Liquid-phase-like functional carbamate antifouling coating as well as preparation method and application thereof

By introducing monohydroxy-terminated polydimethylsiloxane flexible chains into the antifouling coating, forming a liquid-phase-like functional urethane antifouling coating, the depletion of existing coating lubricants and the marine environment is solved. The potentially dangerous problem of the problem is to achieve anti-fouling coating without lubricant release, with good biofouling and ice resistance.

CN119410251AActive Publication Date: 2025-02-11HARBIN ENG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411400509.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2025-02-11
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

When existing antifouling coatings suffer from large-area damage, the lubricant in the coating will be exhausted and lose its antifouling performance. At the same time, the lubricant is highly stable and has potential dangers to the marine environment.

Method used

Using the preparation method of liquid-phase-like functional urethane antifouling coating, by combining monohydroxy-terminated polydimethylsiloxane with hexamethylene diisocyanate trimers, it forms a flexible chain structure, which can be at room temperature. It cures under the condition, inhibits the adhesion of biological fouling and has ice resistance.

Benefits of technology

The anti-fouling coating without lubricant release is realized, which can cure at room temperature, be stable for a long time, inhibit the adhesion of biological fouling, and has good ice resistance and is friendly to the marine environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005075145250000031
    Figure BDA0005075145250000031
  • Figure BDA0005075145250000041
    Figure BDA0005075145250000041
  • Figure BDA0005075145250000051
    Figure BDA0005075145250000051
Patent Text Reader

Abstract

The invention discloses a liquid-phase-like functional carbamate antifouling coating as well as a preparation method and application thereof, and the preparation method comprises the following steps: S1, mixing monohydroxyl-terminated polydimethylsiloxane and polypropylene glycol, and removing water to obtain a solution A; s2, dissolving a hexamethylene diisocyanate tripolymer in xylene to obtain a solution B; slowly dropwise adding the solution B into the solution A, and continuously stirring in the dropwise adding process; s3, after dropwise adding is completed, heating the reaction to 80-85 DEG C, and continuously stirring to ensure that the reaction is sufficient, so as to finally obtain a prepolymer C; s4, adding a curing agent polyaspartic ester, a flatting agent and a defoaming agent into the solution C, and stirring to obtain a solution D; and S5, coating the D on the surface of a base material, and curing at room temperature for 2 hours to obtain the liquid-phase-like functional carbamate antifouling coating. The antifouling coating provided by the invention can be cured at normal temperature, is environment-friendly, inhibits adhesion of fouling organisms, and also has good ice resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of marine antifouling coatings, and in particular to a liquid-phase functional urethane antifouling coating and a preparation method and application thereof. Background Art

[0002] Marine biofouling is a well-known problem. In the shortest possible time, the hulls of ships and other artificial underwater surfaces are inevitably occupied by various marine organisms. Marine biofouling has caused serious economic and environmental problems. It is crucial to effectively control biofouling. Currently, antifouling coatings are an effective means to inhibit biofouling. Among antifouling coatings, smooth liquid injection surfaces are a very typical antifouling coating, but the lubricant in the coating is easily exhausted; when a large area is damaged, the coating will lose a large amount of lubricant and lose its performance; although the lubricant in the coating is harmless, its strong stability poses a certain potential danger to the marine environment. Therefore, it is necessary to develop an antifouling coating preparation technology that does not release lubricants but has a lubricant-like surface, which can be coated on the surface of underwater equipment such as ships, water work platforms, underwater vehicles, etc., to inhibit biofouling.

[0003] For lubricant-free release coatings, Zuo Biao et al. proposed a method for preparing ultra-high grafting density polymer molecular brushes in Chinese patent CN109400827A, "A method for preparing ultra-high grafting density polymer molecular brushes". This method first prepares SiO 2 / Si substrate, and then on SiO 2 / Si substrate surface self-assembled initiator monolayer, and finally the polymer brush was cured at 100℃ for 3 hours. It cannot be cured at room temperature, and the substrate used is SiO 2 / S i sheet, which limits its application on other substrates. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a liquid-phase functional carbamate antifouling coating and a preparation method and application thereof. The liquid-phase functional carbamate antifouling coating can be cured at room temperature, is environmentally friendly, can inhibit the adhesion of fouling organisms, and has good anti-icing performance.

[0005] The technical solutions adopted are:

[0006] The present invention provides a method for preparing a liquid-phase functional urethane antifouling coating, which comprises the following steps:

[0007] S1. The monohydroxy-terminated polydimethylsiloxane and polypropylene glycol are mixed and dehydrated to obtain a solution A;

[0008] S2. dissolving hexamethylene diisocyanate trimer in xylene to obtain solution B; slowly adding solution B dropwise to solution A while stirring continuously during the addition process;

[0009] S3. After the addition is completed, the reaction is heated to 80-85°C and stirred continuously to ensure sufficient reaction, and finally a prepolymer C is obtained;

[0010] S4. Add a curing agent, polyaspartic acid ester, a leveling agent, and a defoaming agent to C, and stir to obtain a solution D;

[0011] S5. Apply D to the surface of the substrate and cure it at room temperature for 2 hours to obtain a liquid-like functional urethane antifouling coating.

[0012] Furthermore, in S1, the molar ratio of the monohydroxy-terminated polydimethylsiloxane, the polypropylene glycol and the hexamethylene diisocyanate trimer in S2 is 0.1-0.5:0.25:1.

[0013] Further, in S1, water is removed at 100-110° C. for 2-3 hours.

[0014] Furthermore, in S2, the total amount of xylene is 30%-50% of the total mass of the monohydroxy-terminated polydimethylsiloxane in S1 and the hexamethylene diisocyanate trimer in S2.

[0015] Furthermore, in S2, the dropping speed is 50-150 g / h, and the dropping lasts for 30-40 minutes.

[0016] Further, stirring was continued for 3-4 hours to ensure sufficient reaction.

[0017] Furthermore, in S4, the mass of the defoamer and the leveling agent is 0.1% of the total mass of the S3 prepolymer and the S4 polyaspartic acid ester, respectively.

[0018] Further, in S4, stirring is performed at 2000-2500 rpm for 5-10 minutes to obtain solution D.

[0019] In the present invention, the leveling agent and the defoaming agent can be selected from commercially available leveling agents and defoaming agents, including but not limited to, for example, the leveling agent is selected from one of the commercially available German BYK BYK-306, BYK-307, BYK-330, and the defoaming agent is selected from one of the commercially available German BYK BY066N, BYK-141, BYK-071, BYK-060N.

[0020] The liquid-phase functional urethane antifouling coating of the present invention is prepared by the above-mentioned preparation method.

[0021] The liquid-phase functional urethane antifouling coating prepared by the preparation method is used in the surface protection of underwater equipment including ships, water work platforms, underwater vehicles, etc. That is, the prepared antifouling coating can be coated on the surface of underwater equipment such as ships, water work platforms, underwater vehicles, etc., to inhibit biofouling.

[0022] In the above technical solution,

[0023] The present invention is to chemically graft flexible monohydroxyl-terminated polydimethylsiloxane to an antifouling coating of carbamate. The grafted monohydroxyl-terminated polydimethylsiloxane flexible chain has a liquid-like smoothness, and the flexible chain grafted on the surface has a very high migration rate. The rapid disturbance of the flexible chain can inhibit the adhesion of biological fouling, thereby improving the antifouling performance of the coating; and the glass transition temperature of the polydimethylsiloxane flexible chain is -127°C, which allows a large number of repeated Si-O bonds to remain in a flexible state in a low-temperature environment. The flexible chain segment can interfere with the formation of ice nuclei through rapid disturbance, playing an anti-icing role, and the coating is environmentally friendly.

[0024] Wherein: the structural formula of monohydroxy-terminated polydimethylsiloxane is as follows:

[0025]

[0026] Where n is the degree of polymerization, usually 10-1000, and R is methyl or ethyl.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The present invention introduces the environmentally friendly and low-cost monohydroxy-terminated polydimethylsiloxane flexible chain into the field of urethane antifouling coatings, and has certain application prospects.

[0029] 2. The monohydroxy-terminated polydimethylsiloxane flexible chain is used to achieve low surface energy and smoothness, thereby inhibiting the adhesion of fouling organisms. Controlling the content of monohydroxy-terminated polydimethylsiloxane and hexamethylene diisocyanate trimer can control the antifouling properties of the resin.

[0030] 3. The disturbance behavior of the flexible chain of monohydroxy-terminated polydimethylsiloxane is used to inhibit the formation of ice nuclei. Controlling the content of monohydroxy-terminated polydimethylsiloxane can control the anti-icing performance of the resin.

[0031] 4. The polymer resin (solution D) has good compatibility with the solvent and can be stored for a long time without deterioration or solidification, which is convenient for subsequent application of marine antifouling coatings or compounding into marine antifouling coatings.

[0032] 5. The polymer resin (Solution D) can be cured at room temperature in two hours. DETAILED DESCRIPTION

[0033] The present invention is described in detail below through specific examples, but the use and purpose of these exemplary implementation modes are only used to illustrate the present invention, and do not constitute any form of limitation on the actual protection scope of the present invention, nor limit the protection scope of the present invention to them.

[0034] Example 1

[0035] A liquid-phase functional urethane antifouling coating of this embodiment is prepared by the following steps:

[0036] (1) 14.2 g of monohydroxy-terminated polydimethylsiloxane and 25 g of PPG (i.e., polypropylene glycol) were added to a three-necked flask and

[0037] Remove water by vacuum at 110°C for 2 hours.

[0038] (2) 60 g of hexamethylene diisocyanate trimer was dissolved in 40 g of xylene, and the solution was slowly added dropwise to a three-necked flask at room temperature for 30 minutes with continuous stirring at a speed of 400 rpm.

[0039] (3) After the addition is completed, the reaction is heated to 80-85°C and stirred for 3 hours to ensure sufficient reaction, and finally a prepolymer is obtained for the subsequent synthesis of antifouling coatings.

[0040] (4) Take 20 g of prepolymer, add 12.8 g of curing agent polyaspartic acid ester, 0.033 g of leveling agent, and 0.033 g of defoaming agent, and stir at 2000 rpm for 5 minutes.

[0041] (5) The resin was applied to the surface of the substrate and cured at room temperature for 2 hours to finally obtain a liquid-phase functional urethane antifouling coating, which was named PPNP-10.

[0042] Do the following experiment:

[0043] 1. Laboratory static inhibition and desorption of diatoms: The sample of Example 1 was evenly spread on a glass sheet with a size of 2.5 cm × 3.5 cm, and a blank glass sheet was selected as a blank control. The sample sheet and the blank glass sheet were immersed in two model algae species (Dinocampus glomerulosa and Nitzschia closterii) for 1 day, 3 days and 5 days respectively. After taking out the samples, the unattached algae were removed, and the algae attachment on the coating was photographed under an optical microscope. Five areas of each coating were randomly selected for photography, and the average number of diatom cells on the blank glass sheet and the sample of Example 1 was calculated by the following formulas (1) and (2):

[0044]

[0045]

[0046] Among them, K is the inhibition rate of diatom attachment, R is the inhibition rate of diatom desorption, NB is the average number of diatom cells on the surface of blank glass slides, N1 is the average number of diatom cells on the surface of samples, and N2 is the average number of diatom cells on the surface of samples after rinsing.

[0047] 2. Anti-icing experiment: The sample of Example 1 was evenly spread on a glass sheet with a size of 2.5 cm×3.5 cm. A blank glass sheet was selected as a blank control. The experiment was conducted using a video optical contact angle meter. The experimental temperature was -20°C. 5 μL of aqueous solution was dropped onto the coating surface to observe the solidification time of the droplet. The solidification time of water on the glass sheet was 12 s.

[0048] The inhibition rate and desorption rate of the 5-day D. diffusa were calculated to be 39.14% and 32.71% respectively, and the delayed freezing time was 40s.

[0049] Example 2

[0050] A liquid-phase functional urethane antifouling coating of this embodiment is prepared by the following steps:

[0051] (1) 28.4 g of monohydroxy-terminated polydimethylsiloxane and 25 g of PPG were added to a three-necked flask and vacuum-dried at 110° C. for 2 hours.

[0052] (2) 60 g of hexamethylene diisocyanate trimer was dissolved in 45 g of xylene, and the solution was slowly added dropwise to a three-necked flask at room temperature for 30 minutes with continuous stirring at a speed of 400 rpm.

[0053] (3) After the addition is completed, the reaction is heated to 80-85°C and stirred for 3 hours to ensure sufficient reaction, and finally a prepolymer is obtained for the subsequent synthesis of antifouling coatings.

[0054] (4) Take 20 g of prepolymer, add 10.69 g of curing agent polyaspartic acid ester, 0.03 g of leveling agent, and 0.03 g of defoaming agent, and stir at 2000 rpm for 5 minutes.

[0055] (5) The resin was applied to the surface of the substrate and cured at room temperature for 2 hours to finally obtain a liquid-phase functional urethane antifouling coating, which was named PPNP-20.

[0056] The inhibition rate and desorption rate of the 5-day D. diffusa were calculated to be 57.97% and 46.12% respectively, and the delayed freezing time was 44s.

[0057] Example 3

[0058] A liquid-phase functional urethane antifouling coating of this embodiment is prepared by the following steps:

[0059] (1) 42.6 g of monohydroxy-terminated polydimethylsiloxane and 25 g of PPG were added to a three-necked flask and vacuum-dried at 110° C. for 2 hours.

[0060] (2) 60 g of hexamethylene diisocyanate trimer was dissolved in 51 g of xylene, and the solution was slowly added dropwise to a three-necked flask at room temperature for 30 minutes with continuous stirring at a speed of 400 rpm.

[0061] (3) After the addition is completed, the reaction is heated to 80-85°C and stirred for 3 hours to ensure sufficient reaction, and finally a prepolymer is obtained for the subsequent synthesis of antifouling coatings.

[0062] (4) Take 20 g of prepolymer, add 9.05 g of curing agent polyaspartic acid ester, 0.029 g of leveling agent, and 0.029 g of defoaming agent, and stir at 2000 rpm for 5 minutes.

[0063] (5) The resin was applied to the surface of the substrate and cured at room temperature for 2 hours to finally obtain a liquid-phase functional urethane antifouling coating, which was named PPNP-30.

[0064] The inhibition rate and desorption rate of the 5-day D. diffusa were calculated to be 62.75% and 63.73% respectively, and the delayed freezing time was 86s.

[0065] Example 4

[0066] A liquid-phase functional urethane antifouling coating of this embodiment is prepared by the following steps:

[0067] (1) 56.8 g of monohydroxy-terminated polydimethylsiloxane and 25 g of PPG were added to a three-necked flask and vacuum-dried at 110° C. for 2 hours.

[0068] (2) 60 g of hexamethylene diisocyanate trimer was dissolved in 56.72 g of xylene, and the solution was slowly added dropwise to a three-necked flask at room temperature for 30 minutes with continuous stirring at a speed of 400 rpm.

[0069] (3) After the addition is completed, the reaction is heated to 80-85°C and stirred for 3 hours to ensure sufficient reaction, and finally a prepolymer is obtained for the subsequent synthesis of antifouling coatings.

[0070] (4) Take 20 g of prepolymer, add 7.73 g of curing agent polyaspartic acid ester, 0.027 g of leveling agent, and 0.027 g of defoaming agent, and stir at 2000 rpm for 5 minutes.

[0071] (5) The resin was applied to the surface of the substrate and cured at room temperature for 2 hours to finally obtain a liquid-phase functional urethane antifouling coating, which was named PPNP-40.

[0072] The inhibition rate and desorption rate of A. diffusa were calculated to be 72.39% and 73.13% respectively after 5 days, and the delayed freezing time was 100s.

[0073] Example 5

[0074] A liquid-phase functional urethane antifouling coating of this embodiment is prepared by the following steps:

[0075] (1) 71 g of monohydroxy-terminated polydimethylsiloxane and 25 g of PPG were added to a three-necked flask and vacuum-dried at 110° C. for 2 hours.

[0076] (2) 60 g of hexamethylene diisocyanate trimer was dissolved in 62 g of xylene, and the solution was slowly added dropwise to a three-necked flask at room temperature for 30 minutes with continuous stirring at a speed of 400 rpm.

[0077] (3) After the addition is completed, the reaction is heated to 80-85°C and stirred for 3 hours to ensure sufficient reaction, and finally a prepolymer is obtained for the subsequent synthesis of antifouling coatings.

[0078] (4) Take 20 g of prepolymer, add 6.65 g of curing agent polyaspartic acid ester, 0.026 g of leveling agent, and 0.026 g of defoaming agent, and stir at 2000 rpm for 5 minutes.

[0079] (5) The resin was applied to the surface of the substrate and cured at room temperature for 2 hours to finally obtain a liquid-phase functional urethane antifouling coating, which was named PPNP-50.

[0080] The inhibition rate and desorption rate of the 5-day D. diffusa were calculated to be 79.15% and 82.86% respectively, and the delayed freezing time was 207s.

[0081] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a liquid-phase functional urethane antifouling coating, characterized in that: The steps include: S1. The monohydroxy-terminated polydimethylsiloxane and polypropylene glycol are mixed and dehydrated to obtain a solution A; S2. dissolving hexamethylene diisocyanate trimer in xylene to obtain solution B; slowly adding solution B dropwise to solution A while stirring continuously during the addition process; S3. After the addition is completed, the reaction is heated to 80-85°C and stirred continuously to ensure sufficient reaction, and finally a prepolymer C is obtained; S4. Add a curing agent, polyaspartic acid ester, a leveling agent, and a defoaming agent to C, and stir to obtain a solution D; S5. Apply D to the surface of the substrate and cure it at room temperature for 2 hours to obtain a liquid-like functional urethane antifouling coating.

2. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S1, the molar ratio of monohydroxy-terminated polydimethylsiloxane, polypropylene glycol and hexamethylene diisocyanate trimer in S2 is 0.1-0.5:0.25:

1.

3. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S1, water is removed at 100-110°C for 2-3 hours.

4. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S2, the total amount of xylene is 30%-50% of the total mass of the monohydroxy-terminated polydimethylsiloxane in S1 and the hexamethylene diisocyanate trimer in S2.

5. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S2, the dropping speed is 50-150 g / h, and the dropping is continued for 30-40 minutes.

6. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: Stirring was continued for 3-4 hours to ensure complete reaction.

7. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S4, the mass of the defoamer and the leveling agent is 0.1% of the total mass of the S3 prepolymer and the S4 polyaspartic acid ester, respectively.

8. The method for preparing the liquid-phase functional urethane antifouling coating according to claim 1, characterized in that: In S4, the mixture was stirred at 2000-2500 rpm for 5-10 minutes to obtain solution D.

9. A liquid-phase functional urethane antifouling coating, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 8.

10. Use of the liquid-phase functional urethane antifouling coating prepared by the preparation method according to any one of claims 1 to 8 in the surface protection of underwater equipment including ships, water work platforms, and underwater vehicles.

Citation Information

Patent Citations

  • Preparation method of ultra-high graft density polymer molecular brush

    CN109400827A

  • Preparation and using method of organic silicon-polyurea self-stratifying coating

    CN107298930A

  • Waterborne anti-fouling polyurethane and waterborne polyurethane anti-fouling coating formed by waterborne anti-fouling polyurethane

    CN117264165A

  • Antibacterial and antifouling furniture board and manufacturing process thereof

    CN117264534A

  • N-octyl-2-hydroxybenzamide grafted polyaspartate polyurea resin as well as preparation method and application thereof

    CN117603424A