y12 ≤ 0.1.
[0132] As a specific example, the positive electrode active material may include a lithium nickel cobalt composite oxide represented by Chemical Formula 13.
[0133] [Chemical Formula 13]
[0134] Li a13 Ni x13 Co y13 M 14 z13 M 15 1-x13-y13-z13 O2
[0135] In Chemical Formula 13, 0.9 ≤ a13 ≤ 1.8, 0.3 ≤ x13 ≤ 0.98, 0.01 ≤ y13 ≤ 0.69, 0.01 ≤ z13 ≤ 0.69, M14 is selected from Al, Mn and combinations thereof, and M 15 Selected from B, Ce, Cr, F, Mg, Mo, Nb, P, S, Si, Sr, Ti, V, W, Zr and combinations thereof.
[0136] In Chemical Formula 13, 0.4≤x13≤0.98, 0.01≤y13≤0.59, and 0.01≤z13≤0.59; 0.5≤x13≤0.98, 0.01≤y13≤0.49, and 0.01≤z13≤0.49; 0.6≤x13≤0.98, 0.01≤y13≤0.39, and 0.01≤z13≤0 .39; 0.7≤x13≤0.98, 0.01≤y13≤0.29, and 0.01≤z13≤0.29; 0.8≤x13≤0.98, 0.01≤y13≤0.19, and 0.01≤z13≤0.19; or 0.9≤x13≤0.98, 0.01≤y13≤0.09, and 0.01≤z13≤0.09.
[0137] For a more specific example, an LCO-based positive electrode active material, a high-nickel NCA-based positive electrode active material, a high-nickel NCM-based positive electrode active material, or a combination thereof (representatively, LiCoO2, LiNi 0.91 Co 0.07 Al 0.02 O2、LiNi 0.82 Co 0.11 Mn 0.07 O2 or a combination thereof) can be used as a positive electrode active material. These materials increase the amount of gas generated from the positive electrode during operation of a rechargeable lithium battery. Even in this case, a metal organic framework structure (such as ZIF-8, Fe-BTC or a combination thereof) can effectively capture the gas.
[0138] The positive electrode active material may contain 85 wt% to 99 wt%, such as 90 wt% to 95 wt%, based on the total weight of the positive electrode active material layer. The binder and the conductive material may contain 1 wt% to 5 wt% each.
[0139] The positive electrode binder improves the bonding properties between the positive electrode active material particles and the bonding properties between the positive electrode active material particles and the current collector. Examples thereof include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0140] The conductive material is used to impart conductivity to the electrode, and any material may be used as long as it does not cause chemical changes in the battery to be configured and is an electronic conductive material. Examples of the conductive material may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotube, etc.; metal-based materials including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0141] Aluminum foil may be used as the positive electrode current collector, but is not limited thereto.
[0142] Negative electrode
[0143] A negative electrode for a rechargeable lithium battery includes a current collector, and a negative electrode active material layer formed on the current collector and including a negative electrode active material.
[0144] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0145] The material that reversibly intercalates / deintercalates lithium ions may include, for example, crystalline carbon, amorphous carbon, or a combination thereof as a carbonaceous negative electrode active material. The crystalline carbon may be amorphous or flaky, thin, spherical or fibrous natural graphite or artificial graphite. The amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbonization product, calcined coke, etc.
[0146] Lithium metal alloys include alloys of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0147] Meanwhile, the negative electrode may include a carbon-based negative electrode active material, a silicon-based negative electrode active material, or a combination thereof as the negative electrode active material.
[0148] The material capable of being doped / undoped with lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may include silicon, a silicon-carbon composite, SiO x(0 < x < 2), Si-Q alloy (where Q is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, Group 15 element, Group 16 element, transition metal, rare earth element, and combinations thereof, but not Si), and the Sn-based negative electrode active material may include Sn, SnO2, Sn-R alloy (where R is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, Group 15 element, Group 16 element, transition metal, rare earth element, and combinations thereof, but not Sn). At least one of these materials may be mixed with SiO2. The elements Q and R may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0149] The silicon-carbon composite may be, for example, a silicon-carbon composite that includes a core containing crystalline carbon and silicon particles and an amorphous carbon coating provided on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon precursor may be coal tar pitch, mesophase pitch, petroleum pitch, coal tar, petroleum heavy oil, or a polymer resin (such as phenol resin, furan resin, or polyimide resin). In this case, based on the total weight of the silicon-carbon composite, the content of silicon may be 10 wt% to 50 wt%. Additionally, based on the total weight of the silicon-carbon composite, the content of crystalline carbon may be 10 wt% to 70 wt%, and based on the total weight of the silicon-carbon composite, the content of amorphous carbon may be 20 wt% to 40 wt%. Additionally, the thickness of the amorphous carbon coating may be 5 nm to 100 nm. The average particle size (D 50 ) of the silicon particles may be 10 nm to 20 μm. The average particle size (D 50 ) may preferably be 10 nm to 200 nm. The silicon particles may exist in an oxidized form, and in this case, the atomic content ratio of Si:O indicating the degree of oxidation in the silicon particles may be a weight ratio of 99:1 to 33:66. The silicon particles may be SiO x particles, and in this case, the range of x in SiO x may be greater than 0 and less than 2. In this specification, unless otherwise defined, the average particle size (D 50 ) indicates the diameter of the particles with a cumulative volume of 50% by volume in the particle size distribution.
[0150] The Si-based negative electrode active material or the Sn-based negative electrode active material may be mixed with the carbon-based negative electrode active material. When the Si-based negative electrode active material or the Sn-based negative electrode active material and the carbon-based negative electrode active material are mixed, the mixing ratio may be a weight ratio of 1:99 to 90:10. For example, a negative electrode active material in which silicon and artificial graphite are mixed at a ratio of 1:99 to 90:10 or 1:99 to 10:90 may be used.
[0151] In the negative electrode active material layer, the negative electrode active material may be included in an amount of 50 wt % to 99 wt % or 60 wt % to 95 wt % based on the total weight of the negative electrode active material layer.
[0152] In an embodiment, the negative electrode active material layer further includes a negative electrode binder and may optionally further include a conductive material. The negative electrode binder and the conductive material in the negative electrode active material layer may each contain 1 wt % to 5 wt % based on the total weight of the negative electrode active material layer.
[0153] The negative electrode binder is used to make the negative electrode active material particles bind well to each other, and also to make the negative electrode active material bind to the current collector. The binder may be a non-water-soluble binder, a water-soluble binder, or a combination thereof.
[0154] Examples of non-water-soluble binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, ethylene propylene copolymers, polystyrene, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0155] The water-soluble binder may include a rubber binder or a polymer resin binder. The rubber binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and combinations thereof. The polymer resin binder may be selected from polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and combinations thereof.
[0156] When a water-soluble binder is used as a negative electrode binder, a cellulose compound capable of imparting viscosity may be further included. As a cellulose compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose or an alkali metal salt thereof may be mixed and used. As an alkali metal, Na, K or Li may be used. Based on 100 parts by weight of the negative electrode active material, the amount of the thickener used may be 0.1 parts by weight to 3 parts by weight.
[0157] A conductive material is included to provide electrode conductivity. Any conductive material can be used as the conductive material unless it causes a chemical change in the battery. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotube, etc.; metal-based materials including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0158] The negative electrode current collector may include one selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0159] Diaphragm
[0160] The separator separates the positive electrode from the negative electrode and provides a transport channel for lithium ions, and can be any commonly used separator in a lithium ion battery. In other words, it can have low ion transport resistance and excellent impregnation of electrolyte. For example, the separator can be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene or a combination thereof. It can have the form of a non-woven fabric or a textile. For example, lithium ion batteries mainly use polyolefin polymer separators, such as polyethylene and polypropylene, and a coated separator including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and can be optionally used in a single layer or multilayer structure.
[0161] Electrolyte
[0162] The electrolyte may be a liquid electrolyte including a nonaqueous organic solvent and a lithium salt, which may be impregnated into the separator of the above-described embodiment (specifically, into the pores of the substrate).
[0163] The non-aqueous organic solvent is used as a medium for transmitting ions involved in the electrochemical reaction of the battery. The non-aqueous organic solvent can be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent or an aprotic solvent. The carbonate solvent can be dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The ester solvent can be methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolactone, valerolactone, mevalonolactone, caprolactone, etc. The ether solvent can be dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., and the ketone solvent can be cyclohexanone, etc. In addition, the alcohol solvent may be ethanol, isopropanol, etc., and the aprotic solvent may be a nitrile, such as R-CN (wherein R is a C2 to C20 straight chain, branched or cyclic hydrocarbon group, and may include a double bond, an aromatic ring or an ether bond), an amide (such as dimethylformamide), a dioxolane (such as 1,3-dioxolane), cyclopentane, etc.
[0164] The nonaqueous organic solvent may be used alone or in a mixture. When the organic solvent is used in a mixture, the mixture ratio may be controlled according to the desired battery performance.
[0165] In addition, in the case of carbonate-based solvents, a mixture of cyclic carbonate and chain carbonate may be used. In this case, when the cyclic carbonate and chain carbonate are mixed in a volume ratio of about 1:1 to 1:9, the electrolyte may exhibit excellent performance.
[0166] The non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of about 1:1 to about 30:1.
[0167] As the aromatic hydrocarbon solvent, an aromatic hydrocarbon compound represented by Chemical Formula I may be used.
[0168] [Chemical Formula I]
[0169]
[0170] In Formula I, R 4 To R 9 are the same or different and are selected from hydrogen, halogen, C1-C10 alkyl, haloalkyl and combinations thereof.
[0171] Specific examples of the aromatic hydrocarbon solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, , 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0172] The electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound of Chemical Formula II to improve the cycle life of the battery.
[0173] [Chemical Formula II]
[0174]
[0175] In Chemical Formula II, R 10 and R 11 are the same or different and are selected from hydrogen, halogen, cyano, nitro and C1-C5 fluorinated alkyl, provided that R 10 and R 11 At least one of them is selected from halogen, cyano, nitro and C1-C5 fluorinated alkyl, but R 10 and R 11 Not all are hydrogen.
[0176] Examples of ethylene carbonate compounds may be difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate or fluoroethylene carbonate. The amount of the additive for improving the cycle life may be used within an appropriate range.
[0177] The lithium salt dissolved in the non-organic solvent supplies lithium ions in the battery, ensures the basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode.
[0178] Examples of lithium salts may include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide): LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers, for example, integers ranging from 1 to 20), at least one of lithium difluoro(bis(oxalato)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB) and lithium difluoro(oxalato)borate (LiDFOB).
[0179] The lithium salt may be used in a concentration ranging from 0.1 M to 2.0 M. When the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0180] Meanwhile, as additives for the electrolyte, in addition to the aforementioned compounds, other additives may be further included.
[0181] Other additives may include at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate (VEC), propylene sultone (PST), propane sultone (PS), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2) and 2-fluorobiphenyl (2-FBP).
[0182] By further including the aforementioned other additives, the cycle life may be further improved, or the gas generated from the positive electrode and the negative electrode may be effectively controlled when stored at a high temperature.
[0183] The other additives may be included in an amount of 0.2 to 20 parts by weight, specifically 0.2 to 15 parts by weight, for example, 0.2 to 10 parts by weight, based on 100 parts by weight of the electrolyte for a rechargeable lithium battery.
[0184] When the contents of other additives are as described above, the increase in membrane resistance can be minimized, thereby contributing to the improvement of battery performance.
[0185] Rechargeable lithium batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries according to the presence of a separator and the type of electrolyte used therein. Rechargeable lithium batteries can have various shapes and sizes, and include cylindrical batteries, prismatic batteries, coin batteries, or pouch batteries, and can be thin film batteries or can be quite large in size. Because the structure and manufacturing methods of these batteries are well known in the art, a detailed description thereof will be omitted.
[0186] Hereinafter, examples of the present invention and comparative examples are described. However, it should be understood that these examples are for illustrative purposes and are not to be construed as limiting the present invention.
[0187] [Preparation Examples and Comparative Preparation Examples]
[0188] Preparation Example 1
[0189] A coating solution (solid content: 10 wt %) was prepared by mixing particulate PVdF as a binder and ZIF-8 as a metal organic framework at a weight ratio of 1:9 and dispersing the mixture in NMP as a solvent.
[0190] A commercially available separator having a three-layer structure of PP / PE / PP (width: 30 mm, length: 40 mm, air permeability: 121 sec / cc, thickness of each layer: 4 μm / 6 μm / 4 μm, total thickness: 14 μm) was used as a substrate and then immersed in a coating solution to form a coating on both surfaces thereof. In this article, the coating and the substrate are formed to have a thickness ratio (coating thickness / substrate thickness) of 1 / 10 and an area ratio (coating area / substrate area) of 1 (i.e., 100 sq%). Specifically, the thickness of the coating is 1.4 μm.
[0191] Preparation Example 2
[0192] A separator for a rechargeable lithium battery of Preparation Example 2 was manufactured in the same manner as Preparation Example 1, except that Fe-BTC was used instead of ZIF-8.
[0193] Comparative Preparation Example 1
[0194] The separator for a rechargeable lithium battery of Comparative Preparation Example 1 was manufactured in the same manner as Preparation Example 1, except that a separator having a three-layer structure of PP / PE / PP itself without a coating layer was used.
[0195] Comparative Preparation Example 2
[0196] A separator for a rechargeable lithium battery of Comparative Preparation Example 2 was manufactured in the same manner as Preparation Example 1, except that zeolite (product name: A-4 Zeolite, manufacturer: Nakamura Choukou Co., Ltd.) was used instead of ZIF-8.
[0197] Comparative Preparation Example 3
[0198] A separator for a rechargeable lithium battery of Comparative Preparation Example 3 was manufactured in the same manner as Preparation Example 1, except that MOF-5 represented by the following chemical formula was used instead of ZIF-8.
[0199]
[0200] Comparative Preparation Example 4
[0201] A separator for a rechargeable lithium battery of Comparative Preparation Example 4 was manufactured in the same manner as Preparation Example 1, except that MOF-74(Co) represented by the following chemical formula was used instead of ZIF-8.
[0202]
[0203] Comparative Preparation Example 5
[0204] A separator for a rechargeable lithium battery of Comparative Preparation Example 5 was manufactured in the same manner as Preparation Example 1, except that MOF-177 represented by the following chemical formula was used instead of ZIF-8.
[0205]
[0206] Comparative Preparation Example 6
[0207] A separator for a rechargeable lithium battery of Comparative Preparation Example 6 was manufactured in the same manner as Preparation Example 1, except that MOF-200 represented by the following chemical formula was used instead of ZIF-8.
[0208]
[0209] Comparative Preparation Example 7
[0210] A separator for a rechargeable lithium battery of Comparative Preparation Example 7 was manufactured in the same manner as Preparation Example 1, except that ZIF-67 represented by the following chemical formula was used instead of ZIF-8.
[0211]
[0212] Comparative Preparation Example 8
[0213] A separator for a rechargeable lithium battery of Comparative Preparation Example 8 was manufactured in the same manner as Preparation Example 1, except that ZIF-68 represented by the following chemical formula was used instead of ZIF-8.
[0214]
[0215] Comparative Preparation Example 9
[0216] A separator for a rechargeable lithium battery of Comparative Preparation Example 9 was manufactured in the same manner as Preparation Example 1, except that ZIF-69 represented by the following chemical formula was used instead of ZIF-8.
[0217]
[0218] Comparative Preparation Example 10
[0219] A separator for a rechargeable lithium battery of Comparative Preparation Example 10 was manufactured in the same manner as Preparation Example 1, except that ZIF-78 represented by the following chemical formula was used instead of ZIF-8.
[0220]
[0221] Comparative Preparation Example 11
[0222] A separator for a rechargeable lithium battery of Comparative Preparation Example 11 was manufactured in the same manner as Preparation Example 1, except that ZIF-81 represented by the following chemical formula was used instead of ZIF-8.
[0223]
[0224] Comparative Preparation Example 12
[0225] A separator for a rechargeable lithium battery of Comparative Preparation Example 12 was manufactured in the same manner as Preparation Example 1, except that MIL-53(Al) represented by the following chemical formula was used instead of ZIF-8.
[0226]
[0227] Comparative Preparation Example 13
[0228] A separator for a rechargeable lithium battery of Comparative Preparation Example 13 was manufactured in the same manner as Preparation Example 1, except that MIL-100(Fe) represented by the following chemical formula was used instead of ZIF-8.
[0229]
[0230] Comparative Preparation Example 14
[0231] A separator for a rechargeable lithium battery of Comparative Preparation Example 14 was manufactured in the same manner as Preparation Example 1, except that MIL-101(Fe) represented by the following chemical formula was used instead of ZIF-8.
[0232]
[0233] Comparative Preparation Example 15
[0234] A separator for a rechargeable lithium battery of Comparative Preparation Example 15 was manufactured in the same manner as Preparation Example 1, except that MIL-127(Fe) represented by the following chemical formula was used instead of ZIF-8.
[0235]
[0236] Comparative Preparation Example 16
[0237] A separator for a rechargeable lithium battery of Comparative Preparation Example 16 was manufactured in the same manner as Preparation Example 1, except that Cu-BTC represented by the following chemical formula was used instead of ZIF-8.
[0238]
[0239] Comparative Preparation Example 17
[0240] A separator for a rechargeable lithium battery of Comparative Preparation Example 17 was manufactured in the same manner as Preparation Example 1, except that UiO-66 represented by the following chemical formula was used instead of ZIF-8.
[0241]
[0242] Comparative Preparation Example 18
[0243] A separator for a rechargeable lithium battery of Comparative Preparation Example 18 was manufactured in the same manner as Preparation Example 1, except that CPO-27 represented by the following chemical formula was used instead of ZIF-8.
[0244] [Including LiNi 0.91 Co 0.07 Al 0.02 Rechargeable lithium battery with O2 positive electrode active material and PP / PE / PP separator]
[0245] Example 1-1
[0246] (1) Fabrication of negative electrode
[0247] A negative electrode active material slurry is prepared by mixing 70 wt % of a negative electrode active material of artificial graphite (D50: 16.6 μm) and silicon (D50: 18.0 μm) in a weight ratio of 9:1, 15 wt % of a conductive material (Super-P) and 15 wt % of a binder (PAA (polyacrylic acid)) in water as a solvent. The negative electrode active material slurry is coated on one surface of a copper foil having a thickness of 10 μm to a thickness of 140 μm, dried, and pressed to produce a negative electrode having a total thickness of 120 μm. In this article, die coating is used as a method for coating the negative electrode active material slurry. After coating, it is first dried at 60° C. in an air atmosphere for 1 hour, and then dried at 110° C. under vacuum conditions for 12 hours. The dried negative electrode plate is cut into 2.2×3.2 cm 2 size.
[0248] (2) Fabrication of positive electrode
[0249] By using 95wt% of LiNi as the positive electrode active material 0.91 Co 0.07 Al 0.02 O2, 3wt% of polyvinylidene fluoride as a binder and 2wt% of Ketjen black as a conductive material are mixed in N-methylpyrrolidone solvent to prepare a positive electrode active material. It is coated with a thickness of 164μm on one surface of an aluminum current collector with a thickness of 12μm, dried, and pressed to produce a positive electrode active material layer with a total thickness of 138μm. In this article, die coating is used as a method for coating the positive electrode active material slurry. After coating, it is first dried at 80°C in an air atmosphere for 1 hour, and vacuum dried at 120°C under vacuum conditions for 12 hours. The dried positive electrode plate is cut into 2×3cm 2 size.
[0250] (3) Manufacturing of battery cells
[0251] The separator of Preparation Example 1 was inserted between the negative electrode and the positive electrode to manufacture an electrode assembly. After the electrode assembly was inserted into a bag, an electrolyte was prepared by mixing ethylene carbonate and diethyl carbonate at a volume ratio of 30:70 and adding 1.5M LiPF6 lithium salt and 12.5wt% FEC in the mixed solvent to manufacture a rechargeable lithium battery cell.
[0252] Example 1-2
[0253] The separator for a rechargeable lithium battery of Example 1-2 was manufactured in the same manner as Example 1-1, except that the separator for a rechargeable lithium battery of Preparation Example 2 was used.
[0254] Comparative Example 1-1 to Comparative Example 1-18
[0255] Each separator for a rechargeable lithium battery of Comparative Examples 1-1 to 1-18 was manufactured in the same manner as Example 1-1, except that the separators for a rechargeable lithium battery of Comparative Preparation Examples 1 to 18 were used, respectively.
[0256] Evaluation Example 1: Including LiNi 0.91 Co 0.07 Al 0.02 Rechargeable O2 positive electrode active material and PP / PE / PP separator Evaluation of lithium battery cells
[0257] (1) Amount of gas generated during formation charge and discharge
[0258] The amount of gas generated during formation charge and discharge of each of the rechargeable lithium battery cells of Examples 1-1 to 1-2 and Comparative Examples 1-1 to 1-18 was evaluated, and the results are shown in Table 1.
[0259] Specifically, the formation charge and discharge of the rechargeable lithium battery cell was performed at 25° C. (room temperature) for 1 charge and discharge cycle under the following conditions.
[0260] Charging conditions: CC (constant current) / CV (constant voltage), 4.2V, 0.02C current cutoff
[0261] Discharge conditions: CC (constant current), 2.5V
[0262] After completing formation charge and discharge under this condition, each rechargeable lithium battery cell was extracted with a syringe and then injected into GC-MS to evaluate the amount of generated gas.
[0263] (2) Amount of gas generated during overcharge
[0264] The amount of gas generated during overcharging of the rechargeable lithium battery cells of Examples 1-1 to 1-2 and Comparative Examples 1-1 to 1-18 was evaluated, and the results are shown in Table 1.
[0265] Specifically, the amount of gas generated by the rechargeable lithium battery cells during overcharging was evaluated under the following conditions at ambient temperature in an explosion-proof chamber.
[0266] Overcharge conditions: 0.2C CC (constant current) charge, 10V, 7.5 hours.
[0267] After the overcharge was completed under this condition, the amount of generated gas was evaluated in the same manner as the method of evaluating the amount of gas generated during formation charge and discharge.
[0268] (3) The amount of gas generated when exposed to heat
[0269] The amount of gas generated by the rechargeable lithium battery cells of Examples 1-1 to 1-2 and Comparative Examples 1-1 to 1-18 when exposed to heat was evaluated, and the results are shown in Table 1.
[0270] Specifically, the rechargeable lithium battery cell was charged to 4.2 V at a cut-off current of 0.02 C, and then, heated to 140° C. at 5° C. / min, and left at 140° C. for 1 hour.
[0271] After the overcharge was completed under this condition, the amount of generated gas was evaluated in the same manner as the method of evaluating the amount of gas generated during formation charge and discharge.
[0272] (Table 1)
[0273]
[0274] Referring to Table 1, compared with the rechargeable lithium battery cells of Comparative Examples 1-1 to 1-18, the rechargeable lithium battery cells of Examples 1-1 and 1-2 show that a very small amount of gas is generated under conditions of formation charge and discharge, overcharge, heat exposure, etc. Accordingly, if a separator for a rechargeable lithium battery including a metal organic framework (such as ZIF-8, Fe-BTC, or a combination thereof) in a coating is provided inside the rechargeable lithium battery, the gas generated inside the rechargeable lithium battery under conditions such as formation charge and discharge, overcharge, heat exposure, etc. can be more effectively captured than any metal organic framework and zeolite to prevent an increase in battery volume and internal pressure.
[0275] On the other hand, in the rechargeable lithium battery cells of Examples 1-1 and 1-2, the battery cell of Example 1-1 using a sheet for a rechargeable lithium battery coated with ZIF-8 shows a significantly less amount of gas produced. According to MOF-related literature (Hasmukh A. Patel et al., ChemSusChem 2017, 10, 1303-1317), it is known that cations (such as zinc ions, etc.) increase polarity, thereby increasing the reaction area of the gas adsorption reaction, and it is known that anions (such as imidazole skeletons, etc.) provide non-shared electron pairs, thereby increasing the chemical adsorption of gas molecules. Gas molecules can be chemically adsorbed by cations / anions on the surface of MOF holes and physically adsorbed in non-polar regions (such as carbon, etc.), but as they move away from the hole surface, physical adsorption occurs mainly due to van der Waals forces rather than chemical adsorption. Accordingly, three factors (such as the binding force of cations / anions to gas molecules, the surface area of the material, and the size of the pores) should be maximized to maximize gas adsorption capacity. ZIF-8 had the greatest gas reduction effect, presumably having a structure that maximizes the effect of gas components generated from rechargeable lithium batteries.
[0276] [Rechargeable lithium battery including LiCoO2 positive electrode active material and PP / PE / PP separator]
[0277] Example 2-1 and Example 2-2
[0278] Each rechargeable lithium battery cell of Example 2-1 and Example 2-2 was manufactured in the same manner as Example 1-1 and Example 1-2, except that LiCoO2 was used instead of LiNi 0.91 Co 0.07 Al 0.02 O2 is used as the positive electrode active material.
[0279] Comparative Example 2-1 to Comparative Example 2-18
[0280] Each rechargeable lithium battery cell of Comparative Examples 2-1 to 2-18 was manufactured in the same manner as Comparative Examples 1-1 to 1-18, except that LiCoO2 was used instead of LiNi 0.91 Co 0.07 Al 0.02 O2 is used as the positive electrode active material.
[0281] Evaluation Example 2: Evaluation of a rechargeable lithium battery including a LiCoO2 positive electrode active material and a PP / PE / PP separator
[0282] The amount of gas generated by the rechargeable lithium battery cells of Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-18 under each condition of formation charge and discharge, overcharge and heat exposure was evaluated in the same manner as Evaluation Example 1, and the results are shown in Table 2.
[0283] (Table 2)
[0284]
[0285]
[0286] Referring to Table 2, compared with the rechargeable lithium battery cells of Comparative Examples 2-1 to Comparative Examples 2-18, the rechargeable lithium battery cells of Examples 2-1 and 2-2 show that the amount of gas generated under conditions such as formation charge and discharge, overcharge, heat exposure, etc. is very small. In addition, among the rechargeable lithium battery cells of Examples 2-1 and 2-2, the battery cell of Example 2-1 using the sheet for a rechargeable lithium battery coated with ZIF-8 shows significantly less gas generated. Accordingly, the same results as those of Evaluation Example 1 were obtained.
[0287] Evaluation Example 3: Evaluation of changes in the substrate of the separator and / or the positive electrode active material
[0288] Each diaphragm of Evaluation Example 3 is manufactured by changing the substrate and / or metal organic framework of the diaphragm from Preparation Example 1. Specifically, a diaphragm having a layer of PP structure (width: 30 mm, length: 40 mm, thickness: 14 μm, air permeability: 145 sec / cc, total thickness: 14 μm) or a diaphragm having a PP / PE / PP three-layer structure (width: 30 mm, length: 40 mm, porosity: 121 sec / cc, thickness of each layer: 4 μm / 6 μm / 4 μm, total thickness: 14 μm) is used. In addition, on the two entire surfaces of the isolation substrate, no coating including a metal organic framework is formed or a coating including ZIF-67, ZIF-8 or Fe-BTC is formed. Other matters other than this are the same as those in Preparation Example 1 to manufacture a diaphragm.
[0289] Subsequently, when the separator manufactured in the above method is used, LiNi 0.91 Co 0.07 Al 0.02 O2, LiCoO2, LiNi 0.82 Co 0.11 Mn 0.07 O2 or LiMn2O4 was used as the positive electrode active material. Matters other than this were the same as those in Example 1-1 to manufacture each rechargeable lithium battery cell of Evaluation Example 3.
[0290] The heat exposure of each rechargeable lithium battery cell of Evaluation Example 3 was evaluated under the same conditions as Evaluation Example 1, and the results of the amount of gas generated are shown in Table 3.
[0291] (Table 3)
[0292] (Unit: mL)
[0293]
[0294] Referring to Table 3, when the same separator substrate is used, the separator with ZIF-8 coating or Fe-BTC coating shows a very small amount of gas generation compared to the separator without coating or with ZIF-67 coating. On the other hand, when ZIF-8 or Fe-BTC is used as the separator coating material, the amount of gas generated is much lower than that of the PP single-layer separator when LiNi 0.91 Co 0.07 Al 0.02 O2, LiCoO2, LiNi 0.82 Co 0.11 Mn 0.07O2 or its combination as the positive electrode active material, PP / PE / PP separators show significantly high gas reduction effects. It is speculated that stacked separators have more excellent mechanical strength and therefore stronger resistance to shrinkage and deformation than single-layer separators, thereby relatively less interfering with the diffusion of gases generated, especially at high temperatures, to MOF. However, when the PP separator is combined with the LiMn2O4 positive electrode, ZIF-67 shows better gas capture effects than ZIF-8 and Fe-BTC. Accordingly, the gas capture effect can vary depending on the positive electrode and the separator combined therewith.
[0295] Evaluation Example 4: Evaluation of Changes in Binder: Metal Organic Framework and / or Solid Content in Coating Solutions
[0296] Each coating solution and diaphragm of Evaluation Example 4 was manufactured by changing the weight ratio and / or solid content of the binder: metal organic framework in the coating solution from Preparation Example 1. Specifically, when the weight ratio of the binder: metal organic framework was changed in the range of 0.3:9.7 to 5:5, a coating was formed on both surfaces of the substrate of the diaphragm by using ZIF-8 or Fe-BTC. Other matters were the same as in Preparation Example 1 to manufacture a diaphragm.
[0297] Each coating solution and separator of Evaluation Example 4 was evaluated under the following conditions, and the results are shown in Table 3.
[0298] Coating solution dispersion evaluation conditions: The solid content (binder + MOF) in the total weight of the coating solution (solvent + binder + MOF) was measured by using a hygrometer (infrared moisture analyzer, product name: MA35M-230N, manufacturer: Sartorius mechatronics). The closer the measured value is to the input reference value (10wt%), the higher the dispersibility.
[0299] Coating uniformity evaluation conditions: The coating thickness was measured at any 8 points in the diaphragm and its deviation was calculated.
[0300] (Table 4)
[0301]
[0302]
[0303] Referring to Table 4, if the solid content in the coating solution is the same, when the weight ratio of binder:MOF is in the range of 0.3:9.7 to 5:5 (specifically 0.4:9.6 to 5:5, more specifically 0.4:9.6 to 4:6), the dispersibility of the coating solution and the uniformity of the coating are improved.
[0304] Evaluation Example 5: Evaluation of an Example in Which the Thickness of the Coating is Changed
[0305] Each separator of Evaluation Example 5 was manufactured by changing the coating thickness of Preparation Example 1. Specifically, when the coating thickness of each surface of the separator was changed in the range of 0.05 μm to 30 μm, no coating was formed on both surfaces of the separator, or a coating was formed by using ZIF-8 or Fe-BTC. Other matters were the same as in Preparation Example 1 to manufacture a separator.
[0306] Subsequently, each rechargeable lithium battery cell of Evaluation Example 5 was manufactured in the same manner as in Example 1-1, except that the separators manufactured in the above-mentioned method were respectively used.
[0307] The amount of gas generated by the rechargeable lithium battery cells of Evaluation Example 5 during heat exposure under the same conditions as Evaluation Example 1 was evaluated, and the results are shown in Table 5.
[0308] (Table 5)
[0309] (Unit: mL)
[0310]
[0311] Referring to Table 5, as long as the separator has a coating formed by using ZIF-8 or Fe-BTC, the amount of gas generated in the rechargeable lithium battery cell is reduced regardless of the thickness of the coating. In particular, when the separator has a coating formed by using ZIF-8 or Fe-BTC, the coating having a thickness of 100 μm to 20 μm per surface of the separator shows the most excellent effect compared to the coating having a thickness of less than 100 μm, but has an equivalent effect in the case where the coating thickness is 20 μm or more.
[0312] While the present disclosure has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments. On the contrary, it is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims.
[0313] [Explanation of Reference Numerals]
[0314] 100: Pouch type rechargeable battery 10: Electrode assembly
[0315] 11: Positive electrode
[0316] 11a: Positive electrode uncoated area
[0317] 12: Negative electrode 12a: Negative electrode uncoated area
[0318] 13: Diaphragm
[0319] 21: Positive electrode terminal 22: Negative electrode terminal
[0320] 25: External materials
[0321] 25a: Upper outer material 25b: Lower outer material
[0322] 30: Sealing part
[0323] 40: Insulation components
Claims
1. A separator for a rechargeable lithium battery, comprising: substrate; and A coating is disposed on one or both surfaces of a substrate and includes a metal organic framework (MOF) of ZIF-8, Fe-BTC, or a combination thereof.
2. The separator for a rechargeable lithium battery according to claim 1, wherein The substrate includes a polyolefin.
3. The separator for a rechargeable lithium battery as claimed in claim 2, wherein The substrate is a laminate in which a first layer including polypropylene, a second layer including polyethylene, and a third layer including polypropylene are sequentially laminated.
4. The separator for a rechargeable lithium battery according to claim 1, wherein The coating further includes a binder.
5. The separator for a rechargeable lithium battery as claimed in claim 4, wherein The binder includes polyvinylidene fluoride (PVdF), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer, ethylene vinyl acetate (EVA), hydroxyethyl cellulose (HEC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), ethylene-acrylic acid copolymer, acrylonitrile, vinyl acetate derivatives, polyethylene glycol, acrylic rubber or a combination thereof.
6. The separator for a rechargeable lithium battery as claimed in claim 4, wherein The weight ratio of the binder to the metal organic framework in the coating is 0.3:9.7 to 5:
5.
7. The separator for a rechargeable lithium battery as claimed in claim 1, wherein The thickness ratio of the coating layer to the substrate (coating layer thickness / substrate thickness) on each surface of the substrate of the diaphragm is 1 / 1000 to 5.
8. The separator for a rechargeable lithium battery as claimed in claim 1, wherein The thickness of the coating layer on each surface of the substrate of the diaphragm is 50 nm to 30 μm.
9. The separator for a rechargeable lithium battery as claimed in claim 1, wherein The coating is completely coated on one surface of the substrate.
10. The separator for a rechargeable lithium battery as claimed in claim 1, wherein The coating is patterned in the form of a plurality of dots, lines, rings, or a combination thereof. 11 . A rechargeable lithium battery, comprising the separator for a rechargeable lithium battery according to claim 1 .
12. The rechargeable lithium battery of claim 11, wherein The rechargeable lithium battery includes an assembly in which the separator is located between a positive electrode and a negative electrode.
13. The rechargeable lithium battery of claim 11, wherein The positive electrode includes a composite oxide of lithium and at least one metal selected from nickel, cobalt, manganese, and aluminum as a positive electrode active material.