Mold and method for forming middle-section paddle core of paddle
By designing the blade mid-section paddle core forming mold and high-ratio foam core forming method, the problems of low efficiency and poor consistency of traditional paddle core manufacturing are solved, and efficient and low-cost paddle core production is achieved, and excellent temperature resistance is achieved.
Patent Information
- Application Number
- CN202510502310.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-22
- Publication Date
- 2025-07-08
AI Technical Summary
Traditional blade core processing and manufacturing efficiency is low, high cost, poor consistency, and poor temperature resistance.
A middle-section paddle core forming mold is designed, including an upper mold seat and a lower mold seat, forming a mold cavity by closing the mold, and forming it with a high-magnification foam core material, setting the molding temperature to 150℃ for 30 minutes, and avoiding secondary expansion and deformation.
The four-blade mid-section cores are efficiently formed, with good consistency and excellent temperature resistance, avoiding secondary processing and reducing production costs.
Smart Images

Figure CN120269755A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of unmanned aerial vehicles, and specifically relates to a forming mold and a forming method for the middle section paddle core of a paddle blade. Background Art
[0002] As a key component of the power composition of an unmanned aerial vehicle, the processing and manufacturing technology of the paddle core of the paddle blade plays an important role in the production quality and efficiency of the paddle blade. Traditional paddle blades generally use machining to mill foam materials to manufacture the paddle core of the paddle blade. This results in low production efficiency, high costs, poor consistency, and relatively poor temperature resistance. Therefore, it is necessary to design a new forming method for the paddle core to improve the overall production efficiency, reduce costs, improve product consistency and temperature resistance. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide a forming mold for the middle section paddle core of a paddle blade with high production efficiency and good product consistency.
[0004] To solve the above problems, the present invention provides a forming mold for the middle section paddle core of a paddle blade, comprising:
[0005] An upper mold base, on which four upper mold cavities are provided, and each of the four upper mold cavities is provided with an upper mounting hole;
[0006] A lower mold base, on which four lower mold cavities corresponding to the positions of the upper mold cavities are provided, and each of the four lower mold cavities is provided with a lower mounting hole corresponding to the position of the upper mounting hole;
[0007] Four avoidance posts, the upper end of each avoidance post is respectively fixed in one of the upper mounting holes, and the lower end is correspondingly fixed in the lower mounting hole corresponding to the position of the upper mounting hole;
[0008] Wherein, when the upper mold base and the lower mold base are correspondingly closed, the four upper mold cavities correspondingly form mold cavities with the four lower mold cavities, and the high-expansion ratio foam cores arranged on the four avoidance posts correspondingly form four middle section paddle cores of the paddle blade in the four mold cavities during the forming process.
[0009] Furthermore, the upper mold base is further provided with an upper mold base limiting groove and an upper mold base limiting boss.
[0010] Furthermore, the lower mold base is provided with a lower mold base limiting boss corresponding to the position of the upper mold base limiting groove and a lower mold base limiting groove corresponding to the position of the upper mold base limiting boss. The upper mold base limiting groove is matched with the lower mold base limiting boss for positioning, and the upper mold base limiting boss is matched with the lower mold base limiting groove for positioning, so as to prevent the upper mold base and the lower mold base from having relative displacement in the longitudinal and transverse directions.
[0011] Further, a draft angle of 10° is provided on both the upper die base limiting groove and the lower die base limiting boss; a draft angle of 10° is provided on both the upper die base limiting boss and the lower die base limiting groove.
[0012] Further, a number of demolding chamfered grooves are also provided on the upper die base.
[0013] The present invention also provides a method for forming a blade middle section blade core, including:
[0014] Step S1, material preparation: cutting four pieces of high magnification foamed core materials with avoidance holes in a certain shape and weighing them;
[0015] Step S2, mold preparation: taking out the blade middle section blade core forming mold from the mold rack, opening the mold, and cleaning the mold thoroughly;
[0016] Step S3, mold preheating: after closing the blade middle section blade core forming mold, placing it on the hot press for preheating to heat the mold surface to 55 - 60 °C, and applying a demolding agent on the mold cavity surface and other inner surfaces of the mold;
[0017] Step S4, placing the foaming material: sleeving the four weighed high magnification foamed core materials with avoidance holes on the avoidance posts so that they are in the mold cavity formed by the upper die base and the lower die base, and the edges are equidistant from the mold closing line;
[0018] Step S5, mold closing: aligning the four - corner positions, respectively making the upper die base limiting groove and the lower die base limiting boss cooperate with each other for positioning, and the upper die base limiting boss and the lower die base limiting groove cooperate with each other for positioning, and then closing the upper die base and the lower die base;
[0019] Step S6, forming: placing the middle section blade core foaming mold on the hot press, setting the forming temperature to 150 °C, and maintaining the temperature for 30 minutes, then four blade middle section blade cores can be formed;
[0020] Step S7, mold cooling: placing the middle section blade core foaming mold on the cooling table, setting the temperature of the cooling table to 20 °C, and the cooling time to 10 minutes;
[0021] Step S8, mold opening: taking out the blade middle section blade core, grinding the edges, after grinding, placing the blade middle section blade core in the finished product placement area, and cleaning the mold with an air gun to prepare for forming the next mold.
[0022] Compared with the prior art, the middle section paddle core of the paddle of the present invention is formed by mold foaming, without the need for secondary processing on the machine tool, has good consistency, can achieve four in one mold, has a high molding efficiency, and at the same time, by setting the molding temperature at 150 °C and maintaining it for 30 minutes, it is beneficial to the stable characteristics of the foamed middle section paddle core, and the formed middle section paddle core of the paddle will not undergo secondary expansion and deformation even under the sun exposure, and has excellent temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for the description of the embodiments will be briefly introduced below. Obviously, the drawings in the following description are some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.
[0024] Figure 1 Schematic diagram of the overall assembly and mold closing of the mold for the embodiment of the present invention;
[0025] Figure 2 Explosion diagram of the embodiment of the present invention;
[0026] Figure 3 Schematic diagram of the draft angle set for the embodiment of the present invention;
[0027] Figure 4 Schematic diagram of the placement of the foaming material for the embodiment of the present invention;
[0028] Figure 5 Schematic diagram of mold opening for the embodiment of the present invention.
[0029] Description of the reference numerals in the drawings:
[0030] 1. Upper mold base, 11. Upper mold base limit groove, 12. Upper mold base limit boss, 13. Upper mold cavity, 14. Upper mounting hole, 15. Demolding chute;
[0031] 2. Lower mold base, 21. Lower mold base limit boss, 22. Lower mold base limit groove, 23. Lower mold cavity, 24. Lower mounting hole;
[0032] 3. Avoidance post;
[0033] 4. High magnification foaming core material, 41. Middle section paddle core of the paddle. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0034] Next, the technical solutions in the embodiments of the present application will be clearly and completely described in conjunction with the accompanying drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in the present application without creative efforts shall fall within the protection scope of the present application.
[0035] It should be understood that when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, wholes, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components, and / or their combinations.
[0036] It should also be understood that the terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. As used in the specification of the present application and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an", and "the" are intended to include the plural forms.
[0037] It should be further understood that the term " / and / " used in the specification of the present application and the appended claims refers to any combination and all possible combinations of one or more of the related listed items, and includes these combinations.
[0038] Please refer to Figure 1 As shown, an embodiment of the present invention provides a forming die for the middle section of a blade core, including: an upper die base 1, a lower die base 2, and four avoidance posts 3. The upper die base 1 and the lower die base 2 are correspondingly closed to form a die, and the four avoidance posts 3 are located between the upper die base 1 and the lower die base 2.
[0039] Please refer to Figures 2 - 5 As shown, four upper die cavities 13 are provided on the upper die base 1, and an upper mounting hole 14 is provided in each of the four upper die cavities 13.
[0040] The upper die base 1 is further provided with an upper die base limit groove 11, an upper die base limit boss 12, and several demolding inclined grooves 15.
[0041] Four lower die cavities 23 corresponding to the positions of the upper die cavities 13 are provided on the lower die base 2, and a lower mounting hole 24 corresponding to the position of the upper mounting hole 14 is provided in each of the four lower die cavities 23.
[0042] The lower die base 2 is provided with a lower die base limit boss 21 corresponding to the position of the upper die base limit groove 11 and a lower die base limit groove 22 corresponding to the position of the upper die base limit boss 12.
[0043] Among them, the limiting groove 11 of the upper die base is matched and positioned with the limiting boss 21 of the lower die base, and the limiting boss 12 of the upper die base is matched and positioned with the limiting groove 22 of the lower die base, which can prevent the relative displacement of the upper die base 1 and the lower die base 2 in the longitudinal and transverse directions.
[0044] The limiting groove 11 of the upper die base and the limiting boss 21 of the lower die base are both provided with a draft angle of 10°; the limiting boss 12 of the upper die base and the limiting groove 22 of the lower die base are also both provided with a draft angle of 10°.
[0045] The upper end of each relief post 3 is respectively fixed in one of the upper mounting holes 14, and the lower end is correspondingly fixed in the lower mounting hole 24 corresponding to the position of this upper mounting hole 14.
[0046] Among them, when the upper die base 1 and the lower die base 2 are correspondingly closed, the four upper die cavities 13 correspondingly form die cavities with the four lower die cavities 23, and the high-expansion foam cores 4 provided on the four relief posts 3 correspondingly form four blade middle-section cores 41 in the four die cavities during the molding process.
[0047] In addition, another embodiment of the present invention also provides a method for forming a blade middle-section core, including the following steps:
[0048] Step S1, material preparation: cutting several pieces (corresponding to 4 pieces in this embodiment) of high-expansion foam cores 4 with relief holes of a certain shape and weighing them;
[0049] Step S2, mold preparation: taking out the blade middle-section core forming mold from the mold rack, opening the mold, and cleaning the mold with an air gun. If there is too much foam residue in the mold and it cannot be cleaned, it can be cleaned with a mold cleaner.
[0050] Step S3, mold preheating: closing the blade middle-section core forming mold and placing it on the hot press for preheating. The surface of the mold is heated to 55 - 60 °C, and a release agent is applied to the mold cavity surface and other inner surfaces of the mold.
[0051] Step S4, reference Figure 4 , placing the foaming material: sleeving the four weighed high-expansion foam cores 4 through the set relief holes on the relief posts 3 and placing them in the mold cavity formed by the upper die base 1 and the lower die base 2, with the edges equidistant from the mold closing line.
[0052] Step S5, closing the mold: aligning the four corners for positioning, respectively making the limiting groove 11 of the upper die base cooperate and position with the limiting boss 21 of the lower die base, and the limiting boss 12 of the upper die base cooperate and position with the limiting groove 22 of the lower die base, and closing the upper die and the lower die.
[0053] Step S6, Molding: Place the middle section paddle core foaming mold on the hot press table, set the molding temperature to 150°C, and maintain the temperature for about 30 minutes, then four paddle blade middle section cores 41 can be molded.
[0054] Among them, in this step, the molding temperature is 150°C and it is maintained for 30 minutes, which is beneficial to the stable characteristics of the foamed middle section paddle core. It will not expand and deform again under sun exposure and has excellent temperature resistance.
[0055] Step S7, Mold Cooling: Place the middle section paddle core foaming mold on the cooling table, set the temperature of the cooling table to 20°C, and the cooling time is about 10 minutes.
[0056] Step S8, Refer to Figure 5 , Mold Opening: Take out the paddle blade middle section core 41 and perform edge grinding. After grinding, place the paddle blade middle section core 41 in the finished product placement area and clean the mold with an air gun to prepare for molding the next mold.
[0057] It can be seen from the above technical solutions that through the four formed cavities, the present invention can ensure that under the same conditions of materials, molding temperature, pressure, etc., four paddle blade middle section cores can be formed at one time, which can effectively ensure the consistency of the four paddle blade middle section cores. The entire process can be formed in one pass without secondary processing on the machine table, and its molding efficiency is relatively high.
[0058] The specific embodiments of the invention have been described in detail above, but they are only examples, and the invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modification or substitution to the invention is also within the scope of the invention. Therefore, equivalent transformations, modifications, improvements, etc. made without departing from the spirit and principles of the invention should all be covered within the scope of the invention.
Claims
1. A forming die for the paddle core in the middle section of a paddle blade, characterized in that, Including: An upper die holder (1), on which four upper die cavities (13) are provided, and each of the four upper die cavities (13) is provided with an upper mounting hole (14); A lower die holder (2), on which four lower die cavities (23) corresponding to the positions of the upper die cavities (13) are provided, and each of the four lower die cavities (23) is provided with a lower mounting hole (24) corresponding to the position of the upper mounting hole (14); Four relief posts (3), the upper end of each relief post (3) is respectively fixed in one of the upper mounting holes (14), and the lower end is correspondingly fixed in the lower mounting hole (24) corresponding to the position of the upper mounting hole (14); Wherein, when the upper die holder (1) and the lower die holder (2) are correspondingly closed, the four upper die cavities (13) correspondingly form die cavities with the four lower die cavities (23), and the high-expansion foam cores (4) arranged on the four relief posts (3) correspondingly form four blade middle-section cores in the four die cavities during the molding process.
2. The paddle core forming die for the middle section of the paddle blade according to claim 1, wherein The upper die holder (1) is further provided with an upper die holder limit groove (11) and an upper die holder limit boss (12).
3. The blade middle section paddle core forming die according to claim 2, characterized in that, The lower die holder (2) is provided with a lower die holder limit boss (21) corresponding to the position of the upper die holder limit groove (11) and a lower die holder limit groove (22) corresponding to the position of the upper die holder limit boss (12). The upper die holder limit groove (11) cooperates with the lower die holder limit boss (21) for positioning, and the upper die holder limit boss (12) cooperates with the lower die holder limit groove (22) for positioning, preventing relative displacement in the longitudinal and transverse directions between the upper die holder (1) and the lower die holder (2).
4. The blade middle section core forming die according to claim 3, characterized in that Both the upper die holder limit groove (11) and the lower die holder limit boss (21) are provided with a draft angle of 10°; both the upper die holder limit boss (12) and the lower die holder limit groove (22) are provided with a draft angle of 10°.
5. The blade middle section paddle core forming die according to claim 4, characterized in that The upper die holder (1) is further provided with a plurality of demolding chamfered grooves (15).
6. A method for forming the paddle core in the middle section of a paddle blade, characterized in that, Including: Step S1, material preparation: cutting four pieces of high-expansion foam cores with relief holes of a certain shape and weighing them; Step S2, mold preparation: taking out the blade middle-section core molding mold from the mold rack, opening the mold, and cleaning the mold; Step S3, mold preheating: after closing the blade middle-section core molding mold, placing it on the hot press for preheating to heat the mold surface to 55 - 60 °C, and applying a mold release agent on the mold cavity surface and other inner surfaces of the mold; Step S4, placing the foaming material: putting the four weighed high-expansion foam cores with relief holes on the relief posts so that they are in the mold cavity formed by the upper die holder and the lower die holder, and the edges are equidistant from the mold closing line; Step S5, mold closing: aligning and positioning the four corners, respectively making the upper die holder limit groove cooperate with the lower die holder limit boss for positioning, and the upper die holder limit boss cooperate with the lower die holder limit groove for positioning, and performing the mold closing of the upper die holder and the lower die holder; Step S6, molding: placing the middle-section core foaming mold on the hot press, setting the molding temperature to 150 °C, and maintaining the temperature for 30 minutes, then four blade middle-section cores can be molded. Step S7, mold cooling: Place the middle-section paddle core foaming mold on the cooling table. The set temperature of the cooling table is 20°C, and the cooling time is 10 minutes; Step S8, mold opening: Take out the middle-section paddle core of the blade, perform edge grinding. After grinding, place the middle-section paddle core of the blade in the finished product placement area, and clean the mold with an air gun to prepare for molding the next batch.