Method for manufacturing conductive substrate

Through the photo production method and the resist film treatment, the thickening of the intersection point of the conductive substrate and the line width problems are solved, and the conductive substrate manufacturing with thin line width and excellent conductivity is realized.

CN119096705APending Publication Date: 2024-12-06FUJIFILM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380035219.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when manufacturing a conductive substrate, the intersection portion of the plated resist pattern is prone to thicken, resulting in the intersection of the conductive thin lines also being thickened, and it is difficult to maintain the thin line width and excellent conductivity.

Method used

The photo production method is used to form a grid-shaped base silver pattern on the surface of the substrate, and a resist pattern is formed through exposure and development of the resist film to ensure that the intersection points of the conductive thin lines do not thicken, the line width is thin and the conductivity is excellent. .

Benefits of technology

It effectively suppresses the thickening of the intersection points of conductive thin lines, maintains the thin line width, and improves the conductivity, and is suitable for applications such as touch panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005093288290000091
    Figure BDA0005093288290000091
  • Figure BDA0005093288290000101
    Figure BDA0005093288290000101
  • Figure BDA0005093288290000111
    Figure BDA0005093288290000111
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for manufacturing a conductive substrate, which is capable of manufacturing a conductive substrate having a conductive thin wire that is suppressed in intersection thickening, has a thin wire width, and has excellent conductivity. A method for manufacturing a conductive substrate according to the present invention comprises: a step for forming a grid-shaped base silver pattern on one surface side of a base material by means of a photograph creation method; a step for disposing a resist film on the surface side of the base material on which the underlying silver pattern is formed; a step for exposing the resist film by irradiating light from the surface side of the substrate on which the underlying silver pattern is not formed; a step for developing the exposed resist film to form a resist pattern; and a step for performing plating treatment using the base silver pattern as a seed layer, and forming a metal pattern on the base silver pattern to obtain a conductive fine wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a conductive substrate. Background Art

[0002] Substrates having conductive fine wires (thin wires showing conductivity) (hereinafter also referred to as "conductive substrates") are widely used in various applications such as touch panels, solar cells, and EL (electroluminescent) elements. In particular, in recent years, the rate of touch panels being installed in mobile phones and portable game consoles has increased, and the demand for conductive substrates for touch panels with electrostatic capacitance that can detect multiple points has rapidly expanded.

[0003] For example, as shown in Patent Document 1, conductive fine wires can be formed by a semi-additive method including the following steps: using a negative photoresist to set a plating resist pattern for a metal wiring pattern on the surface of a first metal layer, performing electrolytic plating, peeling off the plating resist pattern, and then removing the first metal layer.

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-287953 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] The present inventors used the method described in Patent Document 1 to manufacture a conductive substrate having conductive fine wires. As a result, when forming a plating resist pattern, intersection thickening occurred, in which the line width of the opening of the plating resist pattern corresponding to the intersection of the conductive fine wires became thicker than that of the part not being the intersection. When forming conductive fine wires using the plating resist pattern having the above-mentioned intersection thickening, intersection thickening also occurred at the intersection of the formed conductive fine wires, and thus improvement was required.

[0009] Furthermore, in a conductive substrate, it is sometimes required that the conductive thin wires have a small line width and excellent conductivity.

[0010] Therefore, an object of the present invention is to provide a method for producing a conductive substrate capable of producing a conductive substrate having thin conductive wires with a thin line width and excellent conductivity, while suppressing thickening of intersections.

[0011] Means for solving technical problems

[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention. Specifically, they have found that the above-mentioned problems can be solved by the following configuration.

[0013] [1] A method for manufacturing a conductive substrate, comprising:

[0014] A step of forming a grid-like base silver pattern on one surface side of a substrate by a photo production method;

[0015] A step of disposing a resist film on the surface side of the substrate on which the base silver pattern is formed;

[0016] A step of irradiating light from the surface side of the substrate on which the base silver pattern is not formed to expose the resist film;

[0017] A step of developing the exposed resist film to form a resist pattern; and

[0018] The step of performing a plating treatment using the base silver pattern as a seed layer to form a metal pattern on the base silver pattern to obtain conductive fine wires.

[0019] [2] The method for producing a conductive substrate according to [1], wherein:

[0020] The intersection thickening rate of the conductive thin wires is 1.0 to 1.5.

[0021] [3] The method for producing a conductive substrate according to [1] or [2], wherein:

[0022] The conductive thin wires have a line width of 3.0 μm or less.

[0023] [4] The method for producing a conductive substrate according to any one of [1] to [3], wherein:

[0024] The thickness of the base silver pattern is 1.0 μm or less.

[0025] [5] The method for producing a conductive substrate according to any one of [1] to [4], wherein:

[0026] The ratio of the height of the conductive thin wire to the line width of the conductive thin wire is 1.10 or more.

[0027] Effects of the Invention

[0028] According to the present invention, it is possible to provide a method for producing a conductive substrate capable of producing a conductive substrate in which thickening of intersections is suppressed and conductive thin wires having a thin line width and excellent conductivity are formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a top view showing one embodiment of a grid-like base silver pattern.

[0030] Figure 2 It is a diagram for explaining the resist film arrangement step.

[0031] Figure 3 It is a diagram for explaining the resist film exposure step.

[0032] Figure 4 It is a diagram for explaining the resist film development step.

[0033] Figure 5 It is a diagram for explaining the process of forming the conductive thin wires.

[0034] Figure 6 It is a plan view showing an enlarged intersection portion of conductive thin wires for illustrating the thickened intersection.

[0035] Figure 7 It is a plan view showing an enlarged intersection portion of conductive thin wires for illustrating the thickened intersection. DETAILED DESCRIPTION

[0036] Hereinafter, the present invention will be described in detail.

[0037] Although the constituent elements described below are sometimes described based on representative embodiments of the present invention, the present invention is not limited to such embodiments.

[0038] The meaning of each description in this specification is shown below.

[0039] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0040] In the present specification, when two or more kinds of a certain component are present, the "content" of the component means the total content of these two or more kinds of components.

[0041] In this specification, "g" and "mg" respectively represent "mass g" and "mass mg".

[0042] In the present specification, "polymer" or "polymer compound" refers to a compound having a weight average molecular weight of 2000 or more. Here, the weight average molecular weight is defined as a polystyrene conversion value measured by GPC (Gel Permeation Chromatography).

[0043] In this specification, unless otherwise specified, angles represented by specific numerical values, and references to angles such as “parallel”, “perpendicular”, and “orthogonal” include error ranges generally permitted in the corresponding technical fields.

[0044] In the present specification, the "organic group" refers to a group containing at least one carbon atom.

[0045] The method for manufacturing a conductive substrate of the present invention comprises:

[0046] A step of forming a grid-like base silver pattern on one surface side of a substrate by a photo-making method (hereinafter also referred to as a "base silver pattern forming step");

[0047] A step of disposing a resist film on the surface side of the substrate on which the base silver pattern is formed (hereinafter also referred to as a "resist film disposing step");

[0048] A step of irradiating light from the surface side of the substrate on which the base silver pattern is not formed to expose the resist film (hereinafter also referred to as "resist film exposure step");

[0049] A step of developing the exposed resist film to form a resist pattern (hereinafter also referred to as a "resist film developing step"); and

[0050] A step of performing plating treatment using the base silver pattern as a seed layer to form a metal pattern on the base silver pattern to obtain conductive thin wires (hereinafter also referred to as a "conductive thin wire forming step").

[0051] According to the method for manufacturing a conductive substrate of the present invention, a conductive substrate having thin conductive wires with excellent conductivity and with suppressed intersection thickening can be manufactured. Although the mechanism by which a conductive substrate having the above characteristics can be manufactured according to the present invention is not clear, the inventors speculate as follows.

[0052] In the method for manufacturing a conductive substrate of the present invention, first, in the base silver pattern forming step, a grid-like base silver pattern is formed by a photo production method. At this time, since the photo production method is used, it is easy to form a contrast between the exposed part and the unexposed part, and a grid-like base silver pattern with suppressed intersection thickening can be formed. In addition, according to the photo production method, a base silver pattern with a thin line width can be easily formed.

[0053] Furthermore, when the resist film exposure step is performed after the resist film placement step, the resist film is exposed using the base silver pattern with suppressed intersection thickening as a mask, so that in the resist film development step performed subsequently, a resist pattern with suppressed intersection thickening having a shape corresponding to the base silver pattern can be generated. In addition, the resist pattern has an opening having a shape corresponding to the base silver pattern.

[0054] In the conductive fine wire forming process performed after the resist film development process, the opening of the resist pattern is plated to form a metal pattern. Therefore, the line width does not expand beyond the opening of the resist pattern and the metal pattern can be formed on the base silver pattern. Moreover, even if the metal pattern is thickened, the metal pattern is formed along the shape of the resist pattern, so it is easy to form a conductive fine wire with a thin line width and excellent conductivity. In addition, with respect to the above-mentioned resist pattern, since the thickening of the intersection is suppressed, a conductive fine wire with suppressed thickening of the intersection can be formed.

[0055] As a result, according to the method for producing a conductive substrate of the present invention, it is possible to produce a conductive substrate in which thickening of intersections is suppressed and conductive thin wires having a thin line width and excellent conductivity are formed.

[0056] Hereinafter, each step included in the method for producing a conductive substrate of the present invention and steps that may be included will be described.

[0057] <Base silver pattern forming process>

[0058] The method for producing a conductive substrate of the present invention includes a step of forming a grid-like base silver pattern on one surface side of a substrate by a photographic method (base silver pattern forming step).

[0059] In the present invention, "forming a grid-like base silver pattern by a photographic production method" means reducing the silver halide particles contained in the silver halide emulsion layer provided on the support to generate silver particles, thereby forming a silver layer and forming a grid-like base silver pattern.

[0060] As a photograph creating method, for example, the following methods (a) and (b) can be mentioned.

[0061] (a) A method for producing a photograph in which a material having a layer containing silver halide on a support is subjected to a development treatment to reduce the silver halide and precipitate the silver layer.

[0062] (b) A method for producing a photograph by developing a material having a physical development core layer and a layer containing silver halide in sequence on a support, causing the silver layer to precipitate onto the physical development core, and then washing with water to remove the unnecessary layer containing silver halide (silver complex salt diffusion transfer method).

[0063] The method for preparing the photograph in the base silver pattern forming step is not particularly limited, but is preferably carried out by the method (a) described above.

[0064] The grid-like base silver pattern will be described using the drawings.

[0065] Figure 1 This is a plan view showing an example of a grid-like base silver pattern.

[0066] like Figure 1 As shown in FIG. 1 , the grid shape refers to a shape composed of intersecting base silver thin wires 22 and including a plurality of non-thin wire portions (opening portions) 32 that are separated from each other. Figure 1 In the figure, the non-fine line portion 32 has a square shape with a side length of L, but the non-fine line portion of the grid pattern can be other shapes as long as it is the area demarcated by the base silver fine line 22, for example, it can be a polygon (for example, a triangle, a quadrilateral (rhombus, rectangle, etc.), a hexagon and a random polygon). In addition, the shape of the side can be a curved shape other than a straight line, or it can be an arc shape. In the case of setting it to an arc shape, for example, the two opposite sides can be set to an arc shape that bulges outward, and the other two opposite sides can be set to an arc shape that bulges inward. In addition, the shape of each side can also be set to a wavy line shape of a continuous arc bulging outward and an arc bulging inward. Of course, the shape of each side can be set to a sine curve.

[0067] The length L of one side of the square grid-shaped non-fine line portion 32 is not particularly limited, but is preferably less than 1500 μm, more preferably less than 1300 μm, and further preferably less than 1000 μm. The lower limit of the length L is not particularly limited, but is preferably greater than 5 μm, more preferably greater than 30 μm, and further preferably greater than 80 μm. When the length of one side of the non-fine line portion is within the above range, the transparency can be further well maintained, and when the conductive substrate is mounted on the front surface of the display device, the display can be visually recognized without any sense of incongruity.

[0068] From the viewpoint of visible light transmittance, the opening ratio of the base silver pattern is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. The upper limit is not particularly limited, but may be less than 100%.

[0069] The aperture ratio refers to the ratio (area ratio) of the area where the grid-shaped base silver pattern is not arranged to the total area of ​​the surface of the substrate on the side where the grid-shaped base silver pattern is formed.

[0070] The base silver pattern forming step is not particularly limited as long as a grid-shaped base silver pattern is formed by a photographic method, but is preferably a base substrate silver pattern forming step including the following steps A to D in order.

[0071] Step A: forming a silver halide-containing photosensitive layer (hereinafter also referred to as a "photosensitive layer") containing silver halide, gelatin, and a polymer compound different from gelatin (hereinafter also referred to as a "specific polymer") on a substrate

[0072] Step B: After exposing the silver halide-containing photosensitive layer, developing the layer to form a thin line-shaped silver-containing layer containing metallic silver, gelatin and a specific polymer

[0073] Step C: a step of heating the silver-containing layer obtained in step B

[0074] Step D: a step of removing gelatin from the silver-containing layer obtained in step C to form a base silver pattern

[0075] Hereinafter, step A to step D will be described.

[0076] [Process A]

[0077] Step A is a step of forming a photosensitive layer (silver halide-containing photosensitive layer) containing silver halide, gelatin and a specific polymer (a polymer compound different from gelatin) on a substrate. Step A produces a substrate with a photosensitive layer subjected to an exposure treatment described later.

[0078] First, materials (substrate, silver halide, gelatin, and specific polymer) preferably used in the production of the substrate with a photosensitive layer are described, and then the steps of step A are described in detail.

[0079] (Base material)

[0080] As for the substrate, as long as it can transmit the exposure light used in the resist film exposure process, there is no particular restriction, and plastic substrates, glass substrates and metal substrates can be cited, preferably plastic substrates. The material of the substrate can be selected as long as it corresponds to the wavelength of the exposure light used in the resist film exposure process described later. The transmittance of the substrate at the wavelength of the exposure light used in the resist film exposure process is preferably 30% or more, more preferably 50% or more, and further preferably 70% or more. There is no particular restriction on the upper limit, and 100% can be cited. The above transmittance can be measured using a commercially available spectrophotometer.

[0081] As the substrate, from the viewpoint of excellent bendability of the obtained conductive substrate, a flexible substrate is preferably used. As the flexible substrate, the above-mentioned plastic substrate can be cited. In addition, flexibility refers to a substrate that can be bent, specifically, it means that even if it is bent with a bending radius of 2mm, it will not break. The flexible substrate has processability that can be formed into a three-dimensional shape.

[0082] The thickness of the substrate is not particularly limited, but is generally 25 to 500 μm. When the conductive substrate is used in a touch panel and the surface of the substrate is used as a touch surface, the thickness of the substrate may exceed 500 μm.

[0083] As the material constituting the substrate, preferably, resins having a melting point of about 290°C or less such as polyethylene terephthalate (PET) (258°C), polycycloolefin (134°C), polycarbonate (250°C), acrylic film (128°C), polyethylene naphthalate (269°C), polyethylene (135°C), polypropylene (163°C), polystyrene (230°C), polyvinyl chloride (180°C), polyvinylidene chloride (212°C) and triacetyl cellulose (290°C) are used, and PET, polycycloolefin or polycarbonate is more preferred. Among them, PET is particularly preferred from the viewpoint of excellent adhesion to the base silver pattern. The numerical values ​​in the above () are melting points or glass transition temperatures.

[0084] As a material constituting the substrate, polyimide may be selected as long as it transmits the exposure light used in the resist film exposure step.

[0085] The total light transmittance of the substrate is preferably 85 to 100%. The total light transmittance is measured using "Plastics - Method for determining total light transmittance and total light reflectance" specified in JIS (Japanese Industrial Standards) K7375:2008.

[0086] A primer layer may be disposed on the surface of the substrate.

[0087] The primer layer preferably contains a specific polymer described below. When the primer layer is used, the adhesion of the conductive thin wires described below to the substrate is further improved.

[0088] The formation method of the primer layer is not particularly limited, for example, the following method can be cited: a primer layer forming composition comprising a specific polymer described later is applied to a substrate, and heat treated as required. As required, a solvent can be included in the primer layer forming composition. The type of solvent is not particularly limited, and the solvent used in the photosensitive layer forming composition described later can be exemplified. In addition, as the primer layer forming composition comprising a specific polymer, a latex containing particles of the specific polymer can be used.

[0089] The thickness of the primer layer is not particularly limited, but is preferably 0.02 to 0.3 μm, more preferably 0.03 to 0.2 μm, from the viewpoint of better adhesion of the conductive layer to the substrate.

[0090] (Silver Halide)

[0091] The halogen atom contained in the silver halide can be any one of a chlorine atom, a bromine atom, an iodine atom and a fluorine atom, or a combination thereof. For example, preferably, a silver halide with silver chloride, silver bromide or silver iodide as the main body, more preferably a silver halide with silver chloride or silver bromide as the main body. In addition, silver chlorobromide, silver iodochlorobromide or silver iodobromide can also be preferably used.

[0092] Here, for example, "silver halide mainly composed of silver chloride" refers to a silver halide in which the molar fraction of chloride ions in the total halide ions in the silver halide composition is 50% or more. The silver halide mainly composed of silver chloride may contain bromide ions and / or iodide ions in addition to chloride ions.

[0093] Silver halide is usually in the form of solid particles, and the average particle size of the silver halide is preferably 10 to 1000 nm in terms of spherical equivalent diameter, more preferably 10 to 200 nm, and further preferably 50 to 150 nm from the viewpoint of smaller change in resistance value of the conductive thin wire formed in a hot and humid environment.

[0094] In addition, the spherical equivalent diameter refers to the diameter of a spherical particle having the same volume.

[0095] The "spherical equivalent diameter" used as the average particle size of the above-mentioned silver halide is an average value, and is a value obtained by measuring the spherical equivalent diameters of 100 silver halides and arithmetically averaging them.

[0096] The shape of the silver halide particles is not particularly limited, and examples thereof include spherical, cubic, flat (hexagonal, triangular, quadrilateral, etc.) flat, octahedral, and tetradecahedral shapes.

[0097] (gelatin)

[0098] The type of gelatin is not particularly limited, and examples thereof include lime-treated gelatin and acid-treated gelatin. In addition, gelatin hydrolysates, gelatin enzymatic decomposition products, and gelatin modified with amino groups and / or carboxyl groups (phthalated gelatin and acetylated gelatin) can be used.

[0099] (Specific polymer)

[0100] The specific polymer is a polymer compound different from the above-mentioned gelatin. When the photosensitive layer contains the specific polymer, the strength of the base silver pattern formed by the photosensitive layer is easily improved.

[0101] The type of the specific polymer is not particularly limited as long as it is different from gelatin, but is preferably a polymer that is not decomposed by a proteolytic enzyme or oxidizing agent that decomposes gelatin as described below.

[0102] Examples of specific polymers include hydrophobic polymers (water-insoluble polymers), for example, at least one resin selected from the group consisting of (meth)acrylic resins, styrene resins, vinyl resins, polyolefin resins, polyester resins, polyurethane resins, polyamide resins, polycarbonate resins, polydiene resins, epoxy resins, silicone resins, cellulose polymers and chitosan polymers, or a copolymer containing monomers constituting these resins.

[0103] Furthermore, the specific polymer preferably has a reactive group that reacts with a cross-linking agent described below.

[0104] The specific polymer is preferably in a particle form. That is, the silver-containing layer formed of the photosensitive layer preferably contains particles of the specific polymer.

[0105] As the specific polymer, a polymer (copolymer) represented by the following general formula (1) is preferred.

[0106] General formula (1): -(A) x -(B) y -(C) z -(D) w -

[0107] In the general formula (1), A, B, C and D each represent a repeating unit represented by the following general formulae (A) to (D).

[0108] [Chemical formula 1]

[0109]

[0110] R 11 represents a methyl group or a halogen atom, and is preferably a methyl group, a chlorine atom or a bromine atom. p represents an integer of 0 to 2, and is preferably 0 or 1, and more preferably 0.

[0111] R 12 It represents a methyl group or an ethyl group, and is preferably a methyl group.

[0112] R 13 represents a hydrogen atom or a methyl group, preferably a hydrogen atom. L represents a divalent linking group, preferably a group represented by the following general formula (2).

[0113] General formula (2): -(CO-X 1 )rX 2 -

[0114] In the general formula (2), X 1 Represents oxygen atom or -NR 30 -. Here, R 30represents a hydrogen atom, an alkyl group, an aryl group or an acyl group, and each of them may have a substituent (for example, a halogen atom, a nitro group and a hydroxyl group). 30 , preferably a hydrogen atom, an alkyl group having 1 to 10 carbon atoms (for example, methyl, ethyl, n-butyl, and n-octyl), or an acyl group (for example, acetyl and benzoyl). 1 , preferably an oxygen atom or -NH-.

[0115] X 2 represents an alkylene group, an arylene group, an alkylenearylene group, an arylenealkylene group or an alkylenearylenealkylene group, and -O-, -S-, -CO-, -COO-, -NH-, -SO2-, -N(R 31 )-or-N(R 31 )SO2- etc. 31 represents a linear or branched alkyl group having 1 to 6 carbon atoms. 2 , preferably dimethylene, trimethylene, tetramethylene, o-phenylene, m-phenylene, p-phenylene, -CH2CH2OCOCH2CH2- or -CH2CH2OCO(C6H4)-.

[0116] r represents 0 or 1.

[0117] q represents 0 or 1, and is preferably 0.

[0118] R 14 It represents an alkyl group, an alkenyl group or an alkynyl group, and is preferably an alkyl group having 5 to 50 carbon atoms, more preferably an alkyl group having 5 to 30 carbon atoms, and further preferably an alkyl group having 5 to 20 carbon atoms.

[0119] R 15 Represents a hydrogen atom, a methyl group, an ethyl group, a halogen atom, or -CH2COOR 16 , preferably a hydrogen atom, a methyl group, a halogen atom or -CH2COOR 16 , more preferably a hydrogen atom, a methyl group or -CH2COOR 16 , and more preferably a hydrogen atom.

[0120] R 16 represents a hydrogen atom or an alkyl group having 1 to 80 carbon atoms, and may be combined with R 14 Same or different, R 16 The number of carbon atoms in alkylene oxide is preferably 1-70, more preferably 1-60.

[0121] In the general formula (1), x, y, z and w represent the molar ratio of each repeating unit.

[0122] x is 3 to 60 mol %, preferably 3 to 50 mol %, more preferably 3 to 40 mol %.

[0123] y is 30 to 96 mol %, preferably 35 to 95 mol %, more preferably 40 to 90 mol %.

[0124] z is 0.5 to 25 mol %, preferably 0.5 to 20 mol %, more preferably 1 to 20 mol %.

[0125] w is 0.5 to 40 mol %, preferably 0.5 to 30 mol %.

[0126] In the general formula (1), it is preferred that x is 3 to 40 mol %, y is 40 to 90 mol %, z is 0.5 to 20 mol %, and w is 0.5 to 10 mol %.

[0127] As the polymer represented by the general formula (1), a polymer represented by the following general formula (2) is preferred.

[0128] [Chemical formula 2]

[0129]

[0130] In the general formula (2), x, y, z and w are as defined above.

[0131] The polymer represented by the general formula (1) may contain other repeating units in addition to the repeating units represented by the above-mentioned general formulae (A) to (D).

[0132] As the monomer for forming other repeating units, for example, acrylates, methacrylates, vinyl esters, olefins, crotonates, itaconic acid diesters, maleic acid diesters, fumaric acid diesters, acrylamides, unsaturated carboxylic acids, allyl compounds, vinyl ethers, vinyl ketones, vinyl heterocyclic compounds, glycidyl esters and unsaturated nitriles can be cited. As these monomers, they are also recorded in paragraphs

[0010] to

[0022] of Japanese Patent Gazette No. 3754745. From the viewpoint of hydrophobicity, acrylates or methacrylates are preferred, and hydroxyalkyl methacrylate or hydroxyalkyl acrylate is more preferred.

[0133] The polymer represented by the general formula (1) preferably contains a repeating unit represented by the general formula (E).

[0134] [Chemical formula 3]

[0135]

[0136] In the above formula, L E The group represents an alkylene group, and is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 2 to 6 carbon atoms, and further preferably an alkylene group having 2 to 4 carbon atoms.

[0137] As the polymer represented by the general formula (1), a polymer represented by the following general formula (3) is preferred.

[0138] [Chemical formula 4]

[0139] General formula (3)

[0140]

[0141] In the above formula, a1, b1, c1, d1 and e1 represent the molar ratio of each repeating unit, a1 represents 3 to 60 (mol%), b1 represents 30 to 95 (mol%), c1 represents 0.5 to 25 (mol%), d1 represents 0.5 to 40 (mol%), and e1 represents 1 to 10 (mol%).

[0142] The preferred range of a1 is the same as the preferred range of x, the preferred range of b1 is the same as the preferred range of y, the preferred range of c1 is the same as the preferred range of z, and the preferred range of d1 is the same as the preferred range of w.

[0143] e1 is 1 to 10 mol %, preferably 2 to 9 mol %, more preferably 2 to 8 mol %.

[0144] The specific polymer can be synthesized with reference to, for example, Japanese Patent No. 3305459 and Japanese Patent No. 3754745.

[0145] The weight average molecular weight of the specific polymer is not particularly limited, but is preferably 1,000 to 1,000,000, more preferably 2,000 to 750,000, and even more preferably 3,000 to 500,000.

[0146] (Other materials)

[0147] The photosensitive layer may contain other materials in addition to the above-mentioned materials as needed.

[0148] As other materials, for example, metal compounds belonging to Group 8 or Group 9, such as rhodium compounds and iridium compounds, which are used for stabilization and high sensitivity of silver halide, can be cited. Alternatively, as other materials, antistatic agents, nucleation accelerators, spectral sensitizing dyes, surfactants, antifogging agents, hardeners, anti-black spot agents, redox compounds, monomethine compounds, and dihydroxybenzenes described in paragraphs

[0220] to

[0241] of Japanese Patent Application Laid-Open No. 2009-004348 can also be cited.

[0149] In the method of photograph production, when the method (b) is used, other materials may include physical development cores, such as colloids of gold, silver, etc., and metal sulfides obtained by mixing water-soluble salts of palladium, zinc, etc. and sulfides.

[0150] Furthermore, the photosensitive layer may contain a crosslinking agent for crosslinking the above-mentioned specific polymers. By containing the crosslinking agent, the specific polymers are crosslinked, and even when the gelatin is decomposed and removed, the connection between the metallic silver in the layer formed by the photosensitive layer can be maintained.

[0151] In addition, in the photograph production method, when the method (b) is used, a physical development core layer containing a physical development core can be provided between the substrate and the photosensitive layer. The physical development core contained in the physical development core layer is as described above. For the formation method of the physical development core layer, reference can be made to paragraphs

[0007] to

[0016] of Japanese Patent Publication No. 5-265162.

[0152] (Steps of Process A)

[0153] The method for forming the photosensitive layer containing the above-mentioned components in step A is not particularly limited, but from the viewpoint of productivity, a method in which a photosensitive layer-forming composition containing silver halide, gelatin and a specific polymer is brought into contact with a substrate to form the photosensitive layer on the substrate is preferred.

[0154] Hereinafter, the form of the photosensitive layer-forming composition used in this method will be described in detail, and then the process steps will be described in detail.

[0155] (Materials Contained in the Photosensitive Layer-Forming Composition)

[0156] The photosensitive layer forming composition contains the above-mentioned silver halide, gelatin and specific polymer. In addition, the specific polymer may be contained in the photosensitive layer forming composition in the form of particles as required.

[0157] The photosensitive layer-forming composition may contain a solvent as needed.

[0158] Examples of the solvent include water, organic solvents (for example, alcohols, ketones, amides, sulfoxides, esters, and ethers), ionic liquids, and mixed solvents thereof.

[0159] The method of bringing the photosensitive layer-forming composition into contact with the substrate is not particularly limited, and examples thereof include a method of applying the photosensitive layer-forming composition on the substrate and a method of immersing the substrate in the photosensitive layer-forming composition.

[0160] Furthermore, after the above treatment, a drying treatment may be performed as necessary.

[0161] (Photosensitive layer containing silver halide)

[0162] The photosensitive layer (silver halide-containing photosensitive layer) formed through the above steps contains silver halide, gelatin, and a specific polymer.

[0163] The content of silver halide in the photosensitive layer is not particularly limited, but is preferably 1.0 to 10.0 g / m in terms of silver from the viewpoint of functioning as a self-aligned mask pattern in the resist film exposure step described later and suppressing line width deviation of fine lines of the base silver pattern formed after the development treatment described later. 2 , more preferably 2.0 to 7.0 g / m 2 Silver conversion refers to the mass of silver produced when all silver halides are reduced.

[0164] The content of the specific polymer in the photosensitive layer is not particularly limited, but is preferably 0.04 to 2.0 g / m 2 from the viewpoint of achieving better formation of a plated metal pattern and flexibility on the surface of the base layer. 2 , more preferably 0.08 to 1.0 g / m 2 .

[0165] [Process B]

[0166] Step B is a step of exposing the photosensitive layer and then developing the photosensitive layer to form a thin line-shaped silver-containing layer containing metallic silver, gelatin, and a specific polymer.

[0167] By subjecting the photosensitive layer to exposure processing, a latent image is formed in the exposed area.

[0168] The exposure may be performed in a pattern. For example, in order to obtain a mesh pattern composed of conductive thin wires described later, exposure may be performed through a mask having a mesh opening pattern or by scanning a laser beam to perform exposure in a mesh pattern.

[0169] The type of light used for exposure is not particularly limited as long as it can form a latent image on the silver halide, and examples thereof include visible light, ultraviolet light, and X-rays.

[0170] When the exposure is performed using a mask, it is preferred that the exposure treatment be performed with the mask in contact with the photosensitive layer from the viewpoint of further suppressing the thickening of the intersections.

[0171] By subjecting the exposed photosensitive layer to a development process, metallic silver is precipitated in the exposed region (region where the latent image is formed).

[0172] The method of the development treatment is not particularly limited, and examples thereof include known methods used for silver salt photographic films, printing papers, films for printing plate making, and emulsion masks for photomasks.

[0173] In the development treatment, a developer is usually used. The type of the developer is not particularly limited, and examples thereof include PQ (phenidone hydroquinone) developer, MQ (metol hydroquinone) developer, and MAA (metol ascorbic acid) developer.

[0174] The developability of the photosensitive layer is determined by the wavelength of the light source and its light quantity, and the sensitivity characteristics of the photosensitive layer. However, in order to obtain a base silver pattern with a desired line width, for example, it is sufficient to adjust the light quantity during exposure.

[0175] Step B may further include a fixing treatment for removing and stabilizing the silver halide in the unexposed portion.

[0176] The fixing treatment is performed simultaneously with the development and / or after the development. The method of the fixing treatment is not particularly limited, and examples thereof include methods used for silver salt photographic films, printing papers, films for printing plates, and latex masks for photomasks.

[0177] In the fixing process, a fixing solution is usually used. The type of the fixing solution is not particularly limited, and examples thereof include the fixing solutions described in "Chemistry of Photography" (written by Sasai, Photo Industry Publishing Co., Ltd.), p. 321.

[0178] By performing the above-mentioned treatment, a thin line-shaped silver-containing layer containing metallic silver, gelatin, and a specific polymer is formed, and an insulating layer containing no metallic silver but gelatin and a specific polymer is formed.

[0179] As a method of adjusting the width of the silver-containing layer, for example, there is a method of adjusting the opening width of a mask used in exposure.

[0180] Furthermore, when a mask is used during exposure, the width of the formed silver-containing layer can be adjusted by adjusting the exposure amount. For example, when the opening width of the mask is narrower than the width of the target silver-containing layer, the width of the area where the latent image is formed can be adjusted by increasing the exposure amount compared to normal. That is, the line width of the silver-containing layer and the formed conductive fine line can be adjusted by the exposure amount.

[0181] Furthermore, when a laser beam is used, the exposure area can be adjusted by adjusting the focusing range and / or scanning range of the laser beam.

[0182] The width of the silver-containing layer is preferably 0.5 μm or more and less than 5.0 μm, and is more preferably 3.0 μm or less, and further preferably 1.4 μm or less, from the viewpoint of making the formed conductive thin wires difficult to visually recognize.

[0183] The silver-containing layer obtained by the above steps is in the form of thin lines, and the width of the silver-containing layer refers to the length (width) of the silver-containing layer in a direction perpendicular to the direction in which the thin line-shaped silver-containing layer extends.

[0184] [Process C]

[0185] Step C is a step of heat treating the silver-containing layer and the insulating layer (hereinafter, both are also referred to as "silver-containing layer, etc.") obtained in step B. By performing this step, the specific polymers in the silver-containing layer, etc. are welded together, thereby improving the strength of the silver-containing layer, etc.

[0186] The method of heat treatment is not particularly limited, and examples thereof include a method of bringing the silver-containing layer into contact with superheated steam and a method of heating using a temperature control device (eg, a heater). Preferably, the silver-containing layer is brought into contact with superheated steam.

[0187] The superheated steam may be superheated steam or steam obtained by mixing other gases with superheated steam.

[0188] The contact time between the superheated steam and the silver-containing layer etc. is not particularly limited, but is preferably 10 to 70 seconds.

[0189] The supply rate of superheated steam is preferably 500 to 600 g / m 3 The temperature of the superheated steam is preferably 100 to 160° C. (preferably 100 to 120° C.) at 1 atmosphere.

[0190] As heating conditions in the method of heating the silver-containing layer etc. using a temperature control device, heating at 100 to 200° C. (preferably 100 to 150° C.) for 1 to 240 minutes (preferably 60 to 150 minutes) is preferable.

[0191] [Process D]

[0192] Step D is a step of removing gelatin from the silver-containing layer or the like obtained in step C. By carrying out this step, gelatin is removed from the silver-containing layer or the like, and a space is formed in the silver-containing layer or the like.

[0193] The method for removing gelatin is not particularly limited, and examples thereof include a method using a proteolytic enzyme (hereinafter also referred to as "method 1") and a method using an oxidizing agent to decompose and remove gelatin (hereinafter also referred to as "method 2").

[0194] Examples of the proteolytic enzyme used in method 1 include known plant or animal enzymes that can hydrolyze proteins such as gelatin. Examples of the proteolytic enzyme include pepsin, rennet, trypsin, chymotrypsin, cathepsin, papain, ficin, thrombin, renin, collagenase, bromelain, and bacterial proteases, preferably trypsin, papain, ficin, or bacterial proteases.

[0195] The step in method 1 may be any method as long as it is a method of contacting the silver-containing layer etc. with the above-mentioned proteolytic enzyme, for example, a method of contacting the silver-containing layer etc. with a treatment solution containing a proteolytic enzyme (hereinafter also referred to as "enzyme solution") can be mentioned. As the contact method, a method of immersing the silver-containing layer etc. in the enzyme solution and a method of coating the silver-containing layer etc. with the enzyme solution can be mentioned.

[0196] The content of the proteolytic enzyme in the enzyme solution is not particularly limited, but is preferably 0.05 to 20% by mass, more preferably 0.5 to 10% by mass, based on the total amount of the enzyme solution, from the viewpoint of easily controlling the degree of decomposition and removal of gelatin.

[0197] The enzyme solution generally contains water in addition to the above-mentioned proteolytic enzyme.

[0198] If necessary, other additives (eg, pH buffers, antimicrobial compounds, wetting agents, and preservatives) may be included in the enzyme solution.

[0199] The pH of the enzyme solution is selected so as to maximize the action of the enzyme, and is usually preferably 5 to 9.

[0200] The temperature of the enzyme solution is preferably a temperature at which the action of the enzyme increases, and specifically, 25 to 45°C is preferred.

[0201] Furthermore, if necessary, after the treatment with the enzyme solution, the obtained silver-containing layer may be subjected to a cleaning treatment such as washing with hot water.

[0202] The cleaning method is not particularly limited, but is preferably a method of bringing the silver-containing layer into contact with hot water. Examples thereof include a method of immersing the silver-containing layer in hot water and a method of applying hot water to the silver-containing layer.

[0203] The temperature of the hot water can be appropriately selected to be the optimal temperature depending on the type of the proteolytic enzyme used, but is preferably 20 to 80° C., more preferably 40 to 60° C., from the viewpoint of productivity.

[0204] The contact time (cleaning time) of the hot water with the silver-containing layer and the like is not particularly limited, but is preferably 1 to 600 seconds, more preferably 30 to 360 seconds, from the viewpoint of productivity.

[0205] The oxidant used in method 2 may be any oxidant capable of decomposing gelatin, and is preferably an oxidant having a standard electrode potential of +1.5 V or more. In this case, the standard electrode potential refers to the standard electrode potential (25°C, E 0 ).

[0206] As the above-mentioned oxidizing agent, for example, persulfuric acid, percarbonic acid, perphosphoric acid, hypochlorous acid, peracetic acid, meta-chloroperbenzoic acid, hydrogen peroxide, perchloric acid, periodic acid, potassium permanganate, ammonium persulfate, ozone, hypochlorous acid or its salts, etc. can be mentioned, but from the viewpoint of productivity and economy, hydrogen peroxide (standard electrode potential: 1.76V), hypochlorous acid or its salts are preferred, and sodium hypochlorite is more preferred.

[0207] As the step in method 2, any method may be used as long as it is a method of bringing the silver-containing layer etc. into contact with the above-mentioned oxidant, for example, a method of bringing the silver-containing layer etc. into contact with a treatment solution containing an oxidant (hereinafter also referred to as "oxidant solution") can be cited. As the contact method, a method of immersing the silver-containing layer etc. in the oxidant solution and a method of coating the silver-containing layer etc. with the oxidant solution can be cited.

[0208] The type of solvent contained in the oxidizing agent liquid is not particularly limited, and examples thereof include water and organic solvents.

[0209] [Process E]

[0210] The base silver pattern forming step may further include a step E of performing a smoothing treatment after the step D. By performing the step E, a conductive thin wire having a more excellent handling resistance (film strength) can be obtained.

[0211] The method of the smoothing treatment is not particularly limited, and for example, it is preferable to pass the substrate having the silver-containing layer etc. through a calendering treatment step between at least a pair of rollers under pressure. Hereinafter, the smoothing treatment using calendering rollers is referred to as calendering treatment.

[0212] Examples of the roll used for the calendering process include a plastic roll and a metal roll. From the viewpoint of preventing wrinkles, a plastic roll is preferred.

[0213] The pressure between the rolls is not particularly limited, but is preferably 2 MPa or more, more preferably 4 MPa or more, and preferably 120 MPa or less. The pressure between the rolls can be measured using Prescale (for high pressure) manufactured by Fujifilm Corporation.

[0214] The temperature of the smoothing treatment is not particularly limited, but is preferably 10 to 100°C, more preferably 10 to 50°C.

[0215] [Process Z]

[0216] The base silver pattern forming step may include a step Z of forming a non-silver halide layer containing gelatin and a specific polymer on the substrate before step A. By implementing step Z, a non-silver halide layer is formed between the substrate and the silver halide-containing photosensitive layer. The non-silver halide layer plays the role of a so-called anti-halation layer and helps to improve the adhesion between the conductive fine wire and the substrate.

[0217] The silver halide-free layer contains the gelatin and the specific polymer described above. On the other hand, the silver halide-free layer does not contain silver halide.

[0218] The ratio of the mass of the specific polymer to the mass of gelatin in the layer containing no silver halide (mass of specific polymer / mass of gelatin) is not particularly limited, but is preferably 0.1 to 5.0, and more preferably 1.0 to 3.0.

[0219] The content of the specific polymer in the silver halide-free layer is not particularly limited, but is usually 0.03 g / m 2 From the viewpoint of better adhesion of the conductive thin wire portion, 1.0 g / m 2 There is no particular upper limit, but it is usually 1.63 g / m 2 the following.

[0220] The method for forming the silver halide-free layer is not particularly limited, and an example thereof includes a method in which a layer-forming composition containing gelatin and a specific polymer is applied to a substrate and, if necessary, subjected to a heat treatment.

[0221] The layer-forming composition may contain a solvent as necessary. As the type of the solvent, the solvent used in the above-mentioned photosensitive layer-forming composition can be exemplified.

[0222] The thickness of the silver halide-free layer is not particularly limited, but is usually 0.05 μm or more, preferably more than 1.0 μm, and more preferably 1.5 μm or more from the viewpoint of better adhesion of the conductive fine line portion. The upper limit is not particularly limited, but is preferably less than 3.0 μm.

[0223] The line width of the base silver pattern formed by the above-described steps is preferably 0.5 μm or more and less than 5.0 μm, and is more preferably 3.0 μm or less, and further preferably 1.4 μm or less from the viewpoint of making the formed conductive thin wires difficult to visually recognize.

[0224] The line width of the base silver pattern was determined by observing the conductive substrate in a vertical direction from the film surface using a scanning electron microscope (SEM). The more detailed measurement method is the same as that in the examples described below.

[0225] Furthermore, from the viewpoint of reducing the variation in line width of the formed conductive thin lines, the thickness of the base silver pattern is preferably 1.7 μm or less, more preferably 1.5 μm or less, further preferably 1.0 μm or less, and particularly preferably 0.8 μm or less. The lower limit is not particularly limited, but is preferably 0.2 μm or more.

[0226] The thickness of the base silver pattern can be obtained by the following method.

[0227] Select any 10 locations of the substrate on which the base silver pattern is formed, and observe the cross section cut in a direction orthogonal to the extension direction of the base silver fine wire at each location using SEM. The maximum value in the thickness direction of the base silver fine wire is measured based on the observed image obtained. The thickness of the base silver pattern is obtained by calculating the arithmetic mean of the maximum values ​​in the thickness direction measured at the selected 10 locations. A more detailed measurement method is described in the examples described later.

[0228] In addition, in the conductive substrate obtained through the steps described later, when the region of the underlying silver pattern can be discerned, the above-mentioned measurement may be performed on the conductive substrate to measure the thickness of the underlying silver pattern.

[0229] <Resist film placement process>

[0230] The method for producing a conductive substrate of the present invention includes a step of disposing a resist film on the surface side of the substrate on which the base silver pattern is formed (resist film disposing step). More specifically, Figure 2 As shown, by performing this process, the base silver pattern 12 and the resist film 14 are arranged on the substrate 10. The resist film 14 is arranged so as to cover the base silver pattern 12.

[0231] The configuration of the resist film can be implemented by a known method, for example, a method of applying a resist composition containing components contained in the resist film to the surface side of the base silver pattern formed on the substrate and a method of bonding the surface formed with the base silver pattern and a film-like resist film.

[0232] The resist film configured in the resist film configuration step is preferably a negative resist in which the exposed portion is insoluble in the developer used in the resist film development step. The negative resist can use a known negative resist. Among them, a negative resist whose solubility in an alkaline developer is reduced by exposure is preferred.

[0233] <Resist film exposure process>

[0234] The method for producing a conductive substrate of the present invention includes a step of irradiating light from the surface side of the substrate on which the base silver pattern is not formed to expose the resist film (resist film exposure step).

[0235] In the resist film exposure step, light is irradiated to the entire surface of the substrate from the surface side of the substrate where the base silver pattern is not formed, and the resist film is exposed using the base silver pattern as a mask. More specifically, Figure 3 As shown, when light is irradiated from the direction indicated by the white arrow, the base silver pattern 12 acts as a mask and the resist film located on the base silver pattern is not exposed.

[0236] The wavelength of the exposure light used in the resist film exposure process is not particularly limited as long as the resist film can be exposed and can be transmitted through the above-mentioned substrate. As the exposure light and exposure light source used in the resist film exposure process, g-rays (wavelength 436nm), i-rays (365nm), KrF excimer lasers (248nm), ArF excimer lasers (193nm) and F2 excimer lasers (157nm) etc. can be cited. When using laser as the exposure light source, in the above-mentioned exposure, as long as the laser scanning is exposed in a manner that light is irradiated to the entire surface of the substrate.

[0237] The exposure dose in the resist film exposure step can be appropriately adjusted, but is preferably 50 to 2000 mJ / cm 2 , more preferably 100 to 1000 mJ / cm 2 , more preferably 200 to 500 mJ / cm 2 .

[0238] Furthermore, in the resist film exposure process, the resist film may be heated before exposure (pre-baking), or may be heated after exposure (post-baking). The heating may be appropriately adjusted according to the resist film used, but as the heating conditions, for example, heating at 60 to 150° C. for 10 to 300 seconds may be cited.

[0239] <Resist film development step>

[0240] The method for producing a conductive substrate of the present invention includes a step of developing the exposed resist film to form a resist pattern (resist film developing step).

[0241] In the resist film development step, the exposed resist film is developed to remove the portion of the resist film disposed on the base silver pattern, thereby forming a resist pattern having an opening portion having a shape corresponding to the base silver pattern. That is, the resist pattern has a shape that covers only the portion where the base silver pattern is not formed. As described above, the resist pattern is exposed by irradiating light from the surface side of the substrate where the base silver pattern is not formed using the base silver pattern as a mask, thereby forming a resist pattern that is self-aligned (self-aligned) with the base silver pattern. More specifically, by implementing this step, as Figure 4As shown, the base silver pattern 12 and the resist pattern 16 are arranged on the substrate 10. Figure 4 As shown, the resist pattern 16 has an opening corresponding to the position of the base silver pattern 12 .

[0242] In the resist film development step, the resist film can be developed using a known developer, and the developer may be selected according to the type of the resist film. Examples of the developer include alkaline developers and organic solvent developers.

[0243] Furthermore, in the resist film development process, rinsing with a rinse liquid may be performed after development. As the rinse liquid, the liquid used for the developer may be used as the rinse liquid, or other rinse liquids may be used. As the other rinse liquids, water (preferably ion-exchanged water or ultrapure water) may be cited.

[0244] The resist pattern formed in the resist film development step is preferably an inverted trapezoidal shape (inverted tapered shape) or a rectangular shape in which the base silver pattern side becomes a short side.

[0245] <Conductive thin wire formation process>

[0246] The method for producing a conductive substrate of the present invention includes a step of performing a plating treatment using a base silver pattern as a seed layer to form a metal pattern on the base silver pattern to obtain conductive fine wires (conductive fine wire forming step).

[0247] In the conductive fine wire forming process, the resist pattern obtained in the resist film developing process is used as a plating resist, and the base silver pattern is used as a seed layer for plating treatment, and a plating film is selectively formed on the base silver pattern to obtain a metal pattern. More specifically, Figure 5 As shown in FIG. 1 , by implementing this process, a metal pattern 18 is formed on the base silver pattern 12, thereby obtaining a conductive fine wire 20. Figure 5 As shown, the conductive thin wire 20 is composed of a base silver pattern 12 and a metal pattern 20 (plated film).

[0248] The plating method is not particularly limited, and may be electroless plating (chemical reduction plating, displacement plating, etc.) or electrolytic plating, but is preferably electroless plating. As electroless plating, a known electroless plating technique can be used.

[0249] Examples of the plating treatment include silver plating, copper plating, nickel plating, and cobalt plating. From the viewpoint of obtaining better conductivity of the conductive thin wire, silver plating or copper plating is preferred, and silver plating is more preferred.

[0250] The components contained in the plating solution used in the plating treatment are not particularly limited, but generally, in addition to a solvent (e.g., water), it mainly contains 1. metal ions for plating, 2. a reducing agent, 3. an additive (stabilizer) for improving the stability of the metal ions, and 4. a pH adjuster. In addition to these, the plating solution may also contain known additives such as a stabilizer for the plating solution.

[0251] The type of metal ions for plating contained in the plating solution can be appropriately selected according to the type of metal to be deposited, and examples thereof include silver ions, copper ions, nickel ions, and cobalt ions.

[0252] As the plating solution, a commercially available plating solution can be used.

[0253] The plating treatment process is not particularly limited as long as the base silver pattern is brought into contact with the plating solution. For example, there can be mentioned a method of immersing the base silver pattern in the plating solution and a method of applying the plating solution on the base silver pattern.

[0254] The contact time between the base silver pattern and the plating solution is not particularly limited, but is preferably 20 seconds to 30 minutes from the viewpoint of better conductivity of the conductive thin wires and from the viewpoint of productivity.

[0255] After the conductive thin wire forming step is performed, the resist pattern may be removed. As a method for removing the resist pattern, a method of removing the resist pattern using a stripping solution having a high affinity with the material constituting the resist pattern may be mentioned. The stripping solution may be a known stripping solution.

[0256] In addition, the resist pattern may not be removed, and the portion that is insoluble in the developer due to exposure may be used as a component of a product, etc. The resist pattern used without being removed in this way is also called a permanent resist. When the resist pattern is used as a permanent resist, the haze and retardation of the permanent resist preferably have a small change over time. As a resist film that can form such a permanent resist, for example, ATN1021 negative acrylic resist manufactured by Dow Chemical Company can be cited.

[0257] Furthermore, after the conductive thin wire forming step is performed, a blackening layer may be formed on the surface of the formed conductive thin wire on the side opposite to the substrate.

[0258] The black layer prevents reflection of light on the conductive thin wires and improves visibility of light passing through the conductive substrate. The black layer can be formed by plating such as black chrome plating, black nickel plating, or black alumina plating.

[0259] Furthermore, after the conductive thin wire forming step is performed, a step of performing a heat treatment may be further included. By performing this step, a conductive thin wire with better conductivity can be obtained. The method of performing the heat treatment on the conductive thin wire is not particularly limited, and the method described in step C may be cited.

[0260] From the viewpoint of easily forming a conductive fine wire with excellent conductivity, the thickness of the formed metal pattern (thickness of the plated film) is preferably 0.5 μm or more, more preferably 1.0 μm or more, and further preferably 1.5 μm or more. It is believed that when the thickness of the above-mentioned metal pattern is within the preferred range, it is not easily affected by the thickness deviation of the metal pattern, and it is easy to form a conductive fine wire with excellent conductivity. The upper limit is not particularly limited, preferably 10 μm or less, more preferably 8.0 μm or less, and further preferably 6.0 μm or less.

[0261] The thickness of the metal pattern can be measured on a conductive substrate by the same method as the method for measuring the thickness of the base silver pattern. A more detailed measurement method is described in the examples described below.

[0262] The thickness of the metal pattern can be adjusted by the line width of the base silver pattern, the thickness of the resist film, the plating treatment time in the conductive fine wire formation step, and the like.

[0263] In addition, regarding the conductive substrate, the line width of the conductive thin wire is preferably 0.5 μm or more and less than 5.0 μm, and is more preferably 3.0 μm or less, further preferably 1.4 μm or less, and particularly preferably 1.0 μm or less from the viewpoint of making the conductive thin wire difficult to visually recognize.

[0264] The line width of the conductive thin wire can be measured on the conductive substrate by the same method as the method for measuring the thickness of the base silver pattern. A more detailed measurement method is described in the examples described below.

[0265] The line width of the conductive thin wire can be adjusted by the line width of the base silver pattern.

[0266] Furthermore, in the conductive substrate, from the viewpoint of forming a conductive thin line with a thin line width and excellent conductivity, the ratio of the thickness of the metal pattern (thickness of the plated film) to the line width of the conductive thin line is also preferably 0.4 or more. The above ratio is more preferably 0.8 or more, and further preferably 1.0 or more. The upper limit of the above ratio is not particularly limited, but is preferably 5.0 or less, and more preferably 4.0 or less.

[0267] The height of the conductive thin wires can be measured on the conductive substrate by the same method as the method for measuring the thickness of the base silver pattern. A more detailed measurement method is described in the examples described below.

[0268] Furthermore, in the conductive substrate, from the viewpoint of forming a conductive thin wire with a thin line width and excellent conductivity, the ratio of the height of the conductive thin wire to the line width of the conductive thin wire is also preferably 0.80 or more. The above ratio is more preferably 1.10 or more, further preferably 1.20 or more, and particularly preferably 2.00 or more. The upper limit of the above ratio is not particularly limited, but is preferably 5.00 or less, and more preferably 4.00 or less.

[0269] The height of the conductive fine wire can be measured on a conductive substrate by the same method as the method for measuring the thickness of the base silver pattern. A more detailed measurement method is described in the embodiments described below. In addition, the height of the conductive fine wire is the sum of the thickness of the base silver pattern and the thickness of the metal pattern (plating film).

[0270] The above ratio can be adjusted by the line width of the base silver pattern, the thickness of the resist film, the plating treatment time in the conductive fine wire formation step, and the like.

[0271] Furthermore, in the conductive substrate, the intersection thickening ratio of the conductive thin wires is preferably 1.0 to 1.6, and more preferably 1.0 to 1.5.

[0272] In addition, in this specification, intersection thickening is defined as follows.

[0273] Figure 6 and Figure 7 It is a plan view showing an enlarged intersection portion of conductive thin wires for illustrating the thickened intersection.

[0274] Figure 6 Indicates the intersection of the conductive thin lines when there is no thickening of the intersection. Figure 6 In FIG. 1 , the conductive thin wire 22a has a line width Lw, and two conductive thin wires 22a intersect at an angle θ to form an intersection. Figure 6 In the embodiment, the conductive thin wire 22a extends from the intersection to four directions. θ is greater than 0° and less than 90°. Figure 6 In the case shown, with respect to the diameter Ci of the largest inscribed circle which has the largest diameter in the area forming the intersection portion, the angle θ formed and the line width Lw of the conductive fine wire are used, and when θ exceeds 0° and is less than 60°, Ci=2*Lw / (1+sinθ / 2) is assigned, and when θ is 60 to 90°, Ci=Lw / ((sinθ)*(cosθ / 2)) is assigned.

[0275] Figure 7 Indicates the intersection of conductive thin lines when the intersection is thickened. Figure 7 In the embodiment, the conductive thin wires 22b intersect at an angle θ between two conductive thin wires 22b to form an intersection. Figure 7In the embodiment, the conductive thin wire 22b extends from the intersection to four directions. Figure 7 The dashed line in FIG. 1 is a dotted line when there is no thickening of the intersections formed by the conductive fine wires 22b. The line width of the conductive fine wires 22b in the region where no thickening of the intersections occurs is Lw. Figure 7 In the above, the diameter Cw of the largest inscribed circle having the largest diameter in the region forming the intersection is determined.

[0276] Here, the intersection thickening rate is given by the following formula.

[0277] (Intersection thickening ratio) = Cw / Ci

[0278] That is, the intersection thickening rate is equivalent to the ratio of the diameter Cw of the maximum inscribed circle of the intersection where the intersection thickening occurs to the diameter Ci of the maximum inscribed circle of the intersection when it is considered that there is no intersection thickening. In addition, the diameter Ci of the maximum inscribed circle is calculated based on the line width Lw of the conductive fine wire measured by the above method and the angle θ formed at the intersection of the two conductive fine wires. For example, when the angle θ is 90°, that is, the conductive fine wires are orthogonal, the diameter Ci of the maximum inscribed circle becomes √2 times the line width Lw of the conductive fine wire.

[0279] The intersection thickening is obtained by observing the conductive substrate from a direction perpendicular to the plane of the conductive substrate using a SEM and analyzing the obtained image. A more detailed measurement method is described in the examples described below.

[0280] In addition, Figure 6 and Figure 7 In the embodiment, the conductive thin wires are described as extending from the intersection to four directions, but as mentioned above, other methods are also possible. Figure 6 and Figure 7 In the case of other than the above, the diameter Ci of the largest inscribed circle and the diameter Cw of the largest inscribed circle are also obtained by observing with SEM and analyzing the obtained image in the same manner as described above.

[0281] The above-mentioned intersection thickening rate is equivalent to the value obtained by quantifying how many times the effective line width of the intersection is increased by the thickening of the intersection compared with the case where the intersection is not thickened. When there is no thickening of the intersection, the intersection thickening rate is 1. When there is thickening of the intersection, the intersection thickening rate exceeds 1, and when the intersection is thin, the intersection thickening rate is less than 1.

[0282] The diameter Cw of the maximum inscribed circle is the average value of the maximum diameters of the circles inscribed in the five intersections, and Lw is the average value of the line widths of the midpoints between the five intersections.

[0283] <Applications of Conductive Substrates>

[0284] The conductive substrate obtained by the manufacturing method of the conductive substrate of the present invention can be applied to various uses, such as touch panels (or touch panel sensors), semiconductor chips, various electrical wiring boards, FPC (Flexible Printed Circuits), COF (Chip on Film), TAB (Tape Automated Bonding), antennas, multilayer wiring boards, and motherboards. Among them, the conductive substrate is preferably used for touch panels (electrostatic capacitive touch panels).

[0285] In a touch panel having a conductive substrate, the conductive fine wires can effectively function as detection electrodes. When the conductive substrate is used for the touch panel, the display panel used in combination with the conductive substrate includes, for example, a liquid crystal panel and an OLED (Organic Light Emitting Diode) panel, preferably a combination with an OLED panel.

[0286] As the use of the conductive substrate other than the above, for example, an electromagnetic wave shielding member that cuts off electromagnetic waves such as radio waves and microwaves (ultra-short waves) generated by electronic devices such as personal computers and workstations and prevents static electricity can be cited. In addition to the main body of a personal computer, this electromagnetic wave shielding member can also be used in electronic devices such as image capture equipment and electronic medical equipment.

[0287] The conductive substrate can also be used for a transparent heating element.

[0288] The conductive substrate can be used in the form of a laminate having the conductive substrate and other components such as an adhesive sheet and a release sheet during handling and transportation. The release sheet functions as a protective sheet for preventing scratches from being generated on the conductive substrate during transportation of the laminate.

[0289] Furthermore, the conductive substrate may be treated in the form of a composite having the conductive substrate, the adhesive sheet, and the protective layer in this order, for example.

[0290] The present invention is basically configured as described above. The present invention is not limited to the above-described embodiment, and various improvements or changes can be made without departing from the gist of the present invention.

[0291] Example

[0292] Hereinafter, the present invention will be described in further detail based on examples.

[0293] The materials, usage amounts, ratios, treatment contents and treatment procedures shown in the following examples can be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the present invention should not be interpreted in a limiting sense by the examples shown below.

[0294] In Examples 1 to 10 and Comparative Example 1, conductive substrates were produced, and the intersection thickening rate, line width, line width variation, conductivity, and visibility were evaluated as evaluation items. Examples 1 to 10 and Comparative Example 1 are described below.

[0295] <Example 1>

[0296] [Preparation of silver halide emulsion]

[0297] To the following liquid 1 maintained at a temperature of 38°C and a pH (hydrogen ion index) of 4.5, 90% of each of the following liquids 2 and 3 was added simultaneously while stirring for 20 minutes, thereby forming 0.07μm core particles. Next, the following liquids 4 and 5 were added to the mixed solution for 8 minutes, and the remaining 10% of the following liquids 2 and 3 was added for further 2 minutes, so that the particles grew to 0.09μm. Furthermore, 0.15g of potassium iodide was added to the mixed solution, and the mixture was aged for 5 minutes, thereby completing the particle formation.

[0298] 1 fluid:

[0299] Water 750mL

[0300] Gelatin 8.6g

[0301] Sodium chloride 3g

[0302] 1,3-Dimethylimidazolidine-2-thione 20mg

[0303] Sodium benzenethiosulfonate 10mg

[0304] Citric acid 0.7g

[0305] 2 fluids:

[0306] 300 mL water

[0307] Silver nitrate 150g

[0308] 3 fluids:

[0309] 300 mL water

[0310] Sodium chloride 38g

[0311] Potassium bromide 32g

[0312] Potassium hexachloroiridate(III)

[0313] (0.005% KCl 20% aqueous solution) 5 mL

[0314] Ammonium hexachlororhodium

[0315] (0.001% NaCl 20% aqueous solution) 7 mL

[0316] 4 fluids:

[0317] Water 100mL

[0318] Silver nitrate 50g

[0319] 5. Liquid:

[0320] Water 100mL

[0321] Sodium chloride 13g

[0322] Potassium bromide 11g

[0323] Potassium ferrocyanide 5mg

[0324] Then, the particles were washed with water by flocculation method according to the conventional method. Specifically, the temperature of the above-mentioned mixed solution was lowered to 35°C, and the pH of the mixed solution was lowered using sulfuric acid until the silver halide particles were precipitated (within the range of pH 3.6±0.2). Then, about 3 liters of supernatant were removed from the mixed solution (first water wash). Moreover, after adding 3 liters of distilled water to the mixed solution from which the supernatant was removed, sulfuric acid was added until the silver halide was precipitated. Again, 3 liters of supernatant were removed from the mixed solution (second water wash). The same operation as the second water wash was further repeated once (third water wash), and the water washing and desalination process was completed.

[0325] After the emulsion was washed and desalted, the pH was adjusted to 6.4 and the pAg was adjusted to 7.5. Then, 2.5 g of gelatin, 10 mg of sodium benzenethiosulfonate, 3 mg of sodium benzenethiosulfinate, 15 mg of sodium thiosulfate and 10 mg of chloroauric acid were added to the emulsion, and chemical sensitization was performed at 55° C. to obtain the best sensitivity. Then, 100 mg of 1,3,3a,7-tetraazaindene as a stabilizer and 100 mg of PROXEL (trade name, manufactured by ICI Co., Ltd.) as a preservative were further added to the emulsion.

[0326] The emulsion finally obtained was a silver iodide-chlorobromide cubic grain emulsion containing 0.08 mol % of silver iodide, the ratio of silver chlorobromide being 70 mol % of silver chloride and 30 mol % of silver bromide, with an average grain size of 0.10 μm and a coefficient of variation of 9%.

[0327] [Preparation of Photosensitive Layer-Forming Composition]

[0328] 1,3,3a,7-tetraazaindole (1.2×10 -4 mol / mol Ag), hydroquinone (1.2×10 -2 mol / mol Ag), citric acid (3.0×10 -4 mol / mol Ag), 2,4-dichloro-6-hydroxy-1,3,5-triazine sodium salt (0.90 g / mol Ag) and a trace amount of a hardener were added to obtain a composition. Then, the pH of the composition was adjusted to 5.6 using citric acid.

[0329] A polymer latex containing a polymer represented by the following (P-1) (hereinafter also referred to as "polymer 1"), a dispersant containing dialkylphenyl PEO (PEO is the abbreviation of polyethylene oxide) sulfate, and water (the ratio of the mass of the dispersant to the mass of the polymer 1 (mass of the dispersant / mass of the polymer 1, unit: g / g) is 0.02, and the solid content is 22% by mass) is added to the above composition so that the ratio of the mass of the polymer 1 in the composition to the total mass of gelatin (mass of the polymer 1 / mass of the gelatin, unit: g / g) is 0.25 / 1, thereby obtaining a composition containing the polymer latex. Here, in the composition containing the polymer latex, the ratio of the mass of gelatin to the mass of silver derived from the silver halide (mass of gelatin / mass of silver derived from the silver halide, unit: g / g) is 0.11.

[0330] Furthermore, EPOXY RESIN DY 022 (trade name: manufactured by Agase ChemteX Corporation) was added as a crosslinking agent. The amount of the crosslinking agent added was adjusted so that the amount of the crosslinking agent in the silver halide-containing photosensitive layer described later would be 0.09 g / m 2 .

[0331] In the above manner, a photosensitive layer-forming composition was prepared.

[0332] In addition, polymer 1 was synthesized with reference to Japanese Patent Nos. 3305459 and 3754745.

[0333] [Chemical formula 5]

[0334]

[0335] [Formation of Primer Layer]

[0336] The above polymer latex was applied to a polyethylene terephthalate film ("roll-shaped long film manufactured by Fujifilm Corporation") having a thickness of 40 μm to form a primer layer having a thickness of 0.05 μm. This treatment was performed by roll-to-roll, and the following treatments (steps) were also performed by roll-to-roll in the same manner. In addition, the roll width at this time was 1 m and the length was 1000 m.

[0337] (Process Z1, Process A1)

[0338] Next, a composition for forming a layer containing no silver halide and a mixture of the polymer latex and gelatin and a composition for forming a photosensitive layer are simultaneously applied in layers on the undercoat layer to form a layer containing no silver halide and a photosensitive layer containing silver halide on the undercoat layer.

[0339] The thickness of the silver halide-free layer was 2.0 μm, the mixing mass ratio of polymer 1 to gelatin (polymer 1 / gelatin) in the silver halide-free layer was 2 / 1, and the content of polymer 1 was 1.3 g / m 2 .

[0340] The thickness of the silver halide-containing photosensitive layer was 2.0 μm, the mixing mass ratio of polymer 1 to gelatin (polymer 1 / gelatin) in the silver halide-containing photosensitive layer was 0.25 / 1, and the content of polymer 1 was 0.15 g / m 2 .

[0341] (Process B1)

[0342] The photosensitive layer was exposed by irradiating the prepared photosensitive layer with parallel light using a high-pressure mercury lamp as a light source through a grid-shaped photomask. A pattern forming mask was used as a photomask. In addition, the photosensitive layer was exposed while the photomask was in contact with the photosensitive layer. The shape of the photomask and the exposure conditions were set so that a unit square grid with an opening portion with a length L of 400 μm on one side was formed in the conductive substrate formed after the step E1 described later, and the line width Lw of the conductive fine line was 2.1 μm.

[0343] The exposed photosensitive layer was treated with a developer described later and a fixing solution (trade name: CN16X for N3X-R: manufactured by FUJIFILM Corporation) to perform a development process. Then, it was rinsed with pure water at 25° C. and dried to obtain a sample A having silver-containing fine wires containing metallic silver formed in a grid pattern. In sample A, a grid pattern area of ​​10 cm×10 cm was formed (belonging to the base silver pattern).

[0344] The line width of the silver-containing fine wire was measured using a microscope "VHX-5000" manufactured by KEYENCE CORPORATION.

[0345] (Composition of developer)

[0346] The following compounds are contained in 1 liter (L) of the developer.

[0347]

[0348] The obtained sample A was immersed in warm water at 50° C. for 180 seconds, and then dehydrated with an air shower and naturally dried.

[0349] (Process C1)

[0350] The sample A treated in step B1 was placed in a superheated steam treatment tank at 110° C. and allowed to stand for 30 seconds to be treated with superheated steam. The steam flow rate at this time was 100 kg / h.

[0351] (Process D1)

[0352] Sample A treated in step C1 was immersed in an aqueous solution containing hypochlorous acid (25° C.) for 30 seconds. Sample A was taken out of the aqueous solution and washed by immersing it in warm water (liquid temperature: 50° C.) for 120 seconds. Then, it was dehydrated with an air shower and dried naturally.

[0353] As the hypochlorous acid-containing aqueous solution, a diluted solution prepared by diluting a bleaching agent (trade name "Heiter") manufactured by Kao Corporation by two times was used.

[0354] (Process E1)

[0355] Sample A obtained in step E1 was subjected to a calendering treatment at a pressure of 30 kN using a calendering device composed of a combination of a metal roll and a resin roll. The calendering treatment was performed at room temperature.

[0356] Through the above steps, a base silver pattern was formed. The line width and thickness of the formed base silver pattern are shown in the table in the following section. The evaluation method of the line width and thickness of the base silver pattern will be described in the following section.

[0357] (Process G1)

[0358] A liquid negative resist material “ZPN1150” (manufactured by Zeon Corporation) was applied onto substantially the entire surface of the conductive substrate obtained in step E1 on the side where the base silver pattern was formed, thereby forming a resist film (resist film disposing step).

[0359] Next, an ultraviolet exposure device was used to irradiate the resist film with g-rays having a wavelength of 436 nm from the surface of the substrate opposite to the base silver pattern side, thereby exposing the resist film using the base silver pattern as a self-aligned mask pattern (resist film exposure step). During the exposure treatment, the exposure was performed at 320 mJ / cm 2 The exposed photoresist was exposed to an ultraviolet irradiation of 1000 nm, and then PEB (post-exposure baking) was performed at 90° C. for 1 minute. After PEB, the exposed photoresist was developed for 1 minute using a developer (“NMD-3” manufactured by TOKYO OHKAKOGYO CO., LTD.), and the resist film of the unexposed part was removed and then washed with water to form a resist pattern (plating resist pattern) (resist development step), thereby obtaining a sample B having a substrate, a base silver pattern, and a plating resist pattern.

[0360] The shape of the opening of the plating resist pattern is substantially the same as the mesh pattern of the base silver pattern. Also, the opening width of the formed plating resist pattern is substantially the same as the line width of the conductive fine wire constituting the mesh pattern of the base silver pattern.

[0361] (Process H1)

[0362] The sample B obtained in step G1 was immersed in a plating solution A (30° C.) described later. Then, the sample B was taken out from the plating solution A and then immersed in warm water (liquid temperature: 50° C.) for 120 seconds for cleaning, thereby forming a plated film on the base silver pattern using the base silver pattern as a seed layer. In addition, in step H1, the time for immersing the sample B in the plating solution A was adjusted so that the thickness of the plated film became 2.0 μm.

[0363] The composition of the plating solution A (total amount 1200 mL) used is as follows: The amount of potassium carbonate (manufactured by FUJIFILM Wako Pure Chemical Corporation) added was adjusted so that the pH of the plating solution A became 9.5. The following components of the plating solution A were all manufactured by FUJIFILM Wako Pure Chemical Corporation.

[0364] (Composition of Plating Solution A)

[0365]

[0366] Through the above steps, a conductive substrate of Example 1 is manufactured, which has a substrate, conductive fine wires composed of a metal pattern composed of a base silver pattern and a plating film arranged on the substrate, and a plating resist pattern formed in an area on the substrate where no conductive fine wires are arranged.

[0367] In the manufactured conductive substrate, since the metal density of the base silver pattern and the plated film is different, each layer can be identified by a scanning electron microscope (SEM), and the thickness of each layer and the total thickness can be measured.

[0368] Specifically, an ultra-thin slicer was used to cut the conductive substrate along a plane perpendicular to the direction in which the conductive thin wires extended, so that the cut surface including the width direction and the stacking direction (thickness direction) of the conductive thin wires was exposed. Then, as a pretreatment, carbon was vapor-deposited to a thickness of 10 to 20 nm on the exposed cut surface to prepare a test piece for cross-sectional observation.

[0369] The cut surface of the obtained test piece was observed using a SEM manufactured by Hitachi High-Technologies Corporation to obtain an observation image. The observation conditions were set to an acceleration voltage of 5 kV and a reflected electron mode. In the observation image, the region containing multiple elements with large atomic numbers is displayed as white. In the observation image, the densely white region is used as the region of the plated film, and the region darker than the region of the white plated film is used as the region of the base silver pattern to measure the thickness. The method for measuring the thickness is as described above.

[0370] <Example 2 to Example 9>

[0371] In Examples 2 to 9, the conductive substrate was manufactured in the same manner as in Example 1, except that the exposure time in step B1 was adjusted to change the exposure amount so as to adjust the line width of the base silver pattern shown in the table of the later stage, or the plating time in step G1 was changed so as to adjust the plating film thickness shown in the table of the later stage.

[0372] <Examples 10 and 11>

[0373] In Examples 10 and 11, a conductive substrate was manufactured in the same manner as in Example 1, except that a spacer was provided between the photosensitive layer and the photomask for exposure in step B1. The thickness of the spacer in Example 10 was 4.6 μm, and the thickness of the spacer in Example 11 was 6.0 μm. By changing the above steps, the line width after step E1 in Examples 10 and 11 became 2.5 μm.

[0374] <Example 12>

[0375] In Example 12, a conductive substrate was produced in the same manner as in Example 1, except that electroless copper plating was performed using the following electroless copper plating solution during the plating treatment in step H1.

[0376] The electroless copper plating solution used was "OIC ACCERA" and "OIC COPPER" manufactured by OKUNO CHEMICAL INDUSTRIES CO., LTD. The electroless copper plating was performed by immersing the sample B in OIC ACCERA (25°C) for 3 minutes and then in OIC COPPER (55°C) for 10 minutes, followed by rinsing with 25°C pure water.

[0377] <Example 13>

[0378] In Example 13, the line width of the mask used in step B1 is changed and adjusted in a manner so as to obtain the line width and thickness of the base silver pattern shown in the table of the later stage, and the plating time in step G1 is changed and adjusted in a manner so as to obtain the plating film thickness shown in the table of the later stage. Except for this, a conductive substrate is manufactured in the same manner as Example 1.

[0379] <Example 14>

[0380] In Example 14, the exposure amount in step B1 is adjusted so as to obtain the line width and thickness of the base silver pattern shown in the table of the later stage, and the plating time in step G1 is changed so as to obtain the thickness of the plated film shown in the table of the later stage. Otherwise, a conductive substrate is manufactured in the same manner as in Example 13.

[0381] <Example 15>

[0382] In Example 15, a conductive substrate was produced in the same manner as in Example 1, except that the plating time in step G1 was changed and adjusted so as to have the plated film thickness shown in the table in the later stage.

[0383] <Comparative Examples 1 and 2>

[0384] The conductive substrates of Comparative Examples 1 and 2 were manufactured according to Example 1 of Japanese Patent Application Publication No. 2007-287953. That is, a metal layer was formed on a substrate by sputtering, a negative resist film was formed on the metal layer, a resist pattern was formed using the same pattern as in Example 1 of the present invention, a plated film was formed on the opening of the resist pattern by electrolytic plating, and after removing the resist pattern, the metal layer formed by sputtering without forming a plated film was removed to form conductive fine wires having a grid-like pattern, thereby manufacturing a conductive substrate. The substrate was set to a polyethylene terephthalate film with a thickness of 40 μm, the thickness of the plated film on the base metal pattern of Comparative Example 1 was set to 3 μm, and the thickness of the plated film of Comparative Example 2 was set to 6 μm.

[0385] <Evaluation>

[0386] Hereinafter, the intersection thickening rate, line width, line width variation, conductivity, and visibility as evaluation items will be described.

[0387] [Intersection thickening rate]

[0388] The intersection thickening rate is determined by obtaining an image through observation with a scanning electron microscope (SEM) and by the following definition: That is, the angle θ formed by two conductive thin wires is 90°. A smaller value of the intersection thickening rate indicates a smaller degree of thickening of the intersection portion.

[0389] (Intersection thickening rate) = Cw / (√2×Lw)

[0390] Cw is the same as the diameter Cw of the largest inscribed circle of the intersection described above, and is the diameter of the largest circle inscribed in the intersection of the conductive fine wire when the conductive substrate is observed from the vertical direction of the film surface. And Lw represents the average line width of the conductive fine wire. In addition, the unit of the diameter Cw of the largest inscribed circle and the line width Lw is set to μm.

[0391] Specifically, the diameter Cw of the maximum inscribed circle is the average value of the maximum diameters of the circles inscribed in the five intersections, and Lw is the average value of the line widths of the midpoints between the five intersections.

[0392] [Line width and line width deviation]

[0393] The line width W of the conductive fine wire is obtained by observing the film surface of the conductive substrate in the vertical direction using SEM. Specifically, the line widths of 5 points between the intersections of the conductive fine wires formed into a grid pattern are measured at equal intervals and the average value is taken as the line width We, and the above measurement is performed between the intersections of the conductive fine wires at 10 points, and the arithmetic average of the line widths We obtained at the 10 points is taken as the average line width W of the conductive fine wire.

[0394] Furthermore, when the maximum line width is Wmax, the minimum line width is Wmin, and the average line width is W, the line width deviation is calculated by the following equation.

[0395] (Line width deviation) = {(Wmax-Wmin) / W} × 100 (%)

[0396] In addition, the maximum line width Wmax is the value obtained by selecting the maximum line width among the five line width values ​​obtained when measuring the line width We at the above 10 locations and taking the arithmetic average of the 10 values ​​obtained, and the minimum line width Wmin is the value obtained by selecting the minimum line width among the five line width values ​​obtained when measuring the line width We at the above 10 locations and taking the arithmetic average of the 10 values ​​obtained.

[0397] From the viewpoint of excellent conductivity shown in the later section, the line width deviation is preferably small. The line width deviation is preferably 80% or less, more preferably 60% or less, and further preferably 50% or less. The lower limit of the line width deviation is not particularly limited, and may be 0% or more.

[0398] [Conductivity]

[0399] The surface resistivity of the conductive substrate manufactured in each embodiment and comparative example, on the surface on which the conductive fine wires are formed, is measured at any 10 locations using a resistivity meter (using Loresta: 4-probe probe (ASP) manufactured by Mitsubishi Chemical Analytech Co., Ltd.). The average value of the surface resistivity obtained at the 10 locations is taken as the surface resistivity of the conductive substrate. Based on the average resistivity of the conductive substrate, the conductivity of the conductive substrate is evaluated according to the following criteria. The evaluation of conductivity is preferably "B" or above in practical terms.

[0400] "A": Surface resistivity is less than 10Ω / □

[0401] "B": Surface resistivity is 10Ω / □ or more and less than 50Ω / □

[0402] "C": Surface resistivity is 50Ω / □ or more

[0403] [Visibility]

[0404] The obtained conductive substrate was stacked in the order of glass / conductive substrate / polarizer 1 / polarizer 2 / black PET (manufactured by PANAC Co., Ltd., industrial black PET (GPH100E82A04)) to obtain a laminate. In addition, polarizer 1 and polarizer 2 were linear polarizers, and were stacked in such a manner that the polarization directions were orthogonal. In addition, the conductive substrate was arranged so that the conductive fine wire side was located on the glass side.

[0405] Next, the obtained laminate was observed with the naked eye from the front side of the glass surface and at an angle of 30° to 60° in an environment of 500 lux. The above observation was performed by 10 observers, and the visibility was evaluated according to the following criteria. In addition, in the case where the conductive fine wires in the grid pattern are not easily visually recognizable, the optical properties of the conductive substrate are excellent, and the moiré generated when the conductive substrate is laminated on the display is reduced. Among the following 1 to 5, the visibility evaluation is preferably 3 to 5, more preferably 4 or 5, and further preferably 5.

[0406] 5: When observing the laminated body from a position 15 cm away, no observer visually recognized the grid pattern.

[0407] 4: When observing the laminated body from a distance of 30 cm, the number of observers who visually recognized the grid pattern was 0 or 1.

[0408] 3: When observing the laminated body from a distance of 30 cm, 2 to 4 observers visually recognized the grid pattern.

[0409] 2: When observing the laminated body from a distance of 30 cm, 5 or more observers visually recognized the grid pattern.

[0410] 1: When observing the laminated body from a distance of 50 cm, 5 or more observers visually recognized the grid pattern.

[0411] <Results>

[0412] The evaluation results of the above-mentioned examples and comparative examples are shown in the table.

[0413] In the table, "average line width" is the line width (μm) of the conductive thin wires, and is the average line width W of the conductive thin wires.

[0414] In the table, "aspect ratio" is the value obtained by dividing the height (μm) of the conductive fine wire by the line width (μm) of the conductive fine wire, which corresponds to the ratio of the height of the conductive fine wire to the line width of the conductive fine wire. The height of the conductive fine wire is the total value of the thickness of the base silver pattern and the thickness of the plated film, and the line width of the conductive fine wire is the average line width W of the above conductive fine wire.

[0415] [Table 1]

[0416]

[0417] The results in Table 1 show that the method for manufacturing a conductive substrate of the present invention can manufacture a conductive substrate having a conductive thin wire with a thin line width and excellent conductivity while suppressing thickening of intersections. On the other hand, in the conductive substrates of Comparative Examples 1 and 2 manufactured by a method other than the method for manufacturing a conductive substrate of the present invention, thickening of intersections could not be suppressed.

[0418] According to the comparison between Example 13 and other examples, it was confirmed that when the thickness of the base silver pattern was 1.0 μm or less, the line width variation of the formed conductive thin wires was further reduced.

[0419] Comparison between Examples 13 and 14 and Examples 1 to 10 and 12 confirmed that visibility was more excellent when the line width of the conductive thin wire was 3.0 μm or less.

[0420] Comparison between Example 15 and Example 1 confirmed that the conductivity was more excellent when the ratio of the height of the conductive thin wire to the line width of the conductive thin wire was 1.10 or more.

[0421] Comparison between Example 11 and other examples confirmed that when the intersection thickening ratio was 1.0 to 1.5, visibility was more excellent.

[0422] Explanation of symbols

[0423] 10-substrate, 12-base silver pattern, 14-resist film, 16-resist pattern, 18-metal pattern, 20-conductive fine wire, 22-base silver fine wire, 32-non-fine wire portion, 22a, 22b-conductive fine wire.

Claims

1. A method for manufacturing a conductive substrate, comprising: A step of forming a grid-like base silver pattern on one surface side of a substrate by a photo production method; a step of disposing a resist film on the surface side of the substrate on which the base silver pattern is formed; a step of irradiating light from a surface side of the substrate on which the base silver pattern is not formed to expose the resist film; A step of developing the exposed resist film to form a resist pattern; and The step of performing a plating treatment using the base silver pattern as a seed layer to form a metal pattern on the base silver pattern to obtain conductive fine wires.

2. The method for producing a conductive substrate according to claim 1, wherein: The intersection thickening ratio of the conductive thin wires is 1.0 to 1.

5.

3. The method for producing a conductive substrate according to claim 1 or 2, wherein: The conductive thin wire has a line width of 3.0 μm or less.

4. The method for producing a conductive substrate according to claim 1 or 2, wherein: The thickness of the base silver pattern is less than 1.0 μm.

5. The method for producing a conductive substrate according to claim 1 or 2, wherein: A ratio of the height of the conductive thin wire to the line width of the conductive thin wire is greater than or equal to 1.10.

Citation Information

Patent Citations

  • Image receiving material for silver complex salt diffusion transfer

    JP1993265162A

  • Circuit board and its production method

    JP2007287953A

  • Spontaneous emission display, transparent conductive film, method for manufacturing transparent conductive film, electroluminescence device, solar cell transparent electrode, and electronic paper transparent electrode

    JP2009004348A