Lithium manganese iron phosphate composite material and preparation method thereof, positive pole piece and battery
By coating lithium phosphate lithium manganese iron phosphate particles, the problem of poor cycle life of lithium manganese iron phosphate materials at high temperatures is solved, and more stable battery performance and higher energy density are achieved.
Patent Information
- Application Number
- CN202411205147.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-17
AI Technical Summary
磷酸锰铁锂材料在高温下循环寿命差,导致电芯容量衰减快,限制其在二次电池领域的应用。
By adding lithium manganese iron phosphate powder to the mixed solution, forming a gel state during stirring, followed by drying and sintering, a composite material coated with lithium manganese iron phosphate is formed, slowing down the between the material and the electrolyte Side reactions to improve cycle life.
It significantly improves the cycle life of lithium manganese iron phosphate material at high temperatures, slows down the capacity attenuation speed, and improves the energy density and circulation performance of the battery.
Smart Images

Figure CN119153647A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery manufacturing technology, and specifically to a lithium manganese iron phosphate composite material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0002] Secondary batteries usually include positive electrode sheets containing positive electrode materials, and the performance of positive electrode materials has a significant impact on the performance of secondary batteries. Existing positive electrode materials mainly include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium iron phosphate, lithium iron manganese phosphate and ternary materials. As a positive electrode material, lithium iron phosphate has the advantages of high safety, good cycle performance, and good thermal stability. It is widely used in secondary batteries, but its relatively low voltage platform (3.4V) makes its energy density low, which limits its development and application; while lithium iron manganese phosphate has a similar structure to lithium iron phosphate, but its discharge platform (4.1V) is higher and has a higher energy density. It has good prospects for application in secondary batteries and other fields. However, lithium iron manganese phosphate materials have poor cycle life at high temperatures, resulting in rapid cell capacity decay, which is difficult to promote at the application end. Summary of the invention
[0003] Based on this, it is necessary to provide a lithium iron manganese phosphate composite material and a preparation method thereof, a positive electrode sheet and a battery that can improve the cycle life of the lithium iron manganese phosphate material and slow down the capacity decay rate of the battery cell to address the above problems.
[0004] A method for preparing a lithium manganese iron phosphate composite material comprises the following steps:
[0005] Provide lithium iron manganese phosphate powder;
[0006] Dissolving a first phosphorus source, a first lithium source, and a first carbon source in a solvent to form a mixed solution;
[0007] Adding the lithium iron manganese phosphate powder to the mixed solution, and stirring the mixed solution into a gel state;
[0008] Drying the mixed solution in a gel state to obtain a solid mixture; and
[0009] The solid mixture is sintered to obtain a lithium manganese iron phosphate composite material in which lithium phosphate is coated with lithium manganese iron phosphate.
[0010] In some embodiments, the step of providing lithium iron manganese phosphate powder specifically includes:
[0011] preparing a first solution with a manganese source and an iron source as solutes, and preparing a second solution with a second carbon source as solute;
[0012] Mixing the first solution and the second solution to obtain a precipitate;
[0013] The precipitate is filtered, washed and dried to obtain ferromanganese carbonate material;
[0014] The ferromanganese carbonate material is mixed with a second lithium source, a second phosphorus source, and a third carbon source, ball-milled, and dried to obtain a mixed powder;
[0015] The mixed powder is sintered to obtain the lithium iron manganese phosphate powder.
[0016] In some embodiments, the first phosphorus source includes at least one of monoammonium hydrogen phosphate, diammonium hydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and phosphoric acid; and / or,
[0017] The first lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium phosphate, and lithium dihydrogen phosphate; and / or,
[0018] The first carbon source includes at least one of graphite, carbon nanotubes, acetylene black, graphene, superconducting carbon black, glucose, starch, oxalic acid, asphalt, ethylene glycol, polyethylene glycol, sucrose, and citric acid.
[0019] In some embodiments, the step of adding the lithium iron manganese phosphate powder to the mixed solution and stirring the mixed solution into a gel state specifically includes:
[0020] The mixed solution is stirred, and during the stirring process, the lithium iron manganese phosphate powder is continuously added to the mixed solution until the mixed solution is stirred into a gel state.
[0021] In some embodiments, in the step of stirring the mixed solution:
[0022] The temperature of the mixed solution is controlled to be 80° C.-90° C., and the stirring speed is controlled to be 800 rpm-1000 rpm.
[0023] In some embodiments, in the step of drying the mixed solution in a gel state to obtain a solid mixture: the drying temperature is 100° C.-120° C., and the drying time is 6 h-8 h; and / or,
[0024] In the step of sintering the solid mixture: the sintering temperature is 420° C.-480° C., and the sintering time is 6 h-8 h.
[0025] In some embodiments, the mass percentage of lithium phosphate in the lithium manganese iron phosphate composite material is 0.5%-2%.
[0026] A lithium iron manganese phosphate composite material prepared by the preparation method described in any of the above embodiments comprises lithium iron manganese phosphate particles and a coating layer coated on the surface of the lithium iron manganese phosphate particles, wherein the coating layer comprises lithium phosphate.
[0027] A positive electrode plate comprises a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises the lithium manganese iron phosphate composite material as described in any of the above embodiments.
[0028] A battery comprises the positive electrode sheet as described in any of the above embodiments.
[0029] The above-mentioned lithium iron manganese phosphate composite material and its preparation method, positive electrode plate and battery are prepared by adding lithium iron manganese phosphate powder to a mixed solution and stirring the mixed solution into a gel state, so that the first phosphorus source, the first lithium source and the first carbon source in the mixed solution undergo chemical reactions such as hydrolysis, condensation and polymerization to form a stable sol system, and the lithium iron manganese phosphate particles are relatively evenly distributed in the sol system. The mixed solution in a gel state is dried and sintered to form a lithium iron manganese phosphate composite material in which lithium iron manganese phosphate particles are coated with lithium phosphate. In the lithium iron manganese phosphate composite material, since lithium phosphate is coated on the surface of the lithium iron manganese phosphate particles, the side reaction between the lithium iron manganese phosphate and the electrolyte is greatly slowed down when the lithium iron manganese phosphate composite material is used as a positive electrode material, thereby slowing down the capacity decay of the lithium iron manganese phosphate material during the cycle, thereby improving the cycle life of the positive electrode material at high temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a flow chart of the steps of a method for preparing a lithium iron manganese phosphate composite material in one embodiment of the present application;
[0031] Figure 2 for Figure 1 The step flow chart of step S10 of the preparation method shown;
[0032] Figure 3 It is a curve diagram showing the change of capacity retention rate with the number of cycles in Control Example 1 and Examples 1 to 3;
[0033] Figure 4 It is a bar graph of the resistivity of the lithium iron manganese phosphate material in Control Example 1 and the lithium iron manganese phosphate composite materials in Examples 1 to 3. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0035] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0036] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0037] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0038] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0039] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0040] See also Figure 1 The present application provides a method for preparing a lithium manganese iron phosphate composite material, comprising the following steps:
[0041] S10. Provide lithium iron manganese phosphate powder.
[0042] S20, dissolving the first phosphorus source, the first lithium source and the first carbon source in a solvent to form a mixed solution.
[0043] S30, adding lithium iron manganese phosphate powder to the mixed solution, and stirring the mixed solution into a gel state. Specifically, the mixed solution is stirred, and lithium iron manganese phosphate powder is continuously added to the mixed solution during the stirring process until the mixed solution is stirred into a gel state. Optionally, when the mixed solution is stirred, the temperature of the mixed solution is controlled to be 80°C-90°C, and the stirring speed is 800rpm-1000rpm, so that the lithium iron manganese phosphate particles in the formed sol system are more evenly distributed, ensuring that the lithium iron manganese phosphate particles in the formed lithium iron manganese phosphate composite material are better coated with lithium phosphate.
[0044] S40, drying the mixed solution in a gel state to obtain a solid mixture. Optionally, the drying temperature is controlled at 100° C.-120° C., and the drying time is 6 h-8 h.
[0045] S50, sintering the solid mixture to obtain a lithium manganese iron phosphate composite material in which lithium phosphate is coated with lithium manganese iron phosphate. Optionally, the sintering temperature is controlled at 420° C.-480° C., and the sintering time is 6 h-8 h.
[0046] In the above preparation method, lithium iron manganese phosphate powder is added to a mixed solution and the mixed solution is stirred into a gel state, so that the first phosphorus source, the first lithium source and the first carbon source in the mixed solution undergo chemical reactions such as hydrolysis, condensation and polymerization to form a stable sol system, and the lithium iron manganese phosphate particles are relatively evenly distributed in the sol system. The mixed solution in a gel state is dried and sintered to form a lithium iron manganese phosphate composite material in which lithium iron manganese phosphate particles are coated with lithium phosphate. In the lithium iron manganese phosphate composite material, since lithium phosphate is coated on the surface of the lithium iron manganese phosphate particles, the side reaction between the lithium iron manganese phosphate and the electrolyte is greatly slowed down when the lithium iron manganese phosphate composite material is used as a positive electrode material, thereby slowing down the capacity decay of the lithium iron manganese phosphate material during the cycle process, thereby improving the cycle life of the positive electrode material at high temperature.
[0047] It should be noted that by using lithium phosphate to coat lithium iron manganese phosphate particles, on the one hand, lithium phosphate can slow down the side reactions of lithium iron manganese phosphate; on the other hand, lithium phosphate can also serve as a lithium supplement, releasing lithium ions during the charging process to replenish the irreversible capacity loss of the first charge and discharge, thereby significantly improving the energy density of the battery, improving the cycle performance and low-temperature performance, improving the energy efficiency of the energy storage cell, and reducing battery self-discharge.
[0048] Optionally, the first phosphorus source includes at least one of monoammonium hydrogen phosphate, diammonium hydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and phosphoric acid.
[0049] Optionally, the first lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium phosphate, and lithium dihydrogen phosphate.
[0050] Optionally, the first carbon source includes at least one of graphite, carbon nanotubes, acetylene black, graphene, superconducting carbon black, glucose, starch, oxalic acid, asphalt, ethylene glycol, polyethylene glycol, sucrose, and citric acid.
[0051] See also Figure 2 Specifically in the embodiment, step S10 specifically includes:
[0052] S101, prepare a first solution with a manganese source and an iron source as solutes, and prepare a second solution with a second carbon source as solute. Optionally, the first solution can be an aqueous solution with a manganese source and an iron source as solutes. The second solution can be an aqueous solution with a second carbon source as solute. The manganese source can be manganese sulfate, the iron source can be ferrous sulfate, and the second carbon source can be sodium carbonate. The molar ratio of manganese sulfate to ferrous sulfate in the first solution is (2-3): (1.5-2).
[0053] Of course, in other embodiments, the manganese source can also be other raw materials containing manganese, as long as it can provide manganese elements for the preparation of lithium iron manganese phosphate; the iron source can also be other raw materials containing iron, as long as it can provide iron elements for the preparation of lithium iron manganese phosphate; the second carbon source can also be other raw materials containing carbon, as long as it can provide carbon elements for the preparation of lithium iron manganese phosphate, and there is no limitation here.
[0054] S102, mixing the first solution and the second solution, so that the manganese source, the iron source and the second carbon source react chemically to obtain a precipitate of manganese ferrocarbonate. Specifically, the first solution and the second solution are stirred by a stirring device during the mixing process, so that the chemical reaction between the manganese source, the iron source and the second carbon source is faster and more sufficient. Optionally, the volume ratio of the first solution to the second solution is (1-1.5): (1-1.5).
[0055] S103, filtering, washing and drying the precipitate to obtain ferromanganese carbonate material.
[0056] S104, mixing the ferromanganese carbonate material with the second lithium source, the second phosphorus source, and the third carbon source, and then ball milling and drying to obtain a mixed powder. Specifically, alcohol is added when the ferromanganese carbonate material is mixed with the second lithium source, the second phosphorus source, and the third carbon source.
[0057] S105, sintering the mixed powder to obtain lithium iron manganese phosphate powder. Specifically, nitrogen is used to protect the mixed powder during sintering to prevent the mixed powder from contacting with air. The sintering temperature is controlled at 700°C-800°C, and the sintering time is controlled at 10h-20h. It is understandable that after sintering in this step, the lithium iron manganese phosphate needs to be ground and sieved to obtain lithium iron manganese phosphate powder.
[0058] Optionally, the second phosphorus source includes at least one of monoammonium hydrogen phosphate, diammonium hydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and phosphoric acid.
[0059] Optionally, the second lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium phosphate, and lithium dihydrogen phosphate.
[0060] Optionally, the third carbon source includes at least one of graphite, carbon nanotubes, acetylene black, graphene, superconducting carbon black, glucose, starch, oxalic acid, asphalt, ethylene glycol, polyethylene glycol, sucrose, and citric acid.
[0061] It should be noted that the mass proportion of lithium phosphate in the manganese iron phosphate lithium composite material can be adjusted by controlling the amount of the first phosphorus source and the first lithium source. Optionally, the mass proportion of lithium phosphate in the manganese iron phosphate lithium composite material is 0.5%-2%, such as 0.5%, 1.0%, 1.5% or 2.0%.
[0062] Based on the preparation method of the above-mentioned lithium iron manganese phosphate composite material, the present invention also provides a lithium iron manganese phosphate composite material. The lithium iron manganese phosphate composite material includes lithium iron manganese phosphate particles and a coating layer coated on the surface of the lithium iron manganese phosphate particles, and the coating layer includes lithium phosphate. In this way, since lithium phosphate is coated on the surface of the lithium iron manganese phosphate particles, when the lithium iron manganese phosphate composite material is used as a positive electrode material, the side reaction between the lithium iron manganese phosphate and the electrolyte is greatly slowed down, thereby greatly slowing down the capacity decay of the lithium iron manganese phosphate material during the cycle process, thereby greatly improving the cycle life of the positive electrode material at high temperature.
[0063] Based on the above-mentioned lithium iron manganese phosphate composite material, the present invention also provides a positive electrode plate. The positive electrode plate includes a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector. The positive electrode active layer includes the lithium iron manganese phosphate composite material described in any of the above embodiments. It should be noted that, in some embodiments, the positive electrode current collector is only provided with a positive electrode active layer on one side. Of course, in other embodiments, both sides of the positive electrode current collector may be provided with a positive electrode active layer, which is not limited here.
[0064] Based on the above positive electrode sheet, the present invention further provides a battery, which includes the positive electrode sheet as described in any of the above embodiments.
[0065] In order to illustrate the beneficial effects of the preparation method of the lithium iron manganese phosphate composite material of the present application, the lithium iron manganese phosphate composite materials prepared in three embodiments of the present application (i.e., embodiment 1, embodiment 2 and embodiment 3) are compared with the lithium iron manganese phosphate material prepared by the prior art in comparative example 1:
[0066] The difference between Example 1, Example 2 and Example 3 is that in Example 1, a lithium manganese iron phosphate composite material with a lithium phosphate mass ratio of 0.5% is used as the positive electrode active material to prepare a button battery, and the button battery is subjected to a 45°C cycle test. In Example 2, a lithium manganese iron phosphate composite material with a lithium phosphate mass ratio of 1.0% is used as the positive electrode active material to prepare a button battery, and the button battery is subjected to a 45°C cycle test. In Example 3, a lithium manganese iron phosphate composite material with a lithium phosphate mass ratio of 1.5% is used as the positive electrode active material to prepare a button battery, and the button battery is subjected to a 45°C cycle test. In Control Example 1, a button battery is prepared using a lithium manganese iron phosphate material as the positive electrode active material, and the button battery is subjected to a 45°C cycle test.
[0067] Figure 3 The variation curves of capacity retention rate with cycle number in Control Example 1 and Examples 1 to 3 are shown. Figure 3 It can be seen that the capacity retention rate of the control example 1 is 80% after 30 cycles, the capacity retention rate of the embodiment 1 is 80% after 40 cycles, the capacity retention rate of the embodiment 2 is 80% after 75 cycles, and the capacity retention rate of the embodiment 3 is 80% after 50 cycles. It can be seen that compared with the lithium iron manganese phosphate material, the lithium iron manganese phosphate composite material has a lower capacity attenuation rate, which greatly improves the cycle life at high temperature.
[0068] Figure 4 The resistivity of the lithium iron manganese phosphate material in Comparative Example 1 and the lithium iron manganese phosphate composite materials in Examples 1 to 3 are shown. Figure 4 It can be seen that the resistivity of the lithium iron manganese phosphate material in Control Example 1 is 52.3mΩ. The resistivity of the lithium iron manganese phosphate composite material in Example 1 is 46.7mΩ, which is 10.71% lower than the resistivity of the lithium iron manganese phosphate material in Control Example 1. The resistivity of the lithium iron manganese phosphate composite material in Example 2 is 32.3mΩ, which is 38.24% lower than the resistivity of the lithium iron manganese phosphate material in Control Example 1. The resistivity of the lithium iron manganese phosphate composite material in Example 3 is 41.2mΩ, which is 21.22% lower than the resistivity of the lithium iron manganese phosphate material in Control Example 1. It can be seen that the resistivity of the lithium iron manganese phosphate composite material is low, which makes the ion diffusion rate better and greatly improves the electrochemical performance of the positive electrode material.
[0069] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0070] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a lithium manganese iron phosphate composite material, It is characterized in that The following steps are involved: Provide lithium iron manganese phosphate powder; Dissolving a first phosphorus source, a first lithium source, and a first carbon source in a solvent to form a mixed solution; Adding the lithium iron manganese phosphate powder to the mixed solution, and stirring the mixed solution into a gel state; Drying the mixed solution in a gel state to obtain a solid mixture; and The solid mixture is sintered to obtain a lithium manganese iron phosphate composite material in which lithium phosphate is coated with lithium manganese iron phosphate.
2. The method for preparing the lithium iron manganese phosphate composite material according to claim 1, It is characterized in that The step of providing lithium iron manganese phosphate powder specifically includes: preparing a first solution with a manganese source and an iron source as solutes, and preparing a second solution with a second carbon source as solute; Mixing the first solution and the second solution to obtain a precipitate; The precipitate is filtered, washed and dried to obtain ferromanganese carbonate material; The ferromanganese carbonate material is mixed with a second lithium source, a second phosphorus source, and a third carbon source, ball-milled, and dried to obtain a mixed powder; The mixed powder is sintered to obtain the lithium iron manganese phosphate powder.
3. The method for preparing the lithium iron manganese phosphate composite material according to claim 1, It is characterized in that The first phosphorus source includes at least one of monoammonium hydrogen phosphate, diammonium hydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, and phosphoric acid; and / or, The first lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium phosphate, and lithium dihydrogen phosphate; and / or, The first carbon source includes at least one of graphite, carbon nanotubes, acetylene black, graphene, superconducting carbon black, glucose, starch, oxalic acid, asphalt, ethylene glycol, polyethylene glycol, sucrose, and citric acid.
4. The method for preparing the lithium iron manganese phosphate composite material according to claim 1, It is characterized in that The step of adding the lithium iron manganese phosphate powder to the mixed solution and stirring the mixed solution into a gel state specifically includes: The mixed solution is stirred, and during the stirring process, the lithium iron manganese phosphate powder is continuously added to the mixed solution until the mixed solution is stirred into a gel state.
5. The method for preparing the lithium iron manganese phosphate composite material according to claim 4, It is characterized in that In the step of stirring the mixed solution: The temperature of the mixed solution is controlled to be 80° C.-90° C., and the stirring speed is controlled to be 800 rpm-1000 rpm.
6. The method for preparing the lithium iron manganese phosphate composite material according to claim 1, It is characterized in that In the step of drying the mixed solution in a gel state to obtain a solid mixture: the drying temperature is 100° C.-120° C., and the drying time is 6 h-8 h; and / or, In the step of sintering the solid mixture: the sintering temperature is 420° C.-480° C., and the sintering time is 6 h-8 h.
7. The method for preparing the lithium iron manganese phosphate composite material according to claim 1, It is characterized in that The mass proportion of lithium phosphate in the lithium manganese iron phosphate composite material is 0.5%-2%.
8. A lithium manganese iron phosphate composite material prepared by the preparation method according to any one of claims 1 to 7, It is characterized in that The invention comprises lithium iron manganese phosphate particles and a coating layer coated on the surface of the lithium iron manganese phosphate particles, wherein the coating layer comprises lithium phosphate.
9. A positive electrode sheet, It is characterized in that The invention comprises a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises the lithium manganese iron phosphate composite material as claimed in claim 8.
10. A battery, It is characterized in that Comprising the positive electrode sheet as described in claim 9.
Citation Information
Cited By
Lithium manganese iron phosphate positive electrode material, preparation method and pure power battery
CN121331804A