Water-based fireproof coating ceramic simulating method
By optimizing the formula and construction process of water-based fire retardant coatings, combined with lignin nanoparticles and other nanomaterials, the problem of differences in appearance and texture of traditional fire retardant coatings has been solved, significantly improving its fire retardant performance and aesthetics, making it more suitable for use For high-end architectural decoration.
Patent Information
- Application Number
- CN202410879273.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2025-01-24
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional fire-retardant coatings have differences from traditional porcelain surfaces in appearance and texture, which limits their application in high-end architectural decoration fields.
By optimizing the formula and construction process of water -based fireproof coatings, including the use of lignin nanoparticles, modified boron nanomallide particles, aluminum hydroxide, titanium pink powder, talc powder, high luster additives, etc. Nano particles, using alkaline gel treatment and high temperature or frozen drying and crushing, significantly improve the fire resistance and appearance of the coating.
It significantly improves the fire performance and appearance of water -based fireproof coatings, makes it close to the gloss and texture of the traditional porcelain surface, and enhances its application potential in the field of high -end building decoration.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fire retardant coatings, and in particular relates to a method for imitating porcelain of water-based fire retardant coatings. Background Art
[0002] Fire retardant coatings not only effectively improve the fire resistance level of buildings, but also provide more design space and options for architects and owners. However, traditional fire retardant coatings also face some problems and challenges in practical applications. The most prominent problem is that they have high VOC (volatile organic compounds) emissions and are significantly different from traditional porcelain surfaces in appearance and texture. This limits the widespread application of traditional fire retardant coatings in the field of high-end building decoration, especially in places that have high requirements for building appearance, such as high-end residences, commercial buildings and public facilities.
[0003] As a new type of environmentally friendly material, water-based fire retardant coatings usually have water-based emulsions, flame retardants, fillers, and additives as their main ingredients. They mainly play a fire-retardant role by forming a fire-retardant film or inhibiting the spread of flames. Compared with traditional organic solvent-based fire retardant coatings, water-based fire retardant coatings do not contain harmful substances, have the advantages of low VOC emissions, non-toxic and odorless, and environmentally friendly construction, which is in line with the development direction of energy conservation and environmental protection in modern buildings.
[0004] However, although water-based fire retardant coatings have significantly improved their fireproof performance, they are difficult to achieve the gloss and texture of traditional porcelain surfaces in appearance, which restricts their further application in the field of high-end architectural decoration. The surface of water-based fire retardant coatings after application usually presents a relatively smooth but lacks gloss, which is relatively rough and plain compared with traditional porcelain surfaces. This difference in appearance not only limits the application of water-based fire retardant coatings in high-end architectural decoration, but also affects its competitiveness and development space in the market.
[0005] Therefore, how to improve the appearance and texture of water-based fire retardant coatings so that they can better simulate the gloss and texture of traditional porcelain surfaces has become one of the technical problems that need to be solved in the current research and development and application of fire retardant coatings. Through technical means and formula optimization, water-based fire retardant coatings can maintain their fire retardant performance and environmental protection characteristics while achieving a similar appearance to porcelain surfaces. This will be one of the important research directions and market demands in the field of fire retardant coatings in the future. Summary of the invention
[0006] The purpose of the present invention is to provide a method for imitating porcelain of water-based fire retardant coatings, which can significantly improve the fireproof performance and appearance of the water-based fire retardant coatings by optimizing the formula and construction process of the fire retardant coatings, and further improve the safety and environmental stability of the water-based fire retardant coatings.
[0007] A water-based fire-retardant coating, which comprises the following raw materials by weight: 100 parts of deionized water, 10-30 parts of polyvinyl alcohol, 3-5 parts of xanthan gum, 5-10 parts of lignin nanoparticles, 3-7 parts of modified boron nitride nanoparticles, 5-10 parts of aluminum hydroxide, 5-10 parts of titanium dioxide, 5-10 parts of talc, 3-7 parts of sodium tetraborate, 3-7 parts of sodium hydroxide, 3-5 parts of high gloss additives, and 1-3 parts of pigments. The preparation process comprises the following steps: S1. Synthesis of Lignin Nanoparticles: The desired lignin powder was extracted from giant reed plants and then lignin nanoparticles were synthesized via a nanoprecipitation method.
[0008] S2. Mixing of water-based fire retardant coating: deionized water, polyvinyl alcohol, xanthan gum, lignin nanoparticles, modified boron nitride nanoparticles, aluminum hydroxide, titanium dioxide, talc, high gloss additives and pigments are uniformly mixed in required proportions at a temperature of 50-70°C and a rotation speed of 1000-3000 r / min for 10-20 h to obtain a mixed suspension.
[0009] S3. Alkaline gelation of water-based fire retardant coating: Add sodium hydroxide and sodium tetraborate in a required proportion to the mixed suspension obtained in step S2, and stir at a temperature of 50 to 60° C. for 10 to 30 minutes to obtain a gelled fire retardant material.
[0010] S4. Gel drying and crushing: The gelled fireproof material obtained in step S3 is fully dried by high temperature drying or freeze drying, and then crushed to obtain micron-sized mixed particles.
[0011] S5. Redissolving the particles: The mixed particles obtained in step S4 are mixed with deionized water in a ratio of 1:5 at a temperature of 50-70°C using a mechanical stirrer at a stirring speed of 1000-3000 r / min, and then placed in a vacuum box at 1-5 Pa for degassing to obtain a water-based fire retardant coating.
[0012] In some embodiments, the specific steps of synthesizing lignin nanoparticles by nanoprecipitation method in step S1 are as follows: (1) 10-20 parts of air-dried lignin powder extracted from giant reed were added to 100 parts of 70% acetone and then ultrasonically treated at 30-50 kHz for 30-60 min to fully dissolve the lignin.
[0013] (2) The solution was added to 1000 parts of deionized water and then ultrasonically treated at 30-50 kHz for 30-60 min to obtain a stable nanoparticle suspension.
[0014] (3) Vacuum concentration was performed in a rotary evaporator at 50-60 °C to obtain lignocellulose nanoparticles.
[0015] In some embodiments, the molecular weight of the polyvinyl alcohol is between 10,000 and 100,000.
[0016] In some embodiments, the particle size of the modified boron nitride nanoparticles is 1-10 μm.
[0017] In some of the embodiments, the particle sizes of the aluminum hydroxide, titanium dioxide and talc are all 5-15 μm.
[0018] In some of the embodiments, the high temperature drying method in the step S4 of drying and crushing the gel is specifically as follows: placing the obtained gelled fireproof material in a drying oven at 70-90°C for 20-30 hours, and then crushing it with an ultrasonic pulverizer to obtain micron-sized mixed particles.
[0019] In some embodiments, the freeze-drying method in the gel drying and crushing of step S4 is as follows: the obtained gelled fireproof material is placed in a refrigerator at -24°C for 10 to 20 hours to be fully pre-frozen, and then the pre-frozen block is placed in a freeze dryer for 24 to 48 hours, and the drying temperature of the freeze dryer is -30 to -10°C. After drying, an ultrasonic crusher is used to crush the mixed particles to obtain micron-sized particles.
[0020] In some of the embodiments, the high gloss additive is one of polyurethane, siloxane, acrylic, and nano zinc oxide high gloss additives.
[0021] The present invention also provides a method for imitating porcelain of water-based fire retardant coating, the method comprising the following steps: S6. Surface treatment: Clean the substrate surface: Use detergent and deionized water to thoroughly clean the surface of the construction substrate to ensure that there is no dust, oil or loose matter on the surface.
[0022] S7. Primer coating: Select appropriate primer according to the type of substrate, ensure good compatibility between the primer and water-based fire retardant coating, and improve the adhesion and surface smoothness of the coating.
[0023] S8. Intermediate coating: Apply water-based fire retardant paint evenly on the surface of the primer and polish it smooth after drying.
[0024] S9. Topcoat: Apply water-based fire retardant paint again, polish the surface after drying, and apply and polish 2 to 5 times as needed until a smooth porcelain-like effect is achieved.
[0025] S10. Maintenance: After construction, the coating needs to be maintained for more than 7 days to ensure the stability of its fireproof performance and porcelain-like effect.
[0026] (1) The present invention improves the construction process of water-based fire retardant coating, thereby improving its color aesthetics.
[0027] (2) The present invention innovates the formula and preparation process of water-based fire retardant coatings. By adding polyvinyl alcohol, xanthan gum, and lignin nanoparticles thereto and performing gelation treatment with sodium tetraborate and sodium hydroxide, the fire retardant performance and environmental safety of the coatings are improved. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the technical implementation method of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in combination with the technical process steps, specific implementation conditions and materials in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0029] Synthesis of lignin nanoparticles (1) 10 parts of air-dried lignin powder extracted from giant reed were added to 100 parts of 70% acetone and then ultrasonically treated at 30 kHz for 60 min to fully dissolve the lignin.
[0030] (2) The solution was added into 1000 parts of deionized water and then ultrasonicated at 30 kHz for 60 min to obtain a stable nanoparticle suspension.
[0031] (3) After vacuum concentration in a rotary evaporator at 50 °C, lignocellulose nanoparticles were obtained. Example
[0032] Synthesis of lignin nanoparticles (1) 15 parts of air-dried lignin powder extracted from giant reed was added to 100 parts of 70% acetone and then ultrasonically treated at 40 kHz for 50 min to fully dissolve the lignin.
[0033] (2) The solution was added into 1000 parts of deionized water and then ultrasonicated at 40 kHz for 50 min to obtain a stable nanoparticle suspension.
[0034] (3) After vacuum concentration in a rotary evaporator at 55 °C, lignocellulose nanoparticles were obtained. Example
[0035] Synthesis of lignin nanoparticles (1) 20 parts of air-dried lignin powder extracted from giant reed was added to 100 parts of 70% acetone and then ultrasonically treated at 50 kHz for 40 min to fully dissolve the lignin.
[0036] (2) The solution was added into 1000 parts of deionized water and then ultrasonicated at 50 kHz for 40 min to obtain a stable nanoparticle suspension.
[0037] (3) After vacuum concentration in a rotary evaporator at 60 °C, lignocellulose nanoparticles were obtained. Example
[0038] Preparation of water-based fire retardant coating (1) Mixing of water-based fire retardant coating: 100 parts of deionized water, 30 parts of polyvinyl alcohol, 3 parts of xanthan gum, 5 parts of lignin nanoparticles obtained in Example 1, 7 parts of modified boron nitride nanoparticles with a particle size of 1 μm, 5 parts each of aluminum hydroxide with a particle size of 5 μm, titanium dioxide and talc, 3 parts of polyurethane high gloss additives and 1 part of pigment are uniformly mixed in the required proportions at a temperature of 50°C and a rotation speed of 1000 r / min for 20 h to obtain a mixed suspension.
[0039] (2) Alkaline gelation of water-based fire retardant coating: Add 3 parts of sodium hydroxide and 7 parts of sodium tetraborate to the mixed suspension obtained in step (1), and stir at 50°C for 30 minutes to obtain a gelled fire retardant material.
[0040] (3) Gel drying and crushing: The gelled fireproof material obtained in step (2) is fully dried by high-temperature drying at 70°C for 30 h, and then crushed to obtain micron-sized mixed particles.
[0041] (4) Redissolving the particles: The mixed particles obtained in step (3) were mixed with deionized water in a ratio of 1:5 at 50°C using a mechanical stirrer at a stirring speed of 1000 r / min, and then placed in a vacuum box at 1 Pa for degassing to obtain a water-based fire retardant coating. Example
[0042] Preparation of water-based fire retardant coating (1) Mixing of water-based fire retardant coating: 100 parts of deionized water, 20 parts of polyvinyl alcohol, 4 parts of xanthan gum, 6 parts of lignin nanoparticles obtained in Example 2, 6 parts of modified boron nitride nanoparticles with a particle size of 2 μm, 6 parts of aluminum hydroxide with a particle size of 6 μm, 6 parts of titanium dioxide and talc, 4 parts of siloxane high gloss additives and 2 parts of pigments were uniformly mixed in the required proportions at a temperature of 60 °C and a rotation speed of 2000 r / min for 15 h to obtain a mixed suspension.
[0043] (2) Alkaline gelation of water-based fire retardant coating: Add 4 parts of sodium hydroxide and 6 parts of sodium tetraborate to the mixed suspension obtained in step (1), and stir at 60°C for 20 minutes to obtain a gelled fire retardant material.
[0044] (3) Gel drying and crushing: The gelled fireproof material obtained in step (2) is fully dried by high-temperature drying at 80°C for 20 h, and then crushed to obtain micron-sized mixed particles.
[0045] (4) Redissolving the particles: The mixed particles obtained in step (3) are mixed with deionized water in a ratio of 1:5 at 60°C using a mechanical stirrer at a stirring speed of 2000 r / min, and then placed in a vacuum box at 2 Pa for degassing to obtain a water-based fire retardant coating. Example
[0046] Preparation of water-based fire retardant coating (1) Mixing of water-based fire retardant coating: 100 parts of deionized water, 10 parts of polyvinyl alcohol, 6 parts of xanthan gum, 8 parts of lignin nanoparticles obtained in Example 3, 4 parts of modified boron nitride nanoparticles with a particle size of 5 μm, 9 parts each of aluminum hydroxide, titanium dioxide and talc with a particle size of 13 μm, 4 parts of nano zinc oxide high gloss additives and 3 parts of pigments were uniformly mixed in the required proportions at a temperature of 70°C and a rotation speed of 3000 r / min for 10 h to obtain a mixed suspension.
[0047] (2) Alkaline gelation of water-based fire retardant coating: Add 6 parts of sodium hydroxide and 3 parts of sodium tetraborate to the mixed suspension obtained in step (1), and stir at 70°C for 10 minutes to obtain a gelled fire retardant material.
[0048] (3) Gel drying and crushing: The gelled fireproof material obtained in step (2) is placed in a refrigerator at -24°C for 10 h to fully pre-freeze, and then the pre-frozen block is placed in a freeze dryer for 48 h. The drying temperature of the freeze dryer is -10°C. After drying, an ultrasonic crusher is used to crush the mixed particles into micron-sized particles.
[0049] (4) Redissolving the particles: The mixed particles obtained in step (3) were mixed with deionized water in a ratio of 1:5 at 70°C using a mechanical stirrer at a stirring speed of 3000 r / min, and then placed in a vacuum box at 1 Pa for degassing to obtain a water-based fire retardant coating. Example
[0050] Water-based fire retardant coating construction process: (1) Surface treatment: Clean the substrate surface: Use detergent and deionized water to thoroughly clean the surface of the construction substrate to ensure that there is no dust, oil or loose matter on the surface.
[0051] (2) Primer coating: Select a suitable primer according to the type of substrate to ensure good compatibility between the primer and the water-based fire retardant coating and improve the adhesion and surface smoothness of the coating.
[0052] (3) Intermediate coating: The water-based fire retardant coating obtained in Example 4 is evenly applied to the surface of the primer and polished to make it smooth after drying.
[0053] (4) Topcoat application: Apply the water-based fire retardant coating obtained in Example 4 again, polish the surface after drying, and apply and polish multiple times as needed until a smooth porcelain-like effect is obtained.
[0054] (5) Maintenance: After construction is completed, the coating needs to be maintained for more than 7 days to ensure the stability of its fireproof properties and porcelain-like effect.
[0055] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.
Claims
1. A water-based fire retardant coating, characterized in that: The water-based fire retardant coating comprises the following raw materials by weight: 100 parts of deionized water, 10-30 parts of polyvinyl alcohol, 3-5 parts of xanthan gum, 5-10 parts of lignin nanoparticles, 3-7 parts of modified boron nitride nanoparticles, 5-10 parts of aluminum hydroxide, 5-10 parts of titanium dioxide, 5-10 parts of talc, 3-7 parts of sodium tetraborate, 3-7 parts of sodium hydroxide, 3-5 parts of high gloss additives, and 1-3 parts of pigments; the preparation method of the water-based fire retardant coating comprises the following steps: S1. Synthesis of lignin nanoparticles: The desired lignin powder was extracted from giant reed plants, and then lignin nanoparticles were synthesized by nanoprecipitation method. S2. Mixing of water-based fire retardant coating: deionized water, polyvinyl alcohol, xanthan gum, lignin nanoparticles, modified boron nitride nanoparticles, aluminum hydroxide, titanium dioxide, talcum powder, high gloss additives and pigments are uniformly mixed in a desired proportion at a temperature of 50-70°C and a rotation speed of 1000-3000 r / min for 10-20 h to obtain a mixed suspension. S3 alkaline gelation of water-based fire retardant coating: adding the desired proportion of sodium hydroxide and sodium tetraborate to the mixed suspension obtained in step S2, stirring at a temperature of 50 to 60 ° C for 10 to 30 minutes to obtain a gelled fire retardant material, S4 gel drying and crushing: The gelled fireproof material obtained in step S3 is fully dried by high temperature drying or freeze-drying, and then crushed to obtain micron-sized mixed particles, S5. Redissolving the particles: The mixed particles obtained in step S4 are mixed with deionized water in a ratio of 1:5 at a temperature of 50-70°C using a mechanical stirrer at a stirring speed of 1000-3000 r / min, and then placed in a vacuum box at 1-5 Pa for degassing to obtain a water-based fire retardant coating.
2. A water-based fire retardant coating as claimed in claim 1, characterized in that: The specific steps of synthesizing lignin nanoparticles by nanoprecipitation method in step S1 are as follows: (1) 10-20 parts of air-dried lignin powder extracted from giant reed were added to 100 parts of 70% acetone, and then ultrasonically treated at 30-50 kHz for 30-60 min to fully dissolve the lignin. (2) The solution was added to 1000 parts of deionized water, and then ultrasonicated at 30-50 kHz for 30-60 min to obtain a stable nanoparticle suspension. (3) Vacuum concentration was performed in a rotary evaporator at 50-60 °C to obtain lignocellulose nanoparticles.
3. A water-based fire retardant coating according to claim 1, characterized in that: The molecular weight of the polyvinyl alcohol is between 10,000 and 100,000.
4. A water-based fire retardant coating according to claim 1, characterized in that: The particle size of the modified boron nitride nanoparticles is 1-10 μm.
5. A water-based fire retardant coating according to claim 1, characterized in that: The particle sizes of the aluminum hydroxide, titanium dioxide 5 and talcum powder are all 5-15 μm.
6. A water-based fire retardant coating according to claim 1, characterized in that: The specific steps of the high temperature drying method in the gel drying and crushing step S4 are: placing the obtained gelled fireproof material in a drying oven at 70-90°C for 20-30 hours, and then crushing it with an ultrasonic crusher to obtain micron-sized mixed particles.
7. A water-based fire retardant coating according to claim 1, characterized in that: The specific steps of the freeze drying method in the gel drying and crushing step S4 are as follows: the obtained gelled fireproof material is placed in a refrigerator at -24°C for 10 to 20 hours to be fully pre-frozen, and then the pre-frozen block is placed in a freeze dryer for drying for 24 to 48 hours, and the drying temperature of the freeze dryer is -30 to -10°C. After drying, an ultrasonic crusher is used to crush the mixed particles into micron-sized particles.
8. A water-based fire retardant coating as claimed in claim 1, characterized in that: The high gloss additive is one of polyurethane, siloxane, acrylic, and nano zinc oxide high gloss additives.
9. A method for imitating porcelain of a water-based fire retardant coating as claimed in any one of claims 1 to 8, characterized in that: The imitation porcelain method comprises the following steps: S6. Surface treatment: Clean the substrate surface: Use detergent and deionized water to thoroughly clean the surface of the construction substrate to ensure that there is no dust, oil or loose substances on the surface. S7. Primer coating: Select the appropriate primer according to the type of substrate, ensure good compatibility between the primer and the water-based fire retardant coating, improve the adhesion and surface smoothness of the coating, S8. Intermediate coating: Apply water-based fire retardant coating evenly on the surface of primer, and polish it smooth after drying. S9. Topcoat: Apply water-based fire retardant paint again, polish the surface after drying, and apply and polish 2 to 5 times as needed until a smooth porcelain-like effect is achieved. S10. Maintenance: After construction, the coating needs to be maintained for more than 7 days to ensure the stability of its fireproof performance and porcelain-like effect.