Clay, ceramic sanitary ware and their preparation methods

By covering the upper and lower surfaces of the ceramic sanitary ware body with a specific ratio of mud layer and glossy glaze layer, the problem of local shrinkage and deformation during high-temperature firing of ceramic sanitary ware is solved, the product qualification rate and hardness are improved, and the scrap rate is reduced.

CN119143491BActive Publication Date: 2026-11-17FOSHAN HEGII SANITARY WARES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411284719.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2026-11-17
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

Ceramic sanitary ware is prone to localized shrinkage and deformation during high-temperature firing, resulting in a high product scrap rate.

Method used

Using a specific ratio of Al2O3, SiO2, Fe2O3, CaO, MgO, K2O and Na2O as the main components of the clay, by covering the upper and lower surfaces of the green body with first and second clay layers of a specific thickness, and covering the surface with a glossy glaze layer, firing is synergistically promoted, the hardness and strength of the clay are improved, the green body is fixed, and local shrinkage deformation during firing is reduced.

Benefits of technology

It significantly improves the problem of local shrinkage and deformation during the firing of ceramic products, reduces the scrap rate, increases the product qualification rate, and avoids defects such as thin glaze, glaze accumulation, and glaze sedimentation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119143491B_ABST
    Figure CN119143491B_ABST
Patent Text Reader

Abstract

This application provides a clay, ceramic sanitary ware, and a preparation method, belonging to the field of ceramic technology. This application uses Al2O3 and SiO2 as the main components of the clay, laying the foundation for improving the problem of localized shrinkage and deformation during firing of ceramic products. Simultaneously, specific amounts of Fe2O3, CaO, MgO, K2O, and NaO are added to promote firing, further improving the hardness and strength of the clay, mitigating localized shrinkage and deformation during firing of ceramic products, and significantly increasing the yield rate of ceramic products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of ceramic technology, and in particular to a glaze slurry, ceramic sanitary ware, and a method for preparing them. Background Technology

[0002] Ceramic sanitary ware refers to sanitary products made of ceramic materials, such as washbasins, bathtubs, toilets, and urinals. They have advantages such as wear resistance, corrosion resistance, and easy cleaning, and are widely used in building decoration.

[0003] Ceramic sanitary ware requires high-temperature firing, but the body shrinks during this process, leading to defects such as localized shrinkage deformation and a high scrap rate. Therefore, it is necessary to develop a technology to address the problem of localized shrinkage deformation during the firing of ceramic sanitary ware. Summary of the Invention

[0004] Based on the deficiencies of the existing technology, the purpose of this application is to provide a clay ceramic sanitary ware and a preparation method thereof, which aims to improve the technical problem of local shrinkage and deformation during the firing of ceramic sanitary ware and improve the product qualification rate.

[0005] To achieve the above objectives, in a first aspect, this application provides a mud comprising the following chemical components in parts by weight: 56-66 parts Al2O3, 38-41 parts SiO2, 0.45-1 part Fe2O3, 0.64-1 part CaO, 0.07-1 part MgO, 0.17-1 part K2O, and 0.58-1 part Na2O.

[0006] The Al2O3 content in the mud is 55 to 66 parts by weight, such as 55 parts by weight, 57 parts by weight, 58 parts by weight, 59 parts by weight, 60 parts by weight, 61 parts by weight, 62 parts by weight, 63 parts by weight, 64 parts by weight, 65 parts by weight, 66 parts by weight, or any two of the above values ​​forming a range.

[0007] The SiO2 content in the mud is 38 to 41 parts by weight, such as 38 parts by weight, 38.5 parts by weight, 39 parts by weight, 39.5 parts by weight, 40 parts by weight, 40.5 parts by weight, 41 parts by weight, or any two of the above values ​​forming a range.

[0008] The Fe2O3 content in the mud is 0.45 to 1 part by weight, such as 0.45 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or any two of the above values ​​forming a range.

[0009] The CaO content in the mud is 0.64 to 1 part by weight, such as 0.64 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or any two of the above values ​​forming a range.

[0010] The MgO content in the mud is 0.07 to 1 part by weight, such as 0.07 parts by weight, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or any two of the above values ​​forming a range.

[0011] The K2O content in the mud is 0.17 to 1 part by weight, such as 0.17 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or any two of the above values ​​forming a range.

[0012] The Na2O content in the mud is 0.58 parts by weight to 1 part by weight, such as 0.58 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or any two of the above values ​​forming a range.

[0013] The clay is mainly composed of Al2O3 and SiO2. Al2O3 can significantly improve the hardness and strength of the clay and reduce the local shrinkage deformation of ceramic products during firing. SiO2 can improve the adhesion of the clay to the green body and also improve the hardness and strength of the clay, which is beneficial to reducing the local shrinkage deformation of ceramic products during firing. At the same time, specific amounts of Fe2O3, CaO, MgO, K2O and Na2O are added to synergistically promote firing, further improve the hardness and strength of the clay, and improve the problem of local shrinkage deformation of ceramic products during firing.

[0014] Under the synergistic effect of the above-mentioned chemical components in specific amounts, the mud can effectively fix the green body, significantly improve the problem of local shrinkage and deformation during firing of ceramic products, and reduce the product scrap rate.

[0015] In some embodiments of this application, the mass fraction of Al2O3 in the mud is 55% or more, such as 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62% or more, or any two of these values ​​forming a range.

[0016] In some embodiments, the mud is prepared using industrial-grade raw materials such as Al2O3, SiO2, Fe2O3, CaO, MgO, K2O, and Na2O.

[0017] The raw material formula for mud is not limited to the above; the raw material formula for mud can be obtained based on the chemical composition of mud.

[0018] Secondly, this application provides a ceramic sanitary ware, including a blank body, the upper surface of the blank body being covered with a first mud layer, the lower surface of the blank body being covered with a second mud layer, the surface of the first mud layer facing away from the blank body being covered with a glossy glaze layer, wherein the materials of the first mud layer and the second mud layer are each independently mud.

[0019] The ceramic sanitary ware is made by covering the upper and lower surfaces of the blank with a mud layer of a specific composition, which can effectively improve the problem of local shrinkage and deformation during firing and increase the product qualification rate.

[0020] The chemical composition formulas of the first mud layer and the second mud layer can be the same or different.

[0021] Preferably, the thickness of the first mud layer and the second mud layer are each independently 0.1 to 0.7 mm. More preferably, the thickness of the first mud layer and the second mud layer are each independently 0.2 to 0.3 mm.

[0022] When the thickness of the first and second clay layers is independently 0.1–0.7 mm, especially 0.2–0.3 mm, the clay provides better fixation for the ceramic body, resulting in lower local shrinkage and deformation during firing. Furthermore, it better prevents problems such as thin glaze, glaze accumulation, glaze settling, and glaze rolling caused by incomplete melting of the clay during firing, leading to a higher product qualification rate. "Glaze settling" refers to the accumulation and deposition of glaze in uneven areas (such as pits or low-lying areas) on the surface of the ceramic body, resulting in defects such as thick glaze and glaze rolling after firing.

[0023] The thickness of the first mud layer can be selected as 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, or any two of the above values.

[0024] The thickness of the second mud layer can be selected as 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, or any two of the above values.

[0025] The thicknesses of the first mud layer and the second mud layer can be the same or different.

[0026] The composition of the green body is not limited; either conventional or modified green bodies can be selected. In some embodiments of this application, the green body contains a skeleton component and a flux component, wherein the skeleton component includes SiO2 and Al2O3, and the flux component includes K2O and Na2O. The skeleton component is generally derived from lean raw materials; for example, SiO2 can be derived from quartz, feldspar, kaolin, etc., and Al2O3 can be derived from feldspar, kaolin, etc. These raw materials accumulate during the slurry absorption process, forming hydrophobic channels. The flux component acts as a flux, promoting sintering; K2O can be derived from potassium feldspar, potassium-sodium mixed sand, etc., and Na2O can be derived from sodium feldspar, potassium-sodium mixed sand, etc. The green body may also contain components derived from plastic raw materials. Plastic raw materials act as binders, binding lean raw materials, filling voids, and giving the slurry plastic molding properties, such as clay (e.g., black mud, white mud), kaolin, etc. As an example, the billet can be selected from H588-080, H588-090 or H588-100 billets sold by our company.

[0027] Preferably, the thickness of the glossy glaze layer is 0.8 to 1.1 mm. For example, the thickness of the glossy glaze layer is within the range of any two of the following values: 0.8 mm, 0.9 mm, 1 mm, 1.1 mm.

[0028] Preferably, the ceramic sanitary ware includes at least one of a cabinet basin, a washbasin, a toilet, and a squat toilet.

[0029] Thirdly, this application provides a method for preparing the ceramic sanitary ware, comprising the following steps:

[0030] Provide a green body slurry, and use the green body slurry to prepare a green body;

[0031] A slurry is provided and applied to the upper and lower surfaces of the billet, followed by a first drying process to obtain a first semi-finished product.

[0032] A glossy glaze paste is provided, and the glossy glaze paste is applied to the upper surface of the first semi-finished product to obtain a second semi-finished product;

[0033] The second semi-finished product is dried and fired a second time to obtain ceramic sanitary ware.

[0034] Preferably, the slurry has a drying time of 32.5–35.5 min, a specific gravity of 1.725–1.745 g / mL, and a flow rate of 145–160 s. The drying time can be measured by injecting 5 mL of slurry into a plastic ring with an inner diameter of 4 cm, placing it under normal temperature and humidity conditions (e.g., 25°C, 55% relative humidity), and observing and obtaining the slurry drying time.

[0035] Preferably, the slurry is applied to the upper and lower surfaces of the blank by spray gun spraying, wherein the spray gun spraying meets the following conditions: ambient temperature 26-35℃, ambient humidity 68%-75%, spray gun air pressure 0.5-0.6MPa, and slurry pressure 0.5-0.65MPa.

[0036] Applying the glossy glaze slurry to the upper surface of the first semi-finished product and then performing a first drying treatment facilitates the adhesion of the glossy glaze layer. Preferably, the first drying is performed until the product moisture content is 2% to 3%.

[0037] After the first drying, it can be polished to remove the particles attached to the surface, improve problems such as pinholes, pits, and unevenness, and facilitate the adhesion of the glossy glaze.

[0038] After polishing, a dust removal process can be performed to remove dust adhering to the surface, which is beneficial for the adhesion of the glossy glaze. For example, dust removal methods include at least one of blowing dust or wiping with a damp sponge.

[0039] Preferably, the drying time of the glossy glaze slurry is 32.5 to 35.5 min, the specific gravity is 1.725 to 1.745 g / mL, and the flow rate is 145 to 160 s.

[0040] Preferably, the glossy glaze slurry is applied to the upper surface of the first semi-finished product by spray gun spraying, wherein the spray gun spraying meets the following conditions: ambient temperature 26-35℃, ambient humidity 68%-75%, spray gun air pressure 0.5-0.6MPa, and slurry pressure 0.5-0.65MPa.

[0041] The second drying process is performed to ensure that the ceramic sanitary ware has a good glaze gloss, a smooth surface, and is free of defects such as pinholes and cracks. Preferably, the second drying is carried out until the product moisture content is ≤1%. The target product moisture content for the second drying can be selected as 1%, 0.9%, 0.8%, 0.7%, 0.5%, 0.4%, 0.3%, 0.2%, or 0.1%, etc.

[0042] Preferably, the firing temperature is in the range of 1175 to 1179°C, and the firing time is 15 to 18 hours.

[0043] Compared with the prior art, the beneficial effects of this application are as follows:

[0044] (1) This application uses Al2O3 and SiO2 as the main components of clay, which lays the foundation for fixing the green body and improving the problem of local shrinkage and deformation during firing of ceramic products. At the same time, specific amounts of Fe2O3, CaO, MgO, K2O and Na2O are added to synergistically promote firing, further improve the hardness and strength of clay, and improve the problem of local shrinkage and deformation during firing of ceramic products.

[0045] (2) Under the synergistic effect of the above-mentioned chemical components in the specific amount of clay used in this application, the green body can be well fixed, the problem of local shrinkage and deformation during firing of ceramic products can be significantly improved, and the scrap rate of products can be reduced. Attached Figure Description

[0046] Figure 1 Photograph of the ceramic cabinet basin during the production process of Example 1;

[0047] Figure 2 This is a photo of the ceramic cabinet basin after the mud was sprayed during the production process of Example 1 (before it was dried by the fan);

[0048] Figure 3 This is a photograph of the ceramic cabinet basin after it has been sprayed with mud during the production process of Example 1 (after being dried by a fan and polished).

[0049] Figure 4 This is a photograph of the ceramic cabinet basin after glossy glaze has been sprayed on during the production process of Example 1 (before sintering);

[0050] Figure 5 Here is a photo of the ceramic cabinet basin product from Example 1;

[0051] Figure 6 Comparative Example 1: Photo of a ceramic cabinet basin product;

[0052] Figure 7 Photograph of the ceramic strip product in Example A;

[0053] Figure 8 Photo of ceramic strip product A for comparison. Detailed Implementation

[0054] To better illustrate the purpose, technical solutions, and advantages of this application, the following description, in conjunction with specific embodiments and comparative examples, aims to provide a detailed understanding of the content of this application, rather than limiting it. All other embodiments obtained by those skilled in the art without inventive effort are within the protection scope of this application. Unless otherwise specified, the experimental reagents and instruments involved in the implementation of this application are commonly used reagents and instruments. In this application, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0055] Example 1

[0056] This embodiment provides a ceramic cabinet basin, the photograph of which can be found here. Figure 1 It includes a blank body, the upper surface of which is covered with a first clay layer, the lower surface of which is covered with a second clay layer, and the surface of the first clay layer facing away from the blank body is covered with a glossy glaze layer, wherein...

[0057] The blank body is the same as that of our company's H588-080 thin-edged cabinet basin.

[0058] The thickness of both the first and second mud layers is 0.3 mm, and their chemical compositions are as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 0.8 parts;

[0059] The thickness of the glossy glaze is 1 mm.

[0060] The method for preparing the ceramic cabinet basin in this embodiment includes the following steps:

[0061] Provide a green body slurry, and use the green body slurry to prepare a green body;

[0062] According to the chemical composition formula of the first and second mud layers, the mud raw materials were weighed, and water and 0.05% of carboxymethyl cellulose by weight of the mud raw materials were added to prepare mud slurry. The mud slurry was sprayed onto the upper and lower surfaces of the obtained blank using a spray gun, and dried with a fan until the product moisture content was 2%. After polishing, the first semi-finished product was obtained. The mud slurry drying time was 33.5 min, the specific gravity was 1.73 g / mL, and the flow rate was 152 s. The spray gun spraying met the following requirements: ambient temperature 30℃, ambient humidity 70%, spray gun air pressure 0.55 MPa, and slurry pressure 0.575 MPa.

[0063] A glossy glaze is provided, and a spray gun is used to spray and cover the upper surface of the first semi-finished product to obtain a second semi-finished product.

[0064] The resulting second semi-finished product was dried at 80°C until the product moisture content was 1%, and then fired at 1177°C for 16 hours to obtain a ceramic cabinet basin.

[0065] Example 2

[0066] This embodiment provides a ceramic cabinet basin, which differs from Embodiment 1 as follows:

[0067] The chemical composition formulas of the first mud layer and the second mud layer are different. In this embodiment, the chemical composition of the first mud layer and the second mud layer are as follows: by weight, Al2O3 57 parts, SiO2 41 parts, Fe2O3 0.45 parts, CaO 0.64 parts, MgO 0.07 parts, K2O 0.17 parts, NaO 0.58 parts.

[0068] Example 3

[0069] This embodiment provides a ceramic cabinet basin, which differs from Embodiment 1 as follows:

[0070] The chemical composition formulas of the first mud layer and the second mud layer are different. In this embodiment, the chemical composition of the first mud layer and the second mud layer are as follows: by weight, Al2O3 65 parts, SiO2 38 parts, Fe2O3 1 part, CaO 1 part, MgO 1 part, K2O 1 part, NaO 1 part.

[0071] Example 4

[0072] This embodiment provides a ceramic cabinet basin, which differs from Embodiment 1 as follows:

[0073] The thicknesses of the first mud layer and the second mud layer are different. In this embodiment, the thicknesses of the first mud layer and the second mud layer are 0.2 mm.

[0074] Example 5

[0075] This embodiment provides a ceramic cabinet basin, which differs from Embodiment 1 as follows:

[0076] The thicknesses of the first mud layer and the second mud layer are different. In this embodiment, the thicknesses of the first mud layer and the second mud layer are 0.1 mm.

[0077] Example 6

[0078] This embodiment provides a ceramic cabinet basin, which differs from Embodiment 1 as follows:

[0079] The thicknesses of the first mud layer and the second mud layer are different. In this embodiment, the thicknesses of the first mud layer and the second mud layer are 0.7 mm.

[0080] Comparative Example 1

[0081] This comparative example provides a ceramic cabinet basin, the photograph of which can be found here. Figure 2 The ceramic basin differs from Example 1 as follows: it does not contain the first and second mud layers.

[0082] Comparative Example 2

[0083] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0084] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 32 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, and NaO 0.8 parts.

[0085] Comparative Example 3

[0086] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0087] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 45 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 0.8 parts.

[0088] Comparative Example 4

[0089] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0090] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.3 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 0.8 parts.

[0091] Comparative Example 5

[0092] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0093] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 1.2 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 0.8 parts.

[0094] Comparative Example 6

[0095] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0096] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.5 parts, MgO 0.3 parts, K2O 0.4 parts, and NaO 0.8 parts.

[0097] Comparative Example 7

[0098] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0099] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 1.2 parts, MgO 0.3 parts, K2O 0.4 parts, and NaO 0.8 parts.

[0100] Comparative Example 8

[0101] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0102] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.05 parts, K2O 0.4 parts, NaO 0.8 parts.

[0103] Comparative Example 9

[0104] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0105] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 1.2 parts, K2O 0.4 parts, NaO 0.8 parts.

[0106] Comparative Example 10

[0107] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0108] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.1 parts, NaO 0.8 parts.

[0109] Comparative Example 11

[0110] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0111] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 1.2 parts, NaO 0.8 parts.

[0112] Comparative Example 12

[0113] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0114] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 0.4 parts.

[0115] Comparative Example 13

[0116] This comparative example provides a ceramic cabinet basin, which differs from Example 1 as follows:

[0117] The chemical composition formulas of the first and second mud layers are different. In this comparative example, the chemical composition of the first and second mud layers is as follows: by weight, Al2O3 58 parts, SiO2 39.1 parts, Fe2O3 0.6 parts, CaO 0.8 parts, MgO 0.3 parts, K2O 0.4 parts, NaO 1.2 parts.

[0118] Example A

[0119] This embodiment provides a ceramic strip, the photograph of which is shown below. Figure 3 As shown, it includes a blank body, the upper surface of which is covered with a first mud layer, and the lower surface of which is covered with a second mud layer, wherein...

[0120] The chemical composition formula of the green body is the same as that of the green body in Example 1;

[0121] The thickness of both the first and second mud layers is 0.3 mm, and their chemical composition formulas are the same as those of the first and second mud layers in Example 1.

[0122] The method for preparing the ceramic strip in this embodiment includes the following steps:

[0123] A green body with a length of 1.2 cm × width of 0.8 cm × height of 0.4 cm was prepared using the green body slurry of Example 1;

[0124] The slurry material from Example 1 was sprayed onto the upper and lower surfaces of the obtained blank using a spray gun, and then dried at 80°C until the moisture content of the product was 1% to obtain the first semi-finished product. The spray gun spraying process parameters were the same as those for spraying the slurry material in Example 1.

[0125] The resulting first semi-finished product was fired at 1177℃ for 16 hours to obtain ceramic strips.

[0126] Comparative Example A

[0127] This comparative example provides a ceramic strip, the photograph of which is shown below. Figure 4 As shown, its difference from Example A is as follows: it does not contain the first mud layer and the second mud layer.

[0128] Test case

[0129] The ceramic cabinet basins or ceramic strips obtained in the above embodiments and comparative examples were tested as follows:

[0130] Sink test: 80 parallel samples per group, according to Figure 1 and 2 As shown, place the measuring tape firmly against the front end of the sink and observe whether there is a gap between the sink and the measuring tape. If a gap exists, measure the maximum width W of the gap and record the maximum value of W among these 80 parallel samples (i.e., W). max If the maximum width of the gap is less than 2mm and there are no problems such as thin glaze, glaze accumulation, glaze sinking, or glaze rolling, it is considered qualified; otherwise, it is unqualified.

[0131] Ceramic strip test: according to Figure 3 and 4 As shown, use a ruler to measure the width and length of each ceramic strip.

[0132] The test results are shown in Table 1.

[0133] Table 1

[0134] <![CDATA[W max / mm]]> Pass rate / % Example 1 1.2 95 Example 2 1.6 87.5 Example 3 1.5 88.75 Example 4 1.4 92.5 Example 5 1.8 70 Example 6 1.6 72.5 Comparative Example 1 3.1 12.5 Comparative Example 2 2.4 51.25 Comparative Example 3 2.2 48.75 Comparative Example 4 2.7 46.25 Comparative Example 5 2.6 51.25 Comparative Example 6 2.6 57.5 Comparative Example 7 2.1 47.5 Comparative Example 8 2.8 56.25 Comparative Example 9 2.4 53.75 Comparative Example 10 2.5 48.75 Comparative Example 11 2.3 55 Comparative Example 12 2.6 57.5 Comparative Example 13 2.1 46.25

[0135] Table 2

[0136] Ceramic strip width / mm Ceramic strip length / mm Example A 5.9 21 Comparative Example A 5.7 19

[0137] As can be seen from the above data, the ceramic cabinet basins of Examples 1-6 and the ceramic strip of Example A, through the application of clay with a specific chemical composition formula to the upper and lower surfaces of the blank, significantly improve the problem of firing shrinkage and deformation. For example, the ceramic cabinet basins of Examples 1-6 have small gap widths. max For thicknesses below 2mm, the product qualification rate is above 70%; in Example A, the ceramic strip width is above 5.9mm and the length is above 21mm.

[0138] As can be seen from the comparison of Examples 1, 4 to 6, when the thickness of the clay layer (i.e. the first clay layer and the second clay layer) is 0.2-0.3mm, not only is the problem of local shrinkage and deformation during firing significantly improved, but problems such as thin glaze, glaze accumulation, glaze sinking, and glaze rolling are also less likely to occur, resulting in a higher product qualification rate.

[0139] Comparative Example 1 did not apply clay to the green body, resulting in severe local shrinkage and deformation during firing, and a low product qualification rate.

[0140] In Comparative Example 2, the alumina content in the clay was too high, which made the material difficult to sinter, resulting in serious local shrinkage and deformation during firing and a low product qualification rate. In Comparative Example 3, the alumina content was too low, which resulted in weak hardness and strength of the clay layer, serious local shrinkage and deformation during firing, and a low product qualification rate.

[0141] Comparative Examples 4, 6, 8, 10, and 12 had low levels of some fluxing agents, resulting in poor sintering, severe local shrinkage and deformation during firing, and low product qualification rates. Comparative Examples 5, 7, 9, 11, and 13 had high levels of some fluxing agents, making the clay prone to defects such as pores after firing, resulting in weak hardness and strength of the clay layer, severe local shrinkage and deformation during firing, and low product qualification rates.

[0142] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.

Claims

1. A ceramic sanitary ware, characterised in that, The invention includes a blank body, the upper surface of which is covered with a first clay layer, the lower surface of which is covered with a second clay layer, and the first clay layer is covered with a glossy glaze layer on the surface opposite to the blank body, wherein the materials of the first clay layer and the second clay layer are each independently selected from the following clays; The mud contains the following chemical components in parts by weight: 56-66 parts Al2O3, 38-41 parts SiO2, 0.45-1 part Fe2O3, 0.64-1 part CaO, 0.07-1 part MgO, 0.17-1 part K2O, and 0.58-1 part Na2O.

2. The ceramic sanitary ware as described in claim 1, characterized in that, The thickness of the first mud layer and the second mud layer are each 0.1~0.7 mm.

3. The ceramic sanitary ware as described in claim 2, characterized in that, The thickness of the first mud layer and the second mud layer are each 0.2~0.3 mm.

4. The ceramic sanitary ware as described in claim 1, characterized in that, The thickness of the glossy glaze layer is 0.8~1.1 mm.

5. The ceramic sanitary ware as described in claim 1, characterized in that, The ceramic sanitary ware includes at least one of the following: cabinet basin, countertop basin, toilet, and squat toilet.

6. The method for preparing ceramic sanitary ware according to any one of claims 1 to 5, characterized in that, Includes the following steps: A slurry and a blank are provided. The slurry is applied to the upper and lower surfaces of the blank, and then a first drying is performed to obtain a first semi-finished product. A glossy glaze paste is provided, and the glossy glaze paste is applied to the upper surface of the first semi-finished product to obtain a second semi-finished product; The second semi-finished product is dried and fired a second time to obtain ceramic sanitary ware.

7. The method for preparing ceramic sanitary ware as described in claim 6, characterized in that, The slurry has a drying time of 32.5~35.5 min, a specific gravity of 1.725~1.745 g / mL, and a flow rate of 145~160 s.

8. The method for preparing ceramic sanitary ware as described in claim 6, characterized in that, The slurry is applied to the upper and lower surfaces of the blank by spray gun spraying, which meets the following requirements: ambient temperature 26~35℃, ambient humidity 68%~75%, spray gun air pressure 0.5~0.6 MPa, and slurry pressure 0.5~0.65 MPa; the first drying is carried out until the product moisture content is 2%~3%.

9. The method for preparing ceramic sanitary ware as described in claim 6, characterized in that, At least one of the following conditions must be met: (1) The second drying process is carried out until the product moisture content is ≤1%; (2) The firing temperature is in the range of 1175 to 1179°C, and the firing time is 15 to 18 hours.

Citation Information

Patent Citations

  • Processing method of sanitary appliance

    CN117285328A

  • Ceramic material

    WO2014139993A1