Water-based acrylate pressure-sensitive adhesive as well as formula and preparation method thereof

Optimizing the molecular structure and crosslinking structure of acrylates through suspension polymerization, the shortcomings of existing aqueous acrylate pressure-sensitive adhesives in water resistance, cohesion and heat resistance are solved, and higher bonding performance and stability are achieved. In a variety of industrial applications.

CN119490808APending Publication Date: 2025-02-21SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411641508.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-18
Publication Date
2025-02-21

AI Technical Summary

Technical Problem

Existing aqueous acrylate pressure-sensitive adhesives have poor performance in water resistance, cohesion and heat resistance, making it difficult to meet the needs of industrial applications.

Method used

Through suspension polymerization, dibutyl maleate, lauryl acrylate and furfur methacrylate are introduced, and carboxyl crosslinking of zirconium carbonate and acrylic acid are combined to improve the polymerization Strength and bonding properties.

Benefits of technology

It significantly improves the water resistance, cohesive strength and heat resistance of aqueous acrylate pressure-sensitive adhesive, enhances its adhesive properties and stability, and is suitable for a variety of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119490808A_ABST
    Figure CN119490808A_ABST
Patent Text Reader

Abstract

The invention provides a water-based acrylate pressure-sensitive adhesive and a formula and a preparation method thereof, and belongs to the field of high polymer materials, and the formula comprises an acrylate monomer mixture, a dispersing agent, an initiator, water and a cross-linking agent in specific parts by weight. The preparation method comprises the following steps: firstly preparing a mixed monomer mixed solution containing a mixed monomer and an initiator, then preparing a dispersant aqueous solution, slowly dropwise adding the mixed monomer mixed solution into a reaction kettle, keeping the temperature stable and continuously stirring in the dropwise adding process, carrying out a heat preservation reaction after dropwise adding, and finally adding a cross-linking agent and stirring to obtain the water-based acrylate pressure-sensitive adhesive. According to the treatment scheme, the waterborne acrylate pressure-sensitive adhesive is uniform in particle and stable in performance, the preparation process is environment-friendly and safe, operation is simple and easy to control, and the method is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a water-based acrylic pressure-sensitive adhesive and a formula and a preparation method thereof. Background Art

[0002] Pressure-sensitive adhesives are widely used in daily life and industrial production, such as tapes, labels, protective films, etc. Traditional solvent-based pressure-sensitive adhesives have problems such as environmental pollution and safety hazards, while water-based pressure-sensitive adhesives have the advantages of environmental protection, safety, and low cost, and have gradually become the development direction of the pressure-sensitive adhesive field. At present, the preparation method of water-based acrylic pressure-sensitive adhesives often adopts emulsion polymerization, but the pressure-sensitive adhesives obtained by emulsion polymerization have technical problems such as poor water resistance, insufficient cohesion, and poor heat resistance, which are not suitable for promotion. Summary of the invention

[0003] Therefore, in order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a water-based acrylic pressure-sensitive adhesive and its formula and preparation method, and optimizes the molecular structure and cross-linking structure of the pressure-sensitive adhesive by suspension polymerization, thereby improving the water resistance and lasting adhesion of the water-based acrylic pressure-sensitive adhesive. The preparation method has mild reaction conditions, uniform product particle size, and simple post-processing.

[0004] In order to achieve the above object, the present invention provides a formula of a water-based acrylic pressure-sensitive adhesive, comprising the following raw materials calculated by weight:

[0005] Butyl acrylate 30-40 parts;

[0006] 20-30 parts of isooctyl acrylate;

[0007] 10-20 parts of methyl methacrylate;

[0008] 10-20 parts of dibutyl maleate;

[0009] 10-20 parts of lauryl acrylate;

[0010] 10-20 parts of furfuryl methacrylate;

[0011] Acrylic acid 5-10 parts;

[0012] 1-10 parts of ammonium zirconium carbonate;

[0013] Initiator 0.5-1 part;

[0014] 1-2 parts of dispersant;

[0015] 100-150 parts of deionized water.

[0016] In one embodiment, the initiator is dibenzoyl peroxide or azobisisobutyronitrile.

[0017] In one embodiment, the dispersant is polyvinyl alcohol or hydroxypropyl methylcellulose.

[0018] A method for preparing a water-based acrylic pressure-sensitive adhesive comprises:

[0019] Step 1, butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and initiator are mixed uniformly according to the above proportions to obtain a mixed monomer mixture;

[0020] Step 2, adding 30-50 ml of a dispersant aqueous solution with a mass concentration of 5% to 15% into a reaction kettle for stirring, and then dripping the mixed monomer mixture into the reaction kettle. After the dripping is completed, heat-retaining the reaction for 60-90 minutes;

[0021] Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing stirring until the reaction is completed, and sieving to obtain a water-based acrylic pressure-sensitive adhesive.

[0022] In one embodiment, in step 2, the dispersant aqueous solution is added to the reactor for stirring, the stirring speed is controlled at 100-200 rpm, the stirring time is 20-30 min, the reaction temperature is increased to 75-90° C., stirred for 20-30 min, and the stirring speed is 300-500 rpm.

[0023] In one embodiment, the dropping speed of the mixed monomer mixture in step 2 is 2-5 drops per second, and the stirring speed is 400-500 rpm.

[0024] In one embodiment, ammonium zirconium carbonate is added in step 3 and stirring is continued for 90-120 minutes, at which time the reaction is determined to be complete.

[0025] A water-based acrylic pressure-sensitive adhesive is prepared by the above method.

[0026] Compared with the prior art, the advantages of the present invention are: dibutyl maleate, lauryl acrylate and furfuryl methacrylate are successfully introduced into the acrylic ester molecular chain structure by suspension polymerization, which effectively improves the cohesive strength of the polymer. And because its structure contains double bonds and ester groups, the double bonds can participate in the polymerization reaction, so that a tighter cross-linking structure is formed between the polymer molecular chains. This cross-linking structure helps to enhance the ability of the adhesive to resist deformation and fracture when subjected to force, thereby improving the cohesive strength.

[0027] In addition, the ester group in the dibutyl maleate molecule has a certain polarity, which enables the pressure-sensitive adhesive after polymerization to better interact with some polar surfaces and enhance the adhesion performance to polar materials, such as showing better effects when adhering to surfaces such as metal and glass; lauryl acrylate is a long-chain alkyl ester that increases the flexibility of the molecular chain, making the polymer more flexible and sticky at room temperature, which helps to improve the initial adhesion of the pressure-sensitive adhesive and the wettability to the surface of the adherend. This is very important in some application scenarios that require waterproofing or moisture-proofing, such as outdoor labels, waterproof tapes, etc., to prevent moisture from damaging the bonding properties of the adhesive.

[0028] After preparing the acrylic acid water-based pressure-sensitive adhesive by the suspension polymerization process, adding zirconium carbonate to crosslink with the carboxyl group of acrylic acid has the following effects: increasing the crosslinking density and cohesive strength, enhancing the ability of the pressure-sensitive adhesive to resist external forces, and improving the bonding stability and durability; improving water resistance, reducing the penetration and erosion of water to the pressure-sensitive adhesive, and expanding the scope of application; enhancing heat resistance, improving the bonding strength and morphological stability of the pressure-sensitive adhesive at high temperatures, and also improving the cohesive strength and adhesion of the pressure-sensitive adhesive.

[0029] The prepared water-based acrylic pressure-sensitive adhesive has the following advantages: uniform product particle size and good stability; simple post-processing without complicated solvent recovery process; the prepared pressure-sensitive adhesive has good bonding performance, low water absorption and high contact angle.

[0030] The preparation method of the water-based acrylic pressure-sensitive adhesive has a short preparation route, mild reaction, does not require pressure reaction equipment, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 It is a schematic flow chart of a method for preparing a water-based acrylic pressure-sensitive adhesive in an embodiment of the present invention. DETAILED DESCRIPTION

[0033] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0034] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0035] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0036] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0037] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0038] The present application embodiment provides a formula of a water-based acrylic pressure-sensitive adhesive, comprising the following raw materials calculated by weight:

[0039] Butyl acrylate 30-40 parts;

[0040] 20-30 parts of isooctyl acrylate;

[0041] 10-20 parts of methyl methacrylate;

[0042] 10-20 parts of dibutyl maleate;

[0043] 10-20 parts of lauryl acrylate;

[0044] 10-20 parts of furfuryl methacrylate;

[0045] Acrylic acid 5-10 parts;

[0046] 1-10 parts of ammonium zirconium carbonate;

[0047] Initiator 0.5-1 part;

[0048] 1-2 parts of dispersant;

[0049] 100-150 parts of deionized water.

[0050] Initiators, also known as free radical initiators, are a class of compounds that are easily decomposed into free radicals (i.e., primary free radicals) by heat. These compounds can be used to initiate free radical polymerization and copolymerization reactions of olefins and dienes, and can also be used for crosslinking and curing of unsaturated polyesters and crosslinking reactions of polymers. Initiators can be of the following types: 1. Organic peroxides: such as dibenzoyl peroxide, etc.; 2. Azo compounds: such as azobisisobutyronitrile; 3. Persulfates: such as potassium persulfate, ammonium persulfate, etc. In one embodiment, the initiator is dibenzoyl peroxide or azobisisobutyronitrile.

[0051] A dispersant is a surfactant having two opposite properties, lipophilicity and hydrophilicity, in a molecule. It can evenly disperse solid and liquid particles of inorganic and organic pigments that are difficult to dissolve in liquids, and can also prevent the particles from settling and agglomerating, thus forming an amphiphilic agent required for a stable suspension. In one embodiment, the dispersant is polyvinyl alcohol or hydroxypropyl methylcellulose.

[0052] A method for preparing a water-based acrylic pressure-sensitive adhesive comprises:

[0053] Step 1, butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and initiator are mixed uniformly according to the above proportions to obtain a mixed monomer mixture.

[0054] Step 2, adding 30-50 ml of a dispersant aqueous solution with a mass concentration of 5% to 15% into the reactor for stirring, and then dropping the mixed monomer mixture into the reactor. After the dropwise addition is completed, the reaction is kept warm for 60-90 minutes; wherein, in step 2, a one-time dispersant aqueous solution can be added to the reactor for stirring, or stirring can be performed in stages.

[0055] Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing stirring until the reaction is completed, and sieving to obtain a water-based acrylic pressure-sensitive adhesive.

[0056] In one embodiment, in step 2, the dispersant aqueous solution is added to the reactor for stirring, the stirring speed is controlled at 100-200 rpm, the stirring time is 20-30 min, the reaction temperature is increased to 75-90° C., the stirring is carried out for 20-30 min, and the stirring speed is 300-500 rpm. Such a setting can better control the dispersion process and make the obtained product have a good dispersion state.

[0057] In one embodiment, the dropping speed of the mixed monomer mixture in step 2 is 2-5 drops per second, and the stirring speed is 400-500 rpm.

[0058] In one embodiment, ammonium zirconium carbonate is added in step 3 and stirring is continued for 90-120 minutes, at which time the reaction is determined to be complete.

[0059] A water-based acrylic pressure-sensitive adhesive, characterized in that the water-based acrylic pressure-sensitive adhesive is prepared by the above method.

[0060] The above method successfully introduces dibutyl maleate, lauryl acrylate, and furfuryl methacrylate into the acrylic ester molecular chain structure through suspension polymerization, effectively improving the cohesive strength of the polymer. And because its structure contains double bonds and ester groups, the double bonds can participate in the polymerization reaction, so that a tighter cross-linking structure is formed between the polymer molecular chains. This cross-linking structure helps to enhance the ability of the adhesive to resist deformation and fracture when subjected to force, thereby improving the cohesive strength.

[0061] In addition, the ester group in the dibutyl maleate molecule has a certain polarity, which enables the pressure-sensitive adhesive after polymerization to better interact with some polar surfaces and enhance the adhesion performance to polar materials, such as showing better effects when adhering to surfaces such as metal and glass; lauryl acrylate is a long-chain alkyl ester that increases the flexibility of the molecular chain, making the polymer more flexible and sticky at room temperature, which helps to improve the initial adhesion of the pressure-sensitive adhesive and the wettability to the surface of the adherend. This is very important in some application scenarios that require waterproofing or moisture-proofing, such as outdoor labels, waterproof tapes, etc., to prevent moisture from damaging the bonding properties of the adhesive.

[0062] After preparing the acrylic acid water-based pressure-sensitive adhesive by the suspension polymerization process, adding zirconium carbonate to crosslink with the carboxyl group of acrylic acid has the following effects: increasing the crosslinking density and cohesive strength, enhancing the ability of the pressure-sensitive adhesive to resist external forces, and improving the bonding stability and durability; improving water resistance, reducing the penetration and erosion of water to the pressure-sensitive adhesive, and expanding the scope of application; enhancing heat resistance, improving the bonding strength and morphological stability of the pressure-sensitive adhesive at high temperatures, and also improving the cohesive strength and adhesion of the pressure-sensitive adhesive.

[0063] The prepared water-based acrylic pressure-sensitive adhesive has the following advantages: uniform product particle size and good stability; simple post-processing without complicated solvent recovery process; the prepared pressure-sensitive adhesive has good bonding properties, low water absorption and high contact angle, and can be widely used in packaging, labels, tapes and other fields.

[0064] The preparation method of the water-based acrylic pressure-sensitive adhesive has a short preparation route, mild reaction, does not require pressure reaction equipment, and is suitable for industrial production.

[0065] Reagents and instruments used in the examples

[0066]

[0067] The performance test of water-based acrylic pressure-sensitive adhesive is carried out according to the following test standards and methods:

[0068] 1) Determine the holding force according to GB / T4851-1998 standard "Test method for holding force of pressure-sensitive adhesive tapes";

[0069] 2) Viscosity measurement: The viscosity of the emulsion was measured using a rotational viscometer, with the following parameters: 2# rotor, 30r / min speed;

[0070] 3) Water absorption: Tested according to GB / T15330;

[0071] 4) Water contact angle test method: The water contact angle of the water-based acrylic pressure-sensitive adhesive film was tested using an SL200KS optical contact angle tester.

[0072] Example 1

[0073] A formula of a water-based acrylic pressure-sensitive adhesive, consisting of the following raw materials in parts by weight:

[0074] Butyl acrylate is 30 parts;

[0075] Isooctyl acrylate is 20 parts;

[0076] 10 parts of methyl methacrylate;

[0077] Dibutyl maleate is 10 parts;

[0078] Lauryl acrylate is 10 parts;

[0079] Furfuryl methacrylate is 10 parts;

[0080] Acrylic acid is 5 parts;

[0081] Ammonium zirconium carbonate is 1 part;

[0082] Benzoyl peroxide is 0.5 parts;

[0083] Polyvinyl alcohol 1788 is 1 part;

[0084] Deionized water is 100 parts.

[0085] The preparation method comprises the following steps:

[0086] Step 1, butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and dibenzoyl peroxide are uniformly mixed to obtain a mixed monomer mixture;

[0087] Step 2, add 30 ml of 5% polyvinyl alcohol 1788 aqueous solution into the reactor and stir, the stirring speed is controlled at 100 rpm, the stirring time is 20 min, the reaction temperature is increased to 75 ° C, stirred for 20 min, and the stirring speed is 300 rpm; the mixed monomer mixture is added dropwise into the reactor at a dropping speed of 2 drops per second and a stirring speed of 400 rpm. After the addition is completed, the reaction is kept warm for 60 min;

[0088] Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing to stir and react for 90 minutes, and after the reaction is completed, sieving with a 75-mesh sieve to obtain a water-based acrylic pressure-sensitive adhesive.

[0089] Example 2

[0090] A formula of a water-based acrylic pressure-sensitive adhesive, consisting of the following raw materials in parts by weight:

[0091] Butyl acrylate is 40 parts;

[0092] Isooctyl acrylate is 30 parts;

[0093] Methyl methacrylate is 20 parts;

[0094] Dibutyl maleate is 20 parts;

[0095] Lauryl acrylate is 20 parts;

[0096] Furfuryl methacrylate is 20 parts;

[0097] Acrylic acid is 10 parts;

[0098] Ammonium zirconium carbonate is 10 parts;

[0099] Benzoyl peroxide is 1 part;

[0100] Polyvinyl alcohol 1799 is 2 parts;

[0101] Deionized water is 150 parts.

[0102] The preparation method comprises the following steps:

[0103] Step 1, butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and dibenzoyl peroxide are mixed evenly to obtain a mixed monomer mixture.

[0104] Step 2, add 50 ml of 5% polyvinyl alcohol 1799 aqueous solution into the reactor and stir at a stirring speed of 200 rpm for 30 min, raise the reaction temperature to 90°C, stir for 30 min at a stirring speed of 500 rpm; then drop the mixed monomer mixture into the reactor at a dropping speed of 5 drops per second and a stirring speed of 500 rpm. After the dropping is completed, keep the reaction warm for 90 min;

[0105] Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing to stir and react for 120 minutes, and after the reaction is completed, sieving with a 75-mesh sieve to obtain a water-based acrylic pressure-sensitive adhesive.

[0106] Example 3

[0107] A formula of a water-based acrylic pressure-sensitive adhesive, consisting of the following raw materials in parts by weight:

[0108] Butyl acrylate is 35 parts;

[0109] Isooctyl acrylate is 25 parts;

[0110] 15 parts of methyl methacrylate;

[0111] Dibutyl maleate is 15 parts;

[0112] Lauryl acrylate is 15 parts;

[0113] Furfuryl methacrylate is 15 parts;

[0114] Acrylic acid is 7 parts;

[0115] Ammonium zirconium carbonate is 5 parts;

[0116] Benzoyl peroxide is 0.75 parts;

[0117] Polyvinyl alcohol 1788 is 1.5 parts;

[0118] Deionized water is 125 parts.

[0119] The preparation method comprises the following steps:

[0120] Step 1, butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and dibenzoyl peroxide are mixed evenly to obtain a mixed monomer mixture.

[0121] Step 2, add 40 ml of 5% polyvinyl alcohol 1788 aqueous solution into the reactor and stir, the stirring speed is controlled at 150 rpm, the stirring time is 25 min, the reaction temperature is increased to 85 ° C, stirred for 25 min, the stirring speed is 400 rpm, the mixed monomer mixture is weighed, and added dropwise, the dropping speed is 3 drops per second, the stirring speed is 450 rpm, and after the addition is completed, the reaction is kept warm for 80 min.

[0122] Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing to stir and react for 100 minutes, and after the reaction is completed, sieving with a 75-mesh sieve to obtain a water-based acrylic pressure-sensitive adhesive.

[0123] Comparative Example 1

[0124] The water-based acrylic pressure-sensitive adhesive is prepared by emulsion polymerization. The specific method is as follows:

[0125] (1) Add deionized water and emulsifier into a reaction kettle, stir evenly, and heat to 75°C;

[0126] (2) uniformly mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and an initiator to obtain a mixed monomer;

[0127] (3) slowly adding the mixed monomers to the reaction kettle dropwise for 2.5 hours. After the addition is complete, the reaction is continued at the temperature for 2.5 hours;

[0128] (4) After the reaction is completed, the mixture is cooled to room temperature, and aqueous ammonia is added to adjust the pH value to 7-8 to obtain a water-based acrylic pressure-sensitive adhesive.

[0129] Comparative Example 2

[0130] The water-based acrylic pressure-sensitive adhesive is prepared by emulsion polymerization. The specific method is as follows:

[0131] (1) Add deionized water and emulsifier into a reaction kettle, stir evenly, and heat to 75°C;

[0132] (2) uniformly mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and an initiator to obtain a mixed monomer;

[0133] (3) slowly adding the mixed monomers to the reaction kettle dropwise for 2.5 hours. After the addition is complete, the reaction is continued at the temperature for 2.5 hours;

[0134] (4) After the reaction is completed, the mixture is cooled to room temperature, and aqueous ammonia is added to adjust the pH value to 7-8 to obtain a water-based acrylic pressure-sensitive adhesive.

[0135] The performance of the water-based acrylic pressure-sensitive adhesive prepared in Example 1-3 and the water-based acrylic pressure-sensitive adhesive prepared in Comparative Example 1-2 was tested, and the results are shown in the following table:

[0136]

[0137] From the above results, it can be seen that the water-based acrylic pressure-sensitive adhesives prepared by suspension polymerization in Examples 1 to 3 have good bonding properties, water resistance, and a high water contact angle, which are superior to the pressure-sensitive adhesives prepared by emulsion polymerization.

[0138] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A formula of a water-based acrylic pressure-sensitive adhesive, characterized in that: The invention comprises the following raw materials calculated by weight: Butyl acrylate 30-40 parts; 20-30 parts of isooctyl acrylate; 10-20 parts of methyl methacrylate; 10-20 parts of dibutyl maleate; 10-20 parts of lauryl acrylate; 10-20 parts of furfuryl methacrylate; Acrylic acid 5-10 parts; 1-10 parts of ammonium zirconium carbonate; Initiator 0.5-1 part; 1-2 parts of dispersant; 100-150 parts of deionized water.

2. The water-based acrylic pressure-sensitive adhesive according to claim 1, characterized in that: The initiator is dibenzoyl peroxide or azobisisobutyronitrile.

3. The water-based acrylic pressure-sensitive adhesive according to claim 1, characterized in that: The dispersant is polyvinyl alcohol or hydroxypropyl methylcellulose.

4. A method for preparing a water-based acrylic pressure-sensitive adhesive, characterized in that: include: Step 1, uniformly mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, dibutyl maleate, lauryl acrylate, furfuryl methacrylate, acrylic acid and an initiator according to any proportion of claims 1 to 3 to obtain a mixed monomer solution; Step 2, adding 30-50 ml of a dispersant aqueous solution with a mass concentration of 5% to 15% into a reaction kettle for stirring, and then dripping the mixed monomer mixture into the reaction kettle. After the dripping is completed, heat-retaining the reaction for 60-90 minutes; Step 3, cooling to room temperature, adding ammonium zirconium carbonate, continuing stirring until the reaction is completed, and sieving to obtain a water-based acrylic pressure-sensitive adhesive.

5. The preparation method according to claim 4, characterized in that: In step 2, the dispersant aqueous solution is added to the reactor for stirring, the stirring speed is controlled at 100-200 rpm, the stirring time is 20-30 min, the reaction temperature is increased to 75-90° C., the stirring is carried out for 20-30 min, and the stirring speed is 300-500 rpm.

6. The preparation method according to claim 4, characterized in that: The dropping speed of the mixed monomer mixture in step 2 is 2-5 drops per second, and the stirring speed is 400-500 rpm.

7. The preparation method according to claim 4, characterized in that: In step 3, ammonium zirconium carbonate was added and stirring was continued for 90-120 min, at which time the reaction was judged to be complete.

8. A water-based acrylic pressure-sensitive adhesive, characterized in that: The water-based acrylic pressure-sensitive adhesive is prepared by the method according to any one of claims 4 to 7.