Sintered bodies and cutting tools

By controlling the boron concentration in the diamond particles and the bonding material, the oxidation resistance and necking effect of the diamond particles are optimized to form a wear-resistant cutting tip, thus solving the problem of short tool life and achieving extended tool life and improved wear resistance.

CN119156360BActive Publication Date: 2026-11-17SUMITOMO ELECTRIC HARDMETAL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280096151.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-25
Publication Date
2026-11-17
Estimated Expiration
2042-05-25

AI Technical Summary

Technical Problem

In existing technologies, cutting tools have short tool life, making it difficult to meet the needs of high-efficiency machining.

Method used

By controlling the boron concentration range in diamond particles and the bonding material, a new sintered body is formed. The bonding material contains compounds of cobalt, boron, and carbon. The oxidation resistance and necking effect of the diamond particles are optimized. The strength and resistivity of the bonding material, the particle size and ratio of the diamond particles are combined to form a wear-resistant cutting tip.

Benefits of technology

It significantly improves the tool life of cutting tools, enhances the wear resistance and oxidation resistance of the cutting tip, suppresses the generation of frictional plasma, and extends the service life of cutting tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119156360B_ABST
    Figure CN119156360B_ABST
Patent Text Reader

Abstract

The sintered body comprises diamond particles and a binder. The boron concentration in the diamond particles is ≥0.001% by mass and ≤0.1% by mass. The boron concentration in the binder is ≥0.01% by mass and ≤0.5% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to sintered bodies and cutting tools. Background Technology

[0002] Patent Document 1 (Japanese Patent Application Publication No. 2008-133172) discloses a sintered body. The sintered body disclosed in Patent Document 1 is formed by mixing boron-doped diamond powder and carbonate powder, and then heating and pressurizing the mixture.

[0003] Patent Document 2 (Japanese Patent Application Publication No. 58-199777) discloses a sintered body. The sintered body described in Patent Document 2 is formed by mixing diamond powder and catalyst metal powder, and then heating and pressurizing the mixture. Furthermore, the catalyst metal powder includes boron carbide additive powder and metal powder (iron, nickel, cobalt, etc.).

[0004] Existing technical documents Patent documents: Patent Document 1: Japanese Patent Application Publication No. 2008-133172; Patent Document 2: Japanese Patent Application Publication No. 58-199777. Summary of the Invention

[0005] The sintered body disclosed herein comprises diamond particles and a binder material. The boron concentration in the diamond particles is 0.001% by mass or more and 0.1% by mass or less. The boron concentration in the binder material is 0.01% by mass or more and 0.5% by mass or less. Attached Figure Description

[0006] Figure 1 This is a top view of cutting blade 100.

[0007] Figure 2 This is a 3D view of cutting blade 100.

[0008] Figure 3 This is a process diagram showing the manufacturing method of the sintered body constituting the blade tip 20. Detailed Implementation

[0009] [The problem this disclosure aims to solve] The inventors of this invention have conducted in-depth research, and as a result, it has been found that when the sintered bodies described in Patent Document 1 and Patent Document 2 are applied to cutting tools, there is room for improvement in tool life. This disclosure provides a sintered body that can improve tool life when applied to cutting tools.

[0010] [The Effects of This Disclosure] According to the sintered body disclosed herein, tool life can be improved when applied to cutting tools.

[0011] [Description of embodiments of this disclosure] First, embodiments of this disclosure will be described.

[0012] (1) In one embodiment, the sintered body comprises diamond particles and a binder material. The boron concentration in the diamond particles is 0.001% by mass or more and 0.1% by mass or less. The boron concentration in the binder material is 0.01% by mass or more and 0.5% by mass or less.

[0013] The sintered body according to (1) above can improve tool life when applied to cutting tools.

[0014] (2) Alternatively, in the sintered body of (1) above, the boron concentration in the bonding material is 0.05% by mass or more and 0.5% by mass or less.

[0015] (3) Alternatively, the sintered body of (1) or (2) above may also contain a compound precipitated in the bonding material. Alternatively, the compound may contain at least two of cobalt, boron, and carbon. Alternatively, the value obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction is 0.15 or less.

[0016] (4) Alternatively, in the sintered body of (3) above, the compound is Co. 22 B4C2, W2Co 21 At least one of B6, W2Co2B6, and CoWB.

[0017] (5) Alternatively, in the sintered body of (3) or (4) above, the value obtained by dividing the peak intensity of the compound when X-ray diffraction is performed by the peak intensity of diamond is 0.01 or more and 0.15 or less.

[0018] (6) Alternatively, in the sintered body of (1) to (5) above, the resistivity measured in the state after removing the binding material is 3.0 Ω·cm or less.

[0019] According to the sintered body described in (6) above, when applied to a cutting tool, it is possible to suppress the generation of triboelectric plasma.

[0020] (7) Alternatively, in the sintered body described in (1) to (6) above, the average particle size of the diamond particles is 0.5 μm or more and 50 μm or less. Alternatively, the proportion of diamond particles in the sintered body is 80% or more by volume and 99% or less by volume.

[0021] (8) Alternatively, in the sintered bodies described in (1) to (7) above, the bonding material may include at least one element selected from the group consisting of elemental metals, alloys, and intermetallic compounds. Alternatively, the elemental metals, alloys, and intermetallic compounds may include at least one metallic element selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, iron, aluminum, silicon, cobalt, and nickel.

[0022] (9) Alternatively, in the sintered bodies of (1) to (8) above, the bonding material may contain at least cobalt.

[0023] (10) The cutting tool according to one embodiment has a cutting tip. The cutting tip is formed from the sintered body of (1) to (9) above.

[0024] The cutting tool described in (10) above can improve tool life.

[0025] [Details of the embodiments disclosed herein] The embodiments of this disclosure will be described in detail with reference to the accompanying drawings. In the following drawings, the same or equivalent parts are labeled with the same reference numerals, and the description will not be repeated.

[0026] The cutting tool involved in the embodiment is, for example, the cutting insert 100. The cutting tool involved in the embodiment is not limited to the cutting insert 100, but hereafter, the cutting insert 100 will be described as an example of the cutting tool involved in the embodiment. Other examples of the cutting tool involved in the embodiment include drill bits, end mills, wear-resistant tools, etc.

[0027] (The configuration of the cutting tool involved in the implementation method) The structure of the cutting insert 100 will be explained.

[0028] <Overview of the structure of cutting insert 100> Figure 1 This is a top view of cutting blade 100. Figure 2 This is a 3D view of the cutting blade 100. (See image below.) Figure 1 as well as Figure 2 As shown, the cutting insert 100 has a base material 10 and a cutting tip 20. The cutting insert 100 is polygonal in shape (e.g., triangular) when viewed from above. The polygonal shape (triangular shape) may not be strictly polygonal (triangular). More specifically, the corners of the cutting insert 100 may also be rounded when viewed from above.

[0029] The substrate 10 is polygonal in shape (e.g., triangular) when viewed from above. The substrate 10 has a top surface 10a, a bottom surface 10b, and a side surface 10c. The top surface 10a and bottom surface 10b are end faces of the substrate 10 in the thickness direction. The bottom surface 10b is the opposite surface of the top surface 10a in the thickness direction. The side surface 10c is a surface connected to the top surface 10a and bottom surface 10b.

[0030] The top surface 10a has a mounting portion 10d. When viewed from above, the mounting portion 10d is located at a corner of the top surface 10a. The distance between the top surface 10a and the bottom surface 10b within the mounting portion 10d is smaller than the distance between the top surface 10a and the bottom surface 10b outside the mounting portion 10d. That is, a step exists between the mounting portion 10d and the portion of the top surface 10a outside the mounting portion 10d.

[0031] A through hole 11 is formed in the substrate 10. The through hole 11 penetrates the substrate 10 in the thickness direction. The through hole 11 is formed at the center of the substrate 10 when viewed from above. The cutting blade 100 is used for cutting, for example, by inserting a fixing member (not shown) into the through hole 11 and fastening the fixing member to a tool holder (not shown). However, it is also possible not to form a through hole 11 in the substrate 10.

[0032] The substrate 10 is formed, for example, of cemented carbide. Cemented carbide is a composite material formed by sintering carbide particles and a binder material. The carbide particles are, for example, particles of tungsten carbide, titanium carbide, tantalum carbide, etc. The binder material is, for example, cobalt, nickel, iron, etc. However, the substrate 10 may also be formed of materials other than cemented carbide.

[0033] The cutting tip 20 is mounted on the mounting portion 10d. The cutting tip 20 is mounted to the substrate 10, for example, by brazing. The cutting tip 20 has a rake face 20a, a flank face 20b, and a cutting edge 20c. The rake face 20a is connected to a portion of the top surface 10a other than the mounting portion 10d. The flank face 20b is connected to the side surface 10c. The cutting edge 20c is formed along the ridge line of the rake face 20a and the flank face 20b. A backing metal 21 may also be disposed on the bottom surface of the cutting tip 20 (the surface opposite to the rake face 20a). The backing metal 21 is, for example, formed of cemented carbide.

[0034] <Detailed Structure of the Sintered Body Constituting the Blade Tip 20> The blade tip 20 is formed of a sintered body comprising diamond particles and a binder material. The average particle size of the diamond particles in the sintered body constituting the blade tip 20 is preferably 0.5 μm or more and 50 μm or less. The proportion (volume ratio) of the diamond particles in the sintered body constituting the blade tip 20 is preferably 80% or more and 99% or less by volume. The binder material includes, for example, cobalt. In addition to cobalt, the binder material may also include tungsten or titanium. Cobalt is preferably the most abundant component in the binder material.

[0035] The average particle size of the diamond particles in the sintered body constituting the tip 20 is calculated by the following method.

[0036] In calculating the average particle size of the diamond particles in the sintered body constituting the blade tip 20, firstly, a sample including a cross-section is cut from any position of the blade tip 20. This sample cutting is performed, for example, using a focused ion beam device, a cross-section polishing machine, or the like.

[0037] Second, the cross-section of the cut sample was observed using a scanning electron microscope (SEM). This observation yielded a reflected electron image (hereinafter referred to as a "SEM image") of the cross-section of the cut sample. During the SEM observation, the magnification was adjusted to include more than 100 diamond particles within the measurement field. SEM images were acquired at five locations within the cross-section of the cut sample.

[0038] Third, the particle size distribution of diamond particles within the measurement field of view is obtained by image processing of the SEM image. This particle size distribution is a number-based distribution. Image processing is performed using, for example, Win ROOF ver. 7.4.5 or Win ROOF 2018 manufactured by Mitani Corporation. The particle size of each diamond particle is obtained by calculating the equivalent circle diameter based on the area of ​​each diamond particle obtained as a result of image processing. Furthermore, when obtaining the particle size distribution, a portion of diamond particles located outside the measurement field of view is not considered.

[0039] Fourth, the median particle size of the diamond particles contained within the measurement field of view is determined based on the particle size distribution of the diamond particles contained within the measurement field of view as described above. The value obtained by averaging the determined median particle size over five SEM images is regarded as the average particle size of the diamond particles in the sintered body constituting the blade tip 20.

[0040] The proportion of diamond particles in the sintered body constituting the blade tip 20 is calculated using the following method. In calculating the proportion of diamond particles in the sintered body constituting the blade tip 20, firstly, a sample including a cross-section is cut from any position of the blade tip 20. This sample cutting is performed, for example, using a focused ion beam apparatus, a cross-section polishing machine, or the like.

[0041] Second, the cross-section of the cut sample was observed using SEM. This observation yielded SEM images of the cut sample's cross-section. During the SEM observation, the magnification was adjusted to include more than 100 diamond particles within the measurement field. SEM images were acquired at five locations within the cross-section of the cut sample.

[0042] Third, by processing the SEM image, the proportion of diamond particles contained within the measured field of view is calculated. This image processing is performed, for example, using Win ROOF ver. 7.4.5 manufactured by Mitani Corporation. WinROOF2018 and other methods were used to binarize the SEM images. The dark areas in the binarized SEM images corresponded to the regions where diamond particles were present. The value obtained by dividing the area of ​​the dark area by the area of ​​the measurement region was regarded as the volume ratio of the diamond particles in the sintered body constituting the blade tip 20.

[0043] The boron concentration in the diamond particles is 0.001% by mass or more and 0.1% by mass or less. The boron concentration in the bonding material is 0.01% by mass or more and 0.5% by mass or less. Preferably, the boron concentration in the bonding material is greater than or equal to the boron concentration in the diamond particles (i.e., the value obtained by subtracting the boron concentration in the diamond particles from the boron concentration in the bonding material is preferably 0% by mass or more). The boron concentration in the bonding material may be 0.05% by mass or more and 0.5% by mass or less.

[0044] The boron concentration in the diamond particles and the boron concentration in the bonding material were determined by the following method.

[0045] In determining the boron concentration in diamond particles and the boron concentration in the bonding material, firstly, a sample is cut from any position at the tip 20. Secondly, the cut sample is acid-treated. Through this acid treatment, the components of the bonding material contained in the sample are substantially completely dissolved in the acid. That is, the sample after acid treatment is essentially composed only of diamond particles.

[0046] The acid treatment described above was performed using an aqueous solution of fluoronitric acid. This aqueous solution was prepared by mixing a 50% aqueous solution of hydrogen fluoride and a 60% aqueous solution of nitric acid in a 1:1 ratio. The acid treatment was carried out by immersing the sample in the aqueous solution of fluoronitric acid and maintaining it at 200°C for 48 hours.

[0047] Third, glow discharge mass spectrometry analysis was performed on the acid-treated sample to determine the boron concentration in the diamond particles. Additionally, inductively coupled plasma (ICP-C) analysis was performed on the acid used in the acid treatment to determine the boron concentration in the bonding material.

[0048] Compounds can also precipitate from the bonding material. These precipitated compounds contain at least two of cobalt, boron, and carbon. For example, Co is a compound precipitated from the bonding material. 22 B4C2, W2Co 21At least one of B6, W2Co2B6, and CoWB.

[0049] The value obtained by dividing the peak intensity of the compound constituting the sintered body of the blade tip 20 by the peak intensity of diamond during X-ray diffraction is, for example, 0.15 or less. The value obtained by dividing the peak intensity of the compound constituting the sintered body of the blade tip 20 by the peak intensity of diamond during X-ray diffraction is preferably 0.01 or more and 0.15 or less. Furthermore, the value obtained by dividing the peak intensity of the compound constituting the sintered body of the blade tip 20 by the peak intensity of diamond during X-ray diffraction is, for example, greater than 0.

[0050] The value obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction of the sintered body constituting the blade tip 20 is determined by the following method. First, a sample containing a cross-section is cut from any position of the blade tip 20. This sample cutting is performed, for example, using a focused ion beam apparatus or a cross-section polishing machine. Second, the composition of the diamond particles and the bonding material is determined by X-ray diffraction in the aforementioned cross-section. Third, the X-ray diffraction pattern is obtained by analyzing the aforementioned cross-section using X-ray diffraction. The analysis based on X-ray diffraction is performed using Cu-Kα rays with a wavelength of 1.54 Å, a tube voltage of 40 kV, a tube current of 15 mA, a multilayer filter, and a lumped optical system, using the θ-2θ method.

[0051] Fourth, based on the aforementioned X-ray diffraction pattern and the composition of the diamond particles and the bonding material, the peak intensities (peak height, cps) originating from each component are determined. The peak intensities are obtained using the first peak of each component. Fifth, by dividing the sum of the peak intensities of the compounds in the bonding material obtained as described above by the sum of the diamond peaks, the value obtained by dividing the peak intensities of the compounds by the peak intensities of the diamond when performing X-ray diffraction on the sintered body constituting the blade tip 20 is obtained.

[0052] The resistivity of the sintered body constituting the blade tip 20 after removing the bonding material is preferably 3.0 Ω·cm or less. The bonding material is removed by acid treatment, similar to that used when determining the boron concentration in diamond particles. The resistivity of the sintered body is measured using a four-terminal method. The resistivity of the sintered body is measured using a 182 SENSITIVE DIGITAL VOLTMETER manufactured by KEITHLEY, under conditions of a measurement temperature of 22°C, a measurement humidity of 60%, and an electrode spacing of 0.5 mm. A four-probe manufactured by NTT Advance Technology is used as the probe for the measurement device. A 3 mm × 1 mm × 6 mm sample is cut from the sintered body constituting the blade tip 20 for resistivity measurement.

[0053] The diamond powder prepared in powder preparation step S1 does not contain boron. Boron is introduced into the diamond particles in sintering step S3, so the boron tends to be present near the surface of the diamond particles. Therefore, if the boron concentration in the diamond particles is the same, the resistivity of the sintered body constituting the blade tip 20 after removing the bonding material is smaller than the resistivity of the sintered body obtained by sintering pre-doped boron-containing diamond powder.

[0054] <Manufacturing method of the sintered body constituting the blade tip 20> Figure 3 This is a process diagram illustrating the manufacturing method of the sintered body constituting the blade tip 20. (Example) Figure 3 As shown, the manufacturing method of the sintered body constituting the blade tip 20 includes a powder preparation step S1, a powder mixing step S2, and a sintering step S3.

[0055] In the powder preparation step S1, diamond powder, binder powder, and boron-added powder are prepared. The diamond powder is powder of diamond, and the binder powder is powder formed from the materials constituting the binder. The boron-added powder is powder of boron or boron oxide. The ratio of diamond powder, binder powder, and boron-added powder is appropriately selected based on the volume ratio of diamond particles in the sintered body constituting the blade tip 20 and the boron concentration in the diamond particles and the binder.

[0056] The powder mixing process S2 is divided into a first process and a second process performed after the first process. In the first process, the boron-added powder is pulverized. The pulverization of the boron-added powder is performed, for example, so that the average particle size of the boron-added powder is 5 μm or less. The pulverization of the boron-added powder may also be performed after mixing the diamond powder and the binder powder with the boron-added powder. The pulverization of the boron-added powder is preferably performed so that the average particle size of the boron-added powder is 0.5 μm or less. The average particle size of the boron-added powder is measured, for example, by a particle size distribution measuring device such as Microtrac. The smaller the average particle size of the pulverized boron-added powder, the easier it is to introduce boron into the diamond particles in the sintering process S3. In the second process, the diamond powder, the binder powder, and the pulverized boron-added powder are mixed. This mixing is performed using, for example, a grinding mill or a ball mill. However, the mixing method is not limited to these. Hereinafter, the powder obtained by mixing the diamond powder, the binder powder, and the boron-added powder is referred to as "mixed powder".

[0057] In sintering step S3, the mixed powder is sintered. This sintering is performed by placing the mixed powder in a container and holding it at a predetermined sintering temperature and under a predetermined sintering pressure. To prevent impurities from contaminating the mixed powder (sintered body), the container is made of a high-melting-point metal such as tantalum or niobium. The sintering temperature can be appropriately selected based on the boron concentration in the diamond particles and the boron concentration in the bonding material. The sintering temperature is, for example, 1500°C or higher and 1700°C or lower. Furthermore, the higher the sintering temperature, the easier it is for boron to diffuse into the diamond particles; however, if the sintering temperature is too high, graphitization of the diamond is more likely to occur, reducing the strength of the bonding material. The sintering pressure is, for example, 4.5 GPa or higher and 6.5 GPa or lower. The holding time is, for example, 40 minutes or higher and less than 60 minutes.

[0058] (Effects of the cutting tool involved in the implementation method) The following explains the effect of the cutting blade 100.

[0059] By incorporating boron into the diamond particles, their oxidation resistance can be improved, resulting in improved wear resistance of the cutting tip 20. According to the inventors' findings, when the boron concentration in the diamond particles is less than 0.001% by mass, there is no improvement in oxidation resistance of the boron-based diamond particles. On the other hand, if the boron concentration in the diamond particles is greater than 0.1% by mass, there is an excess of boron in the diamond particles, leading to a decrease in the hardness of the diamond particles and a reduction in the wear resistance of the cutting tip 20.

[0060] In sintering step S3, the binder powder melts, and the boron additive powder dissolves in the molten binder. Furthermore, a portion of the diamond powder dissolves in the molten binder, causing diamond particles to precipitate again, thereby resulting in the bonding (necking) of the diamond particles together. The boron in the dissolved binder acts as a sintering aid; therefore, when the boron concentration in the binder is less than 0.01% by mass, necking of the diamond particles is unlikely to occur. Additionally, according to the inventors' findings, when the boron concentration in the binder is greater than 0.5% by mass, compounds containing cobalt, boron, carbon, etc., readily precipitate in the binder. These compounds reduce the strength and wear resistance of the binder.

[0061] In the cutting insert 100, the boron concentration in the diamond particles contained in the sintered body constituting the tip 20 is 0.001% by mass or more and 0.1% by mass or less, thus improving the oxidation resistance of the diamond particles while maintaining their hardness. In the cutting insert 100, the boron concentration in the bonding material contained in the sintered body constituting the tip 20 is 0.01% by mass or more and 0.5% by mass or less, thus ensuring the neck growth strength between the diamond particles and the strength of the bonding material. Therefore, the wear resistance of the tip 20 can be improved according to the cutting insert 100.

[0062] When the average particle size of the diamond particles in the sintered body constituting the blade tip 20 is less than 0.5 μm, the surface area of ​​the diamond particles increases, thus facilitating oxidation of the diamond particle surface. When the average particle size of the diamond particles in the sintered body constituting the blade tip 20 is greater than 50 μm, the toughness of the sintered body constituting the blade tip 20 decreases, making it prone to defects. Therefore, by setting the average particle size of the diamond particles in the sintered body constituting the blade tip 20 to be between 0.5 μm and 50 μm, the wear resistance of the blade tip 20 can be further improved.

[0063] When the proportion of diamond particles in the sintered body constituting the cutting tip 20 is less than 80% by volume, the hardness of the cutting tip 20 decreases. Therefore, by setting the proportion of diamond in the sintered body constituting the cutting tip 20 to 80% or more and 99% or less by volume, the wear resistance of the cutting tip 20 can be further improved.

[0064] When the cutting tip 20 becomes charged due to contact with the workpiece, frictional plasma may be generated between the cutting tip 20 and the workpiece, making wear of the cutting tip 20 more likely. However, when the resistivity of the sintered body constituting the cutting tip 20, measured after removing the bonding material, is 3.0 Ω·cm or less, the cutting tip 20 is less likely to become charged due to contact with the workpiece, thus suppressing wear of the cutting tip 20 caused by the generation of frictional plasma.

[0065] (Example) To evaluate the relationship between the particle size of the boron-added powder prepared in the powder preparation step S1 and the boron concentration in the binder material contained in the sintered body constituting the blade tip 20, Sample 1 and Sample 2 were prepared as sintered body samples. As shown in Table 1, in Sample 1 and Sample 2, the ratio of the mass of the boron-added powder to the mass of the binder material powder (the value obtained by dividing the mass of the boron-added powder by the mass of the binder material powder), sintering pressure, sintering temperature, and sintering time were the same. However, in Sample 1, the average particle size of the boron-added powder was less than 5 μm, while in Sample 2, the average particle size of the boron-added powder was greater than 5 μm.

[0066]

[0067] As shown in Table 1, in Sample 1, the boron concentration in the bonding material is between 0.01% and 0.5% by mass. In Sample 2, the boron concentration in the bonding material is not between 0.01% and 0.5% by mass. Furthermore, in both Sample 1 and Sample 2, the boron concentration in the diamond particles is between 0.001% and 0.1% by mass. This comparison shows that by making the average particle size of the boron-added powder less than 5 μm, it is possible to achieve a boron concentration in the bonding material that is between 0.01% and 0.5% by mass.

[0068] To evaluate the relationship between the boron concentration in the diamond particles and the bonding material of the sintered body constituting the blade tip 20 and the wear resistance of the blade tip 20, samples 3 to 24 were prepared as sintered body samples. As shown in Table 2, the boron concentration in the diamond particles and the bonding material of the sintered body constituting the blade tip 20 varied in samples 3 to 24.

[0069]

[0070] Condition A is defined as a boron concentration in the diamond particles being 0.001% by mass or more and 0.1% by mass or less, and condition B is defined as a boron concentration in the bonding material being 0.01% by mass or more and 0.1% by mass or less. In samples 3 to 18, both conditions A and B are satisfied. In samples 19 to 24, at least one of conditions A and B is not satisfied.

[0071] For cutting tests, cutting inserts with a tool tip 20 formed using samples 3 to 24 were prepared. These cutting inserts have a shape corresponding to the SNEW1204ADFR cutting insert manufactured by Sumitomo Electric Carbide Co., Ltd. Furthermore, these cutting inserts were mounted on a retainer RF4160R manufactured by Sumitomo Electric Carbide Co., Ltd., and used for milling operations. The milling operation was performed with a feed rate of 0.2 mm / t and a depth of cut of 0.6 mm. This cutting operation was a dry machining process without coolant. The workpiece dimensions for this cutting operation were 90 mm × 90 mm × 90 mm, and the material of the workpiece was a glass-containing resin. In the cutting tests, the number of passes that could be machined until the average flank wear reached 250 μm was evaluated.

[0072]

[0073] As shown in Table 3, among the cutting inserts with the tip 20 formed using samples 3 to 18, the number of machining passes is increased compared to those with the tip 20 formed using samples 19 to 24. As described above, samples 3 to 18 satisfy both conditions A and B, while samples 19 to 24 do not satisfy at least one of conditions A and B. This comparison shows that satisfying both conditions A and B improves the wear resistance of the tip 20.

[0074] Condition C is defined as having an average diamond particle size of 0.5 μm or more and 50 μm or less. Condition D is defined as having a diamond particle proportion of 80% or more and 99% or less in the sintered body. In samples 3 to 15, conditions A and B are met, as are conditions C and D. In samples 16 to 18, conditions A and B are met, but neither condition C nor condition D is met.

[0075] Furthermore, among the cutting inserts with the tip 20 formed using samples 3 to 15, the number of machining passes is increased compared to those with the tip 20 formed using samples 16 to 18. This comparison shows that by further satisfying conditions C and D, the wear resistance of the tip 20 can be further improved.

[0076] Table 3 also shows the values ​​obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction. In samples 3 to 18, the values ​​obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction were less than 0.15. In samples 20 and 21, where the boron concentration in the bonding material was greater than 0.5% by mass, the values ​​obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction were greater than 0.15. Therefore, by setting the boron concentration in the bonding material to less than 0.5% by mass and obtaining a value of less than 0.15 for the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction, the precipitation of compounds in the bonding material can be suppressed.

[0077] To evaluate the effect of pre-doping boron in diamond powder on the resistivity of the sintered body after the binder material has been removed, samples 25 and 26 were prepared as sintered body samples. As shown in Table 4, in samples 25 and 26, the boron concentration in the diamond particles and the boron concentration in the binder material were the same. Sample 25 was formed using undoped diamond powder. In sample 26, half of the diamond powder was pre-doped with boron.

[0078]

[0079] As shown in Table 5, in sample 25, the resistivity of the sintered body after removing the binder material was below 3.0 Ω·cm. On the other hand, in sample 26, the resistivity of the sintered body after removing the binder material was greater than 3.0 Ω·cm. This comparison shows that, even without pre-doping boron into the diamond powder, and even with the same boron concentration in the diamond particles, boron tends to be present on the surface of the diamond particles, thus improving the resistivity of the sintered body after removing the binder material.

[0080]

[0081] (Variation example) In the above description, the case in which the bonding material contained in the sintered body constituting the blade tip 20 is cobalt was used as an example, but the bonding material contained in the sintered body constituting the blade tip 20 is not limited to cobalt.

[0082] The bonding material contained in the sintered body constituting the blade tip 20 may also include at least one element selected from the group consisting of monomeric metals, alloys, and intermetallic compounds. This monomeric metal, alloy, and intermetallic compound includes at least one metallic element selected from the group consisting of Group IV elements (e.g., titanium, zirconium, hafnium), Group V elements (e.g., vanadium, tantalum, niobium), Group VI elements (e.g., chromium, molybdenum, tungsten), aluminum, iron, silicon, cobalt, and nickel. Furthermore, the aforementioned periodic table refers to a so-called long-period periodic table.

[0083] In the above description, the case where the cutting blade 100 has a base material 10 has been described, but the portion of the cutting blade 100 other than the tip portion 20 may also be formed from the same sintered body as the tip portion 20.

[0084] The embodiments disclosed herein should be considered exemplary in all respects, not limiting. The scope of the invention is defined not by the above-described embodiments, but by the claims, and is intended to include all modifications equivalent to and within the scope of the claims.

[0085] Explanation of reference numerals in the attached figures 10: Substrate; 10a: Top surface; 10b: Bottom surface; 10c: Side surface; 10d: Mounting part; 11: Through hole; 20: Tool tip; 20a: Rake face; 20b: Back face; 20c: Cutting edge; 21: Backing metal; 100: Cutting insert; S1: Powder preparation process; S2: Powder mixing process; S3: Sintering process.

Claims

1. A sintered body, wherein, The sintered body comprises diamond particles, a binder, and a compound precipitated in the binder. The boron concentration in the diamond particles is above 0.001% by mass and below 0.1% by mass. The boron concentration in the bonding material is above 0.01% by mass and below 0.5% by mass. The compound is Co. 22 B4C2, W2Co 21 At least one of B6, W2Co2B6, and CoWB The value obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction is less than 0.

15. The bonding material comprises at least one selected from the group consisting of elemental metals, alloys, and intermetallic compounds. The elemental metal, the alloy, and the intermetallic compound comprise at least one metallic element selected from the group consisting of Group 4, Group 5, Group 6 elements of the periodic table, iron, aluminum, silicon, cobalt, and nickel. The periodic table is a long-period periodic table.

2. The sintered body according to claim 1, wherein, The boron concentration in the bonding material is above 0.05% by mass and below 0.5% by mass.

3. The sintered body according to claim 1, wherein, The value obtained by dividing the peak intensity of the compound by the peak intensity of diamond during X-ray diffraction is greater than 0.01 and less than 0.

15.

4. The sintered body according to any one of claims 1 to 3, wherein, The resistivity measured with the bonding material removed is below 3.0 Ω·cm.

5. The sintered body according to any one of claims 1 to 3, wherein, The diamond particles have an average particle size of 0.5 μm or more and 50 μm or less. The proportion of diamond particles in the sintered body is above 80% by volume and below 99% by volume.

6. The sintered body according to any one of claims 1 to 3, wherein, The bonding material contains at least cobalt.

7. A cutting tool, wherein, The cutting tool has a cutting tip. The blade tip is formed from the sintered body as described in any one of claims 1 to 6.

Citation Information

Patent Citations

  • Diamond sintered body for tool and manufacture

    JP1983199777A

  • Boron-doped diamond sinter and process for producing the same

    JP2008133172A

  • Sintered body and cutting tool

    CN116529004A