Sand-textured real stone paint coating, color matching method and application of sand-textured real stone paint coating

By introducing water-based colorful coating technology, the introduction of colorful soft and hard spots into the real stone paint formula has solved the shortcomings of real stone paint coatings in terms of weather resistance and stain resistance, and significantly improved product performance and stability.

CN119978879APending Publication Date: 2025-05-13LANGFANG NIPPON PAINT CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510189639.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-20
Publication Date
2025-05-13

AI Technical Summary

Technical Problem

The existing real stone paint coatings have shortcomings in weather resistance and stain resistance, and the large amount of natural colored sand has caused low batch stability, environmental protection problems and increased costs.

Method used

Water-based colorful paint technology is used to introduce colorful soft spots and colorful hard spots into the real stone paint formula system, and the weather resistance and stain resistance of real stone paint are improved through color adjustment methods, and the use of natural colored sand is reduced.

Benefits of technology

It significantly improves the weather resistance and stain resistance of real stone paint, improves batch stability, reduces dependence on natural colored sand, reduces production costs, and improves the color effect stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119978879A_ABST
    Figure CN119978879A_ABST
Patent Text Reader

Abstract

The invention discloses a sand textured real stone paint coating, a color matching method and application thereof, and belongs to the technical field of real stone paint coatings. The sand wall type real stone paint coating comprises real stone paint, colorful soft spots and colorful hard spots. The color matching method comprises the following steps: S1, according to a target color, pre-mixing colorful soft spots with a proper amount of real stone paint to form a soft spot coloring bag for later use; s2, putting the soft spot coloring bag and the colorful hard spots in the step S1 into the real stone paint, and mixing, so as to obtain the toning real stone paint; and S3, packaging and storing the mixed toning stone-like paint in the step S2 to prepare the sand wall-like stone-like paint coating. According to the invention, a water-based colorful paint technology is innovatively introduced into a real stone paint formula system, so that the performance of a real stone paint product is improved. Wherein the most significant performance improvement comprises weather resistance and stain resistance of the real stone paint, and the two performances are also one of key indexes which can best reflect the product level after construction of the real stone paint is completed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of real stone paint, and in particular relates to a sand-wall-shaped real stone paint, a coloring method and application thereof. Background Art

[0002] At present, the color scheme of real stone paint on the market is mainly based on colored sand / white sand as the main color, and color paste is used to correct or adjust the color. The method of using colored sand will consume a large amount of natural colored sand, and the batch stability of natural colored sand is not high, and it is a non-renewable resource. Large-scale mining is not conducive to environmental protection. Without the use of topcoat varnish, the weather resistance and stain resistance of real stone paint cannot achieve satisfactory results. In addition, the production technology of real stone paint is highly mature, and the market has entered the stage of price competition. The low-price strategy cannot bring long-term competitive advantages to real stone paint. Only by focusing on the product itself and improving performance can the bottleneck of the real stone paint market be broken.

[0003] Therefore, the market urgently needs a method to improve the performance of real stone paint to help it get rid of low-price competition and break the vicious cycle. In order to improve the batch stability of existing real stone paint, reduce the use of natural colored sand, and improve the stain resistance and weather resistance of real stone paint. Summary of the invention

[0004] The invention aims to solve the problems existing in the prior art and provide a sand-walled real stone paint, a coloring method and its application. The present invention innovatively introduces water-based multi-color paint technology into the real stone paint formula system, thereby improving the performance of the real stone paint product. Among them, the most significant performance improvement includes the weather resistance and stain resistance of the real stone paint, which are also one of the key indicators that best reflect the product level after the real stone paint is completed.

[0005] The coloring method of the sand-walled real stone paint of the present invention has a simple process and is easy to operate, and effectively improves the shortcomings of existing real stone paint products in terms of weather resistance and stain resistance, as well as the batch stability problem caused by the large-scale use of natural colored sand. In addition, the coloring method has a wide range of applications, which can meet the small-scale coloring needs of retail stores and is also suitable for large-scale production in factories.

[0006] The first invention object of the present invention is:

[0007] A method for coloring a sand-walled real stone paint is provided, wherein the sand-walled real stone paint comprises the following raw material components in parts by weight:

[0008] Real stone paint 800-900 parts, colorful soft paint 100-200 parts, colorful hard paint 0-100 parts;

[0009] The colorful soft spots are prepared according to the composition and preparation method of wet colored sand in the patent application publication CN116515354A, a lightweight real stone paint and its preparation method;

[0010] The multi-colored hard spots are prepared according to the patent application publication CN117624984A, a water-based reactive type scrapable water-coated sand-coated multi-colored paint and its preparation, construction method and composition and preparation method of the multi-colored paint particles in its application;

[0011] This technical solution divides the colored dots into colorful soft dots and colorful hard dots according to their functions. Colorful soft dots mainly provide the coloring function, which can be quickly and evenly dispersed in the real stone paint without revealing the color dot shape; colorful hard dots mainly provide the imitation of large-grained gravel effect, which can ensure that after being added to the real stone paint, a certain proportion of the colored dots will not be ground or disappear within the specified stirring and mixing time, and can provide the real stone paint with the effect of large-grained natural colored sand.

[0012] The color mixing method of the sand-walled real stone paint comprises the following steps:

[0013] S1. According to the target color, the colorful soft spots are pre-mixed with an appropriate amount of real stone paint into a soft spot coloring package for standby use;

[0014] S2. The soft point coloring package and the colorful hard point in step S1 are mixed into the remaining portion of the real stone paint to obtain a color real stone paint;

[0015] S3. The toned real stone paint mixed in step S2 is packaged and stored to prepare the sand-walled real stone paint.

[0016] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0017] It also includes step S4;

[0018] S4. Scrape and dry the sand-walled real stone paint in step S3, and compare it with the target color to determine the color difference; if there is no color difference, it is determined to be qualified.

[0019] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0020] The real stone paint comprises:

[0021] Real stone paint uses 120-280 parts of base paint, 480-780 parts of natural white sand, and 0-100 parts of natural colored sand.

[0022] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0023] The natural white sand is natural white quartz sand.

[0024] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0025] The soft spot coloring package described in step S1 is a mixture of colorful soft spots and an appropriate amount of real stone paint by a shaking mixing method or a stirring mixing method, the purpose of which is to provide a color adjustment function for the real stone paint, and is an intermediate product.

[0026] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0027] The oscillation mixing method uses an oscillation mixer (suitable for packaging with a capacity of 18L barrels or less);

[0028] It includes the following mixing steps:

[0029] A1. Put colorful soft dots and proper amount of real stone paint into the container and seal it well;

[0030] A2. Place the sealed container in a shaking mixer;

[0031] A3. Set the shaking time to 5 to 10 minutes. After the shaking is over, the mixed soft spot coloring package is obtained;

[0032] The stirring and mixing method adopts a stepless speed mixer;

[0033] It includes the following mixing steps:

[0034] B1. Put colorful soft dots and appropriate amount of real stone paint into the container;

[0035] B2. Mix with a disperser and stir with a ribbon; the mixing speed is 50 to 200 rpm and the mixing time is 10 to 20 minutes (the larger the container capacity, the higher the mixing speed and the longer the mixing time required);

[0036] B3. After the stirring and mixing is completed, the mixed soft point coloring bag is obtained.

[0037] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0038] The soft spot coloring package, the colorful hard spots and the remaining real stone paint described in step S2 are mixed by a stirring mixing method, the purpose of which is to provide the real stone paint with a coloring effect similar to that of coarse-grained colored sand.

[0039] The color mixing method of the sand-walled real stone paint coating of the present invention is further optimized as follows:

[0040] The stirring and mixing method in step S2 uses a continuously variable speed mixer or a handheld mixer;

[0041] It includes the following mixing steps:

[0042] C1. Put the soft spot coloring pack, colorful hard spots and the remaining real stone paint into the container;

[0043] C2. Mix with a continuously variable speed mixer or hand-held mixer, using a ribbon mixer; the mixing speed is 50-200 rpm, and the mixing time is 10-20 minutes (the larger the container capacity, the higher the mixing speed and the longer the mixing time required);

[0044] C3. After the stirring and mixing is completed, the mixed color-matching real stone paint is obtained.

[0045] The second object of the present invention is:

[0046] Provided is a sand-wall-like real stone paint coating, which is prepared according to the above-mentioned color mixing method of the sand-wall-like real stone paint coating.

[0047] The third invention object of the present invention is:

[0048] Provide an application of the aforementioned sand-walled real stone paint:

[0049] The sand-wall-like real stone paint is applied to the exterior wall of a building.

[0050] The sand-wall-like real stone paint is applied by spraying, such as by using a real stone paint spray gun.

[0051] The sand-walled real stone paint coating and the coloring method thereof of the present invention, its production process and production equipment can be compatible with water-based multi-color paint and traditional real stone paint, without the need for additional new equipment support. The sand-walled real stone paint coating of the present invention can be constructed by spraying, which is simple to operate and has a smooth construction process. The coloring method of the sand-walled real stone paint coating of the present invention can reduce the use of natural colored sand, improve batch stability, and significantly improve the weather resistance and stain resistance of the real stone paint. The method of the present invention is easy to produce and flexible to store, and is suitable for both retail and factory mass production. Compared with directly using color paste to color, the effect of this method is more transparent and the color is more realistic.

[0052] The invention discloses a sand-walled real stone paint, a coloring method and an application thereof, and specifically relates to the improvement of the performance of the real stone paint for building exterior walls in terms of color creation and coloring, stain resistance, surface stone imitation effect, etc. The water-based multi-color paint technology is creatively introduced into the real stone paint, thereby improving the performance of the real stone paint.

[0053] Because water-based multi-color paint uses modified cellulose and protective glue system, the stain resistance and weather resistance of the paint after film formation are better than those of real stone paint. This method adopts the method of preparing water-based multi-color paint into a semi-finished product of coloring points, and introducing water-based multi-color paint into the real stone paint formula system by the method of coloring real stone paint. Under normal circumstances, water-based multi-color paint can be toned using color paste and white sand, which can hardly use natural colored sand and can improve the stability of product effects. The water-based multi-color paint is prepared into colored color points, used as a toning raw material, and mixed with real stone paint, which can effectively replace natural colored sand and improve the batch stability of the color effect of real stone paint. In addition, after a certain proportion of colored color points are mixed, the stain resistance and weather resistance of real stone paint are significantly improved.

[0054] Water-based multi-color paint uses modified cellulose and protective glue system, and its pollution resistance and weather resistance after film formation are better than real stone paint. Usually, water-based multi-color paint can be toned by color paste and white sand, which almost does not require the use of natural colored sand and can also improve the stability of product effects.

[0055] In the technical solution of the present invention, a water-based multi-color paint is first prepared into a semi-finished color point, and then introduced into the real stone paint formula system by the method of coloring the real stone paint. First, the water-based multi-color paint is prepared into a color point, which is mixed with the real stone paint as a coloring raw material, which can effectively replace the natural colored sand; at the same time, it can also improve the batch stability of the color effect of the real stone paint. In addition, when a certain proportion of the color point is mixed, the pollution resistance and weather resistance of the real stone paint will be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a comparison diagram of the actual effects of the sand-wall-like real stone paint containing different proportions of colored points of the present invention and the traditional real stone paint. DETAILED DESCRIPTION

[0057] In order to make the application, technical scheme and advantages of the present invention more clear, the present invention is described in detail in conjunction with specific embodiments. It should be understood that the embodiments are only used to illustrate the present invention, but not to limit the protection scope of the present invention. All simple improvements to the preparation method of the present invention under the premise of the concept of the present invention belong to the protection scope of the present invention.

[0058] Example 1

[0059] A coloring method for a sand-walled real stone paint, wherein the sand-walled real stone paint comprises the following raw material components in parts by weight:

[0060] 800 parts of real stone paint, 200 parts of colorful soft spots;

[0061] The real stone paint comprises:

[0062] Real stone paint uses 280 parts of base paint and 520 parts of white sand.

[0063] The colorful soft spots are prepared according to the composition and preparation method of wet colored sand in the patent application publication CN116515354A, a lightweight real stone paint and its preparation method;

[0064] The colorful hard spots described in the following examples are prepared according to the composition and preparation method of the colorful paint particles in the patent application publication CN117624984A, which discloses a water-based reactive type scraperable water-coated sand-coated colorful paint and its preparation, construction method and application;

[0065] Other raw materials, unless otherwise specified, can be purchased commercially.

[0066] The color mixing method of the sand-walled real stone paint comprises the following steps:

[0067] S1. According to the target color, the colorful soft spots are pre-mixed with an appropriate amount of real stone paint into a soft spot coloring package for standby use;

[0068] S2. The soft point coloring package and the colorful hard point (here the colorful hard point is 0) in step S1 are put into the remaining part of the real stone paint and mixed to obtain a color-matching real stone paint;

[0069] S3. The mixed color real stone paint in step S2 is packaged and stored to prepare the sand-walled real stone paint;

[0070] S4. Scrape and dry the sand-walled real stone paint in step S3, and compare it with the target color to determine the color difference; if there is no color difference, it is determined to be qualified.

[0071] Example 2

[0072] The preparation method of Example 2 is the same as that of Example 1, the main difference being that:

[0073] The sand-walled real stone paint comprises the following raw material components in parts by weight:

[0074] 800 parts of real stone paint, 100 parts of colorful soft paint, 100 parts of colorful hard paint;

[0075] The real stone paint comprises:

[0076] Real stone paint uses 280 parts of base paint and 520 parts of white sand.

[0077] Example 3

[0078] The preparation method of Example 3 is the same as that of Example 1, the main difference being that:

[0079] 800 parts of real stone paint, 100 parts of colorful soft paint, 100 parts of colorful hard paint;

[0080] The real stone paint comprises:

[0081] Real stone paint uses 220 parts of base paint, 480 parts of white sand, and 100 parts of natural colored sand.

[0082] Comparative Example 1

[0083] The preparation method of Comparative Example 1 is basically the same as that of Example 1, the main difference being that:

[0084] 990 parts of real stone paint, 10 parts of colorful soft spots;

[0085] The real stone paint comprises:

[0086] Real stone paint uses 330 parts of base paint and 660 parts of white sand.

[0087] Comparative Example 2

[0088] The preparation method of Comparative Example 2 is basically the same as that of Example 1, the main difference being that:

[0089] 990 parts of real stone paint, 10 parts of colorful hard spots;

[0090] The real stone paint comprises:

[0091] Real stone paint uses 330 parts of base paint and 660 parts of white sand.

[0092] Comparative Example 3

[0093] The preparation method of Comparative Example 3 is basically the same as that of Example 1, with the main difference being:

[0094] It only includes:

[0095] Real stone paint uses 330 parts of base paint and 670 parts of white sand.

[0096] Performance Testing:

[0097] The products prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were sprayed on the asbestos-free fiber cement board, one coat was sprayed, and the consumption of each coat was 2 to 3 kg / m 2 The specific construction steps are as follows: Use a real stone paint spray gun to spray the same amount of color-matched real stone paint on the asbestos-free fiber cement board, and dry it after spraying.

[0098] The products prepared in the above embodiments and comparative examples were subjected to a series of performance tests, and the test results are shown in Table 1 below.

[0099] The specific test method is as follows:

[0100] The test method for the construction performance of the toned real stone paint is: at room temperature, spray the toned real stone paint evenly on the asbestos-free fiber cement board, and observe the uniformity of the paint atomization and dispersion. Observe whether there is any sand falling.

[0101] The stain resistance test method is:

[0102] Determine according to method 5.5.1.3 in GB / T9780-2013.

[0103] The test method for resistance to artificial aging is:

[0104] Determine according to method 6.5.19 in HGT4343-2024 "Water-based Multi-color Architectural Coatings".

[0105] The test method for thermal storage stability is:

[0106] The water-in-water multi-color paint was placed in a 500 mL sample can, the lid was tightened and sealed, and then placed in a constant temperature drying oven, stored at 50±2°C accelerated conditions for 4 weeks, and then cooled to room temperature and the state of the sample paint in the can was observed.

[0107] Table 1

[0108]

[0109] The results of the above three embodiments and three comparative examples show that:

[0110] The addition amount of colorful soft spots and colorful hard spots prepared based on water-based colorful coatings improves the construction sand shedding, stain resistance, artificial aging resistance, and thermal storage stability of the toned real stone paint.

[0111] When the amount of coloring dots added is sufficient, whether it is a colorful soft dot or a colorful hard dot, the above coating properties can be improved. (Examples 1 and 2)

[0112] When the amount of coloring point added is sufficient, whether white sand or natural colored sand is added to the real stone paint, the above-mentioned coating properties of the color-tuned real stone paint are not greatly affected. (Examples 1, 3)

[0113] When the amount of coloring point added is insufficient, or no coloring point is added, the above coating properties of the finished product will be reduced to a certain extent. (Comparative Examples 1, 2, 3)

[0114] To sum up, the above are only preferred embodiments of the present invention and are not intended to limit the present invention in any form. Any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the disclosed technical content are regarded as equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

[0115] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0116] The experimental methods without specific conditions in the present invention are usually carried out under conventional conditions or conditions recommended by the manufacturer.

[0117] Unless otherwise stated, the various optimization technical solutions in the present invention can be combined with each other.

[0118] Unless otherwise indicated, percentages and parts are by weight.

[0119] Experimental methods without specific conditions specified in the instructions and examples are usually carried out under conventional conditions or conditions recommended by the manufacturers.

[0120] Unless otherwise defined, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention.

Claims

1. A color matching method for a sand-walled real stone paint, characterized in that: The sand-walled real stone paint comprises the following raw material components in parts by weight: Real stone paint 800-900 parts, colorful soft paint 100-200 parts, colorful hard paint 0-100 parts; The color mixing method of the sand-walled real stone paint comprises the following steps: S1. According to the target color, the colorful soft spots are pre-mixed with an appropriate amount of real stone paint into a soft spot coloring package for standby use; S2. The soft point coloring package and the colorful hard point in step S1 are mixed into the remaining portion of the real stone paint to obtain a color real stone paint; S3. The toned real stone paint mixed in step S2 is packaged and stored to prepare the sand-walled real stone paint.

2. The color matching method of the sand-walled real stone paint according to claim 1, characterized in that: It also includes step S4; S4. Scrape and dry the sand-walled real stone paint in step S3, and compare it with the target color to determine the color difference; if there is no color difference, it is determined to be qualified.

3. The color matching method of the sand-walled real stone paint according to claim 1, characterized in that: The real stone paint comprises: Real stone paint uses 120-280 parts of base paint, 480-780 parts of natural white sand, and 0-100 parts of natural colored sand.

4. The color matching method of the sand-walled real stone paint according to claim 3, characterized in that: The natural white sand is natural white quartz sand.

5. The color matching method of the sand-walled real stone paint according to claim 1, characterized in that: The soft spot coloring package described in step S1 is prepared by mixing colorful soft spots with an appropriate amount of real stone paint by a shaking mixing method or a stirring mixing method.

6. The color matching method of the sand-walled real stone paint according to claim 5, characterized in that: The oscillation mixing method adopts an oscillation mixer; It includes the following mixing steps: A1. Put colorful soft dots and proper amount of real stone paint into the container and seal it well; A2. Place the sealed container in a shaking mixer; A3. Set the shaking time to 5 to 10 minutes. After the shaking is over, the mixed soft spot coloring package is obtained; The stirring and mixing method adopts a stepless speed mixer; It includes the following mixing steps: B1. Put colorful soft dots and appropriate amount of real stone paint into the container; B2. Mix with a disperser and stir with a ribbon; the mixing speed is 50 to 200 rpm and the mixing time is 10 to 20 minutes; B3. After the stirring and mixing is completed, the mixed soft point coloring bag is obtained.

7. The color matching method of the sand-walled real stone paint according to claim 1, characterized in that: The soft spot coloring package, the colorful hard spots and the remaining real stone paint described in step S2 are mixed by a stirring mixing method.

8. The color matching method of the sand-walled real stone paint according to claim 7, characterized in that: The stirring and mixing method adopts a stepless speed mixer or a hand-held mixer; It includes the following mixing steps: C1. Put the soft spot coloring pack, colorful hard spots and the remaining real stone paint into the container; C2. Mix with a continuously variable speed mixer or a hand-held mixer, using a ribbon mixer; the mixing speed is 50 to 200 rpm, and the mixing time is 10 to 20 minutes; C3. After the stirring and mixing is completed, the mixed color-matching real stone paint is obtained.

9. A sand-walled real stone paint, characterized in that: The method is prepared according to the color matching method of the sand-walled real stone paint according to claim 1.

10. An application of the sand-walled real stone paint according to claim 9, characterized in that: The sand-wall-like real stone paint is applied to the exterior walls of buildings.

Citation Information

Patent Citations

  • Light stone-like coating and preparation method thereof

    CN116515354A

  • Water-based reaction type sand-in-water multicolor paint capable of being scraped in batches, and preparation, construction method and application thereof

    CN117624984A