Hot-dip plating solution for bridge cable steel wire, preparation method and use method
By increasing the aluminum content and adding rare earth elements and silicon in the hot-dip plating solution of the cable wire, the hot-dip plating process is optimized to form a uniform Zn-Al-RE-Si alloy plating layer, the problem of insufficient corrosion resistance and adhesion of the cable wire in harsh environments is solved, and high-performance coating structure and mechanical properties are achieved.
Patent Information
- Application Number
- CN202510671229.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2025-08-29
AI Technical Summary
The hot-dip coating of existing cable wires is insufficient in corrosion resistance and adhesion in harsh environments and cannot meet the requirements of harsh working conditions.
By increasing the aluminum content in the hot-dip plating solution and adding rare earth elements (RE) and silicon (Si), the Si/RE ratio should not exceed 3.0, and the hot-dip plating temperature and time are optimized to form a uniform Zn-Al-RE-Si alloy plating layer.
The corrosion resistance and adhesion of the cable wires are significantly improved, and the uniformity of the coating structure and comprehensive performance of the coating are improved. They are suitable for cable wires of different diameters, with low cost and simple process.
Smart Images

Figure CN120555931A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hot-dip plating solution for metal wire rod steel and a preparation method thereof, and in particular to a hot-dip plating solution for bridge cable steel wire, a preparation method thereof and a use method thereof. Background Art
[0002] Hot-dip coatings offer advantages such as excellent corrosion resistance, strong adhesion, low cost, and a simple process. This makes them the most widely used surface corrosion treatment for steel materials. Hot-dip coating involves first degreasing and cleaning the surface of a metal material or metal product, then performing a pre-plating treatment to enhance coating adhesion. The metal material or metal product is then immersed in a molten metal or alloy solution. After a certain period of time, the object is removed from the solution, cooled, and then treated accordingly to achieve zinc coating on the surface. The hot-dip coating microstructure is formed by the formation of an iron-zinc / alloy layer between the iron substrate and the outermost plating solution. The iron-zinc / alloy layer formed on the workpiece surface during hot-dip coating ensures a good bond between the iron and zinc / alloy layers. Therefore, the hot-dip coating microstructure can affect the corrosion resistance and mechanical properties of the component. Therefore, factors influencing the coating microstructure have a significant impact on coating quality, with the composition of the plating solution being the most direct factor affecting the coating microstructure. Pure zinc plating baths have poor corrosion resistance. Aluminum is a commonly added alloying element in hot-dip galvanizing. Its function is to reduce oxidation on the zinc pool surface, inhibit the rapid reaction between iron and zinc, increase the surface brightness of the coating, improve the electrochemical properties of the coating, enhance the corrosion resistance of the coating, and enhance the plastic processing and welding properties of the coating. Because Al and Fe have a stronger affinity than Zn and Fe, Fe2Al5 and FeAl3 alloy transition layers are preferentially formed during hot-dip Zn-Al alloy plating, preventing Fe ions from diffusing into Zn, thereby inhibiting the formation of the Fe-Zn alloy layer and preventing the alloy transition layer from participating in anodic dissolution, thereby improving the electrochemical properties.
[0003] RE has the function of reducing intergranular corrosion, purifying grain boundaries, and improving the corrosion resistance of the coating. The mechanism is that the impurity elements O and S in the zinc alloy easily precipitate at the grain boundaries of the coating, causing the grain boundaries to have a high electronegativity. Therefore, the corrosion of Zn-Al alloy coatings is generally intergranular corrosion. Rare earth easily combines with these impurity elements to form stable rare earth oxides and sulfides, which reduces the electronegativity of the grain boundaries and thus improves the coating's resistance to intergranular corrosion. Si can inhibit the growth of compounds between iron and aluminum or iron and zinc metals, thereby improving the adhesion of the coating. Si can also refine the grain size of the coating, and adding an appropriate amount can enhance corrosion resistance. Zn-Al alloy coatings have many defects such as cracks and pores, which become starting points for corrosion. The addition of Si can improve the quality of the coating, increase its uniformity, and thus enhance its corrosion resistance. The addition of Si has a significant effect on improving the corrosion resistance of Zn-Al alloy coatings. However, due to its harsh working environment, bridge cable steel wire faces severe coupling effects of corrosion and fatigue stress, and the protective effect of its surface coating is still not ideal.
[0004] After searching: Chinese patent application number CN201711012554.3 discloses a "Hot-dip Method for Zinc-Aluminum Coating of Bridge Cables." The steel wire is first zinc-coated in a zinc furnace, then zinc-aluminum alloyed in a zinc-aluminum alloy furnace. To ensure the quality of the zinc-aluminum alloy coating and control the aluminum content of the coating, a "double-dip" process is employed: the hot-dip process is split into two, with an additional hot-dip alloy furnace. During the hot-dip process, the steel wire first passes through the zinc furnace and then through the zinc-aluminum alloy furnace. Because the steel wire is already uniformly coated with a pure zinc layer containing 5%-10% aluminum, the most preferred aluminum content for this method is 6.0-6.5 wt%. While the coating structure within this range is relatively uniform, its corrosion resistance is not well adapted to the operating environment of bridge cable steel wires. Optimizing the coating structure and morphology while increasing the aluminum content can improve the corrosion resistance of the coating.
[0005] The document with Chinese patent application number CN202010035764.X discloses "A Double Dip Plating Process for Zinc-Aluminum Alloy Steel Wire Coating for New Bridge Cables", which includes the following steps: Step 1. Reeling the bridge cable onto a pay-off stand; Step 2. Supporting and guiding one end of the bridge cable on the pay-off stand through a guide pulley and placing it into a lead liquid tank for static placement; Step 3. Leading the bridge cable with a lead layer on its surface into a cooling water tank through a guide pulley, and after cooling, passing it through a pickling tank for reaction, then passing it into a clean water tank for cleaning, and finally passing it into a flux bath for reaction; Step 4. Drying the bridge cable treated in Step 3 in a drying oven; Step 5. Immersing the dried bridge cable in Step 3 into a zinc pot for galvanizing; Step 6. Leading the bridge cable into a zinc-aluminum pot for re-plating, and finally, after cooling, reeling it onto a take-up stand. This invention reduces the problem of plating leakage and achieves a thicker coating by adopting a double dip plating process. However, from the perspective of adhesion performance, the improved performance cannot meet today's requirements. An overly thick layer often leads to insufficient adhesion of the coating, which is easy to peel off and thus affects the corrosion resistance of the coating. Summary of the Invention
[0006] The present invention aims to address the deficiencies in the prior art and provide a hot-dip plating solution for bridge cable steel wire, a preparation method and a use method thereof, which are obtained by increasing the aluminum content in the hot-dip plating solution, adding RE and silicon elements, and controlling the Si / RE ratio to not exceed 3.0. In addition, in response to the existing hot-dip plating process, suitable hot-dip plating temperatures and hot-dip plating times for steel wires of different diameters are proposed to improve the microstructure of the coating, enhance adhesion, and thus enhance the corrosion resistance of the coating of the bridge cable steel wire.
[0007] Measures to achieve the above objectives: A hot-dip plating solution for bridge cable steel wires has the following chemical composition and mass percentage content: Al: 5-20%, RE: 0.05-1.0%, Si: 0.05-3.0%, and the remainder is Zn and unavoidable impurities; and satisfies: Si / RE does not exceed 3.0; the RE is Ce and La, and the two are added in a ratio of 1:1.
[0008] Preferably: Si / RE does not exceed 2.5.
[0009] Preferably, the mass percentage content of RE is 0.07-0.75%.
[0010] Preferably, the Si mass percentage content is 0.07-2.25%.
[0011] A method for preparing a hot-dip plating solution for bridge cable steel wires, comprising the following steps: 1) Preheat the zinc ingot and aluminum block to 150-200°C, and control the moisture content of the preheated zinc ingot and aluminum block to no more than 0.02%; 2) Preheat the melting furnace to no less than 400°C; 3) Place the zinc ingot in the container and heat it to melt at 450-480°C until the ingot is completely melted, stirring during the melting process. 4) Add the aluminum in three batches: 50% of the total amount in the first batch, 30% in the second batch, and the remaining 20% in the third batch. While adding the aluminum, raise the temperature to 600-620°C and continue stirring until the aluminum is completely dissolved. 5) Add RE and silicon A. When the melt temperature drops to 550-570°C after adding the aluminum block, mix the set RE and silicon and add them all at once, and control the Si / RE ratio not to exceed 3 / 3. Continue stirring during the addition process until the RE and silicon are completely dissolved; B. Add or pass impurity adsorbent into the completely dissolved RE and silicon mixture and keep warm for 10 to 30 minutes; add impurity adsorbent in an amount such that the impurities in the RE and silicon mixture are ≤0.005%; 6) Cool the hot dip bath naturally to 440-480°C and set aside.
[0012] The invention is characterized in that: the impurity adsorbent is hexachloroethane or an inert gas.
[0013] A method for using a hot-dip plating solution for bridge cable steel wires, comprising the following steps: 1) Pretreatment stage of bridge cable wire A. First, perform alkaline degreasing cleaning: The temperature of the alkaline degreasing solution is controlled at 60-80°C and soaked at this temperature for 8-12 minutes; the alkaline degreasing solution is a NaOH solution containing 30-80g / L; B. Electrolytic degreasing: process parameters: voltage 3-12V, DC power supply 5-15 A / dm, electrolytic degreasing temperature 60-80℃; C. Carry out hydrochloric acid pickling and rust removal The mass concentration of hydrochloric acid pickling solution is 18-22%, the pickling temperature is 25-35℃, and the pickling time is 5-15min; D. For slow release, add 0.5-1.0% of hexamethylenetetramine as corrosion inhibitor; E. Water washing and neutralization Use three-stage countercurrent water washing, the conductivity does not exceed 50μS / cm, and the pH value is adjusted between 6.5 and 7.5; 2) Perform flux plating treatment A. Impregnation is performed, the immersion temperature is controlled at 60-70°C, the immersion solution is: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%. The pH value of the immersion solution is 3.5-4.5, the immersion time is 1-2min, and a dense compound pre-plating layer of 10-15μm is formed; B. Drying, the drying temperature is 120 ~ 150 ℃, and the drying time does not exceed 30s; C. Heat the steel wire until the temperature difference between its surface and the zinc liquid is no more than 50°C; 3) Hot dip galvanizing A. The temperature of the hot-dip plating solution is controlled at 440-480℃, and the temperature fluctuation is controlled at ±2℃; and the Fe content in the hot-dip plating solution is controlled to be less than 0.03%; B. Hot dip galvanizing The bridge cable wire enters the zinc pot at an angle of 5 to 10 degrees; According to the diameter of the bridge cable wire: When the bridge cable steel wire is ф5mm series, the hot dip coating temperature is 440~460℃, and the hot dip coating time is 30~60s; When the bridge cable steel wire is ф7.0mm series, the hot dip coating temperature is 450-460℃, and the hot dip coating time is 30-60s; C. Use nitrogen air knife pressure of 0.2~0.4MPa, 50~100mm away from zinc liquid surface, and control the coating thickness accuracy within 10μm; .4) Processing A. Perform graded cooling First, air-cool the sample from 450°C to 250-300°C at a cooling rate of 50°C / s; then naturally cool the sample to room temperature; B. Passivation is performed using a chromate passivation plating solution with a mass concentration of 3 to 5 g / L to form a brown passivation film with a thickness of 0.5 to 1 μm. The passivation time is 30 to 60 seconds. 5) For oil protection, use electrostatic spraying of anti-rust oil, control the oil film thickness at 2-5μm, and the friction coefficient at 0.08-0.12.
[0014] It should be noted that the values of the following items in the embodiments are all within the specified ranges: 1. Alkaline degreasing solution is a NaOH solution containing 30-80g / L; 2. In the impregnation solution: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%; 3. The Fe content in the hot dip bath is less than 0.03%; 4. The mass concentration of chromate passivation plating solution is 3-5g / L.
[0015] Functions and mechanisms of the components and main processes in the present invention Al: When 5 wt.% Al is added to the zinc bath, it forms a zinc-aluminum eutectic structure. The alloy with a 5% aluminum content has a relatively low melting point of 381°C, which significantly impacts the mechanical properties of the bridge cable steel wire during hot-dip plating. This makes it a popular choice for cold-drawn bridge cable steel wire. However, increasing the aluminum content increases the bath melting point, reduces the eutectic structure, and increases dendrite size, negatively impacting the mechanical properties and corrosion resistance of the coating. Overcoming this shortcoming is crucial, so this paper uses aluminum contents ranging from 5% to 20% for comparison.
[0016] RE: The addition of rare earth elements to the alloy bath of this invention primarily improves the wettability of the bath on the bridge cable steel wire substrate and refines the microstructure. Silicon is added to the bath to prevent a strong exothermic reaction between the bath and the bridge cable steel wire substrate and to refine the microstructure. The addition of rare earth elements and silicon improves the coating quality. However, if the addition amount is below a specified limit, the improvement in microstructure is insignificant. If the addition amount is above the specified limit, a rare earth secondary phase is generated, exacerbating intergranular corrosion and reducing the corrosion resistance of the coating. Therefore, the present invention limits the content to 0.05-1.0%.
[0017] Si: Si inhibits the growth of compounds between iron and aluminum or iron and zinc, thereby improving the adhesion of the coating. It also refines the coating's grain size, and adding it in appropriate amounts can enhance corrosion resistance. Zn-Al alloy coatings often contain defects such as cracks and pores, which serve as initiation points for corrosion. The addition of Si improves the coating's quality and uniformity, thereby enhancing its corrosion resistance. Si significantly improves the corrosion resistance of Zn-Al alloy coatings. Si increases the undercooling of the Zn-Al-Mg alloy melt and significantly refines the coarse, dendritic structure of the Al-rich phase. The effect is more pronounced with higher Si content. Si, with a diameter of tens of nanometers, inhibits the diffusion of iron from the substrate surface into the zinc solution, thereby preventing the formation of an Al-Fe alloy layer. When Si is added to the plating bath, it precipitates at the interface between the substrate and the coating during hot-dip plating, reducing the coating thickness and contributing to improved coating processability. The addition of Si inhibits the excessive growth of the alloy layer and refines the coating's grain size. However, when the added amount is lower than the limit value, the effect of the organizational change is not obvious; when the added amount is higher than the limit value, a silicon-rich second phase will be generated, aggravating intergranular corrosion and destroying the stability of the coating; therefore, the present invention limits the limit to 0.05~3.0%.
[0018] The reason why the present invention controls Si / RE to not exceed 3.0 is that both rare earth elements and silicon elements have the effect of refining grains, and the amount of silicon added is often greater than that of rare earth elements. Therefore, we designed different ratios to explore the optimal ratio for their synergistic effect.
[0019] The reason why the zinc ingot and the aluminum block are preheated to 150-200°C is to remove moisture from the zinc ingot and the aluminum block and reduce thermal shock.
[0020] The reason why the present invention preheats the smelting furnace to not less than 400°C is to reduce thermal shock, improve smelting efficiency, and uniformly heat the raw materials.
[0021] The reason why the aluminum blocks are added in at least two batches in the present invention is to make the composition of the plating solution uniform, reduce segregation, and reduce the oxidation of rare earth and silicon.
[0022] The reason why the present invention adopts the method of adding metal cerium, lanthanum and silicon at one time to cool the solution to 550-570°C is that the amount of cerium, lanthanum and silicon added is small and can be added at one time, and lowering the temperature can reduce the loss of these elements.
[0023] The reason why the hot dip plating solution temperature is naturally cooled to 440-480° C. in the present invention is that the plating solution has good fluidity in this range and is suitable for hot dip plating of steel wire. Too high a temperature has a greater impact on the mechanical properties of the steel wire.
[0024] The present invention controls the temperature of the alkaline degreasing solution at 60-80°C and soaks at this temperature for 8-12 minutes; the alkaline degreasing solution is a 30-80g / L NaOH solution because it is conducive to fully removing grease from the surface of the steel wire and reducing plating leakage.
[0025] The reason why the present invention controls the concentration of the hydrochloric acid pickling solution to be 18-22%, the pickling temperature to be 25-35° C., and the pickling time to be 5-15 minutes is that the oxide layer and rust on the surface of the steel wire need to be removed to reduce plating leakage.
[0026] The present invention adopts three-stage countercurrent water washing, controls the conductivity to not exceed 50 μS / cm, and adjusts the pH value to 6.5-7.5 because it is necessary to remove the acid on the surface of the steel wire and improve the effect of hot-dip plating.
[0027] The reason why the present invention controls the immersion temperature at 60-70°C, the immersion liquid is: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%, the pH value of the immersion liquid is 3.5-4.5, the immersion time is 1-2min, and a dense compound pre-plating layer of 10-15μm is formed, is because the formed pre-plating layer can improve the coating adhesion effect.
[0028] The reason why the present invention controls the drying temperature to be 120-150° C. and the drying time to be no more than 30 seconds is that high-temperature drying for too long a time will destroy the pre-plating layer, resulting in a decrease in the adhesion of the plating layer.
[0029] The reason why the present invention heats the steel wire until the temperature difference between its surface temperature and the zinc liquid temperature does not exceed 50°C is to reduce the sudden drop in the zinc liquid temperature, stabilize the fluidity of the zinc, control the internal thermal stress of the steel wire, and prevent it from cracking.
[0030] The present invention controls during hot dip coating: A. The temperature of the hot-dip plating solution is controlled at 440-480℃, and the temperature fluctuation is controlled at ±2℃; and the Fe content in the hot-dip plating solution is controlled to be less than 0.03%; B. Hot dip galvanizing The bridge cable wire enters the zinc pot at an angle of 5 to 10 degrees; According to the diameter of the bridge cable wire: When the bridge cable steel wire is ф5mm series, the hot dip coating temperature is 440~460℃ and the hot dip coating time is 30~60s; When the bridge cable steel wire is ф7.0mm series, the hot dip coating temperature is 450-460℃, and the hot dip coating time is 30-60s; C. Use nitrogen air knife with pressure of 0.2~0.4MPa, 50~100mm away from zinc liquid surface, and control coating thickness with accuracy of ±10μm. This is to isolate oxygen from the liquid surface, prevent zinc from oxidizing at night, reduce zinc slag, and not disturb the liquid surface. Uniform coating thickness is conducive to coating adhesion.
[0031] The present invention uses a chromate passivation plating solution with a mass concentration of 3 to 5 g / L to form a brown passivation film with a thickness of 0.5 to 1 μm, and the passivation time is 30 to 60 seconds. The surface treatment uses chromate passivation to form a 0.5-1μm passivation film. This is because the passivation layer can further improve the corrosion resistance of the coating. If it is too thin, the effect is not good, and if it is too thick, the original coating structure will be damaged.
[0032] The present invention adopts electrostatic spraying of anti-rust oil, controls the oil film thickness to be 2-5 μm, and the friction coefficient to be 0.08-0.12, because too thin an oil film cannot achieve the anti-rust effect, and too thick an oil film leads to excessively high costs, affecting the use effect.
[0033] It should be noted that the following items are sufficient as long as they are within the specified scope: 1. Alkaline degreasing solution is a NaOH solution containing 30-80g / L; 2. In the impregnation solution: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%; 3. The Fe content in the hot dip bath is less than 0.03%; 4. The mass concentration of chromate passivation plating solution is 3-5g / L.
[0034] Compared with existing technologies: 1. Due to the use of Zn-Al-RE-Si alloy hot-dip plating solution, the present invention makes the microstructure distribution of the prepared coating more uniform, the corrosion resistance is better, the protective performance of the coating is significantly improved, and the coating has good bonding with the substrate. Excellent intermetallic compounds are formed between the coating and the substrate, effectively enhancing the comprehensive performance of the coating.
[0035] 2. The present invention proposes a new type of hot-dip galvanizing solution composition and corresponding process suitable for various types of bridge cable steel wires, which has low cost, streamlined process, simple operation, uniform coating structure, good corrosion resistance, and wide application range, providing reference and practical guidance for the application and development of hot-dip galvanizing process for bridge cable steel wires.
[0036] 3. The present invention provides a facilitation process particularly suitable for bridge cable steel wires, forming a dense Fe-Zn compound pre-plating layer of 10 to 15 μm, further enhancing the bonding strength of the coating.
[0037] 4. This invention simplifies the hot-dip coating process. Short-term hot-dip coating significantly impacts the mechanical properties of ultra-high-strength bridge cable steel wire. By precisely controlling the hot-dip coating temperature and time, and precisely controlling the aging of cementite spheroidization during the hot-dip coating process, we can combine heat treatment with hot-dip coating, simplifying the process and achieving both excellent corrosion resistance and mechanical properties during the hot-dip coating process.
[0038] According to the hot-dip coating temperature and hot-dip coating time applicable to steel wires of different diameters, the present invention ensures that the 5mm diameter series steel wire has the best performance when hot-dip coated at 440-450°C for 30-60s, with a tensile strength of 2148 MPa, an elongation of 4.95%, and a number of twisting cycles of 15 times; and the 7mm diameter series steel wire has the best performance when hot-dip coated at 450-460°C for 30-60s, with a tensile strength of 2160 MPa, an elongation of 5.53%, and a number of twisting cycles of 14 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the SEM image of the coating structure of the present invention. DETAILED DESCRIPTION
[0040] The present invention is described in detail below: Table 1 is a list of chemical compositions of various embodiments and comparative examples of the present invention; Table 2 is a list of main process parameters for preparing hot dip plating solutions of various embodiments of the present invention and comparative examples; Table 3 is a list of process parameter values for each embodiment and comparative example of the present invention; Table 4 is a list of mechanical property test results of various embodiments of the present invention and comparative examples.
[0041] Each embodiment of the present invention is produced according to the following steps: 1) Preheat the zinc ingot and aluminum block to 150-200°C, and control the moisture content of the preheated zinc ingot and aluminum block to no more than 0.02%; 2) Preheat the melting furnace to no less than 400°C; 3) Place the zinc ingot in the container and heat it to melt at 450-480°C until the ingot is completely melted, stirring during the melting process. 4) Add the aluminum in three batches: 50% of the total amount in the first batch, 30% in the second batch, and the remaining 20% in the third batch. While adding the aluminum, raise the temperature to 600-620°C and continue stirring until the aluminum is completely dissolved. 5) Add RE and silicon A. When the melt temperature drops to 550-570°C after adding the aluminum block, mix the set RE and silicon and add them all at once, and control the Si / RE ratio not to exceed 3 / 3. Continue stirring during the addition process until the RE and silicon are completely dissolved; B. Add or pass impurity adsorbent into the completely dissolved RE and silicon mixture and keep warm for 10 to 30 minutes; add impurity adsorbent in an amount such that the impurities in the RE and silicon mixture are ≤0.005%; 6) Cool the hot dip bath naturally to 440-480°C and set aside.
[0042] A method for using a hot-dip plating solution for bridge cable steel wires, comprising the following steps: 1) Pretreatment stage of bridge cable wire A. First, perform alkaline degreasing cleaning: The temperature of the alkaline degreasing solution is controlled at 60-80°C and soaked at this temperature for 8-12 minutes; the alkaline degreasing solution is a NaOH solution containing 30-80g / L; B. Electrolytic degreasing: process parameters: voltage 3-12V, DC power supply 5-15 A / dm, electrolytic degreasing temperature 60-80℃; C. Carry out hydrochloric acid pickling and rust removal The mass concentration of hydrochloric acid pickling solution is 18-22%, the pickling temperature is 25-35℃, and the pickling time is 5-15min; D. For slow release, add 0.5-1.0% of hexamethylenetetramine as corrosion inhibitor; E. Water washing and neutralization Use three-stage countercurrent water washing, the conductivity does not exceed 50μS / cm, and the pH value is adjusted between 6.5 and 7.5; 2) Perform flux plating treatment A. Impregnation is performed, the immersion temperature is controlled at 60-70°C, the immersion solution is: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%. The pH value of the immersion solution is 3.5-4.5, the immersion time is 1-2min, and a dense compound pre-plating layer of 10-15μm is formed; B. Drying, the drying temperature is 120 ~ 150 ℃, and the drying time does not exceed 30s; C. Heat the steel wire until the temperature difference between its surface and the zinc liquid is no more than 50°C; 3) Hot dip galvanizing A. The temperature of the hot-dip plating solution is controlled at 440-480℃, and the temperature fluctuation is controlled at ±2℃; and the Fe content in the hot-dip plating solution is controlled to be less than 0.03%; B. Hot dip galvanizing The bridge cable wire enters the zinc pot at an angle of 5 to 10 degrees; According to the diameter of the bridge cable wire: When the bridge cable steel wire is ф5mm series, the hot dip coating temperature is 440~460℃, and the hot dip coating time is 30~60s; When the bridge cable steel wire is ф7.0mm series, the hot dip coating temperature is 450-460℃, and the hot dip coating time is 30-60s; C. Use nitrogen air knife pressure of 0.2~0.4MPa, 50~100mm away from zinc liquid surface, and control the coating thickness accuracy within 10μm; .4) Processing A. Perform graded cooling First, air-cool the sample from 450°C to 250-300°C at a cooling rate of 50°C / s; then naturally cool the sample to room temperature; B. Passivation is performed using a chromate passivation plating solution with a mass concentration of 3 to 5 g / L to form a brown passivation film with a thickness of 0.5 to 1 μm. The passivation time is 30 to 60 seconds. 5) For oil protection, use electrostatic spraying of anti-rust oil, control the oil film thickness at 2-5μm, and the friction coefficient at 0.08-0.12.
[0043] It should be noted that the values of the following items in the embodiments are all within the specified ranges: 1. Alkaline degreasing solution is a NaOH solution containing 30-80g / L; 2. In the impregnation solution: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%; 3. The Fe content in the hot dip bath is less than 0.03%; 4. The mass concentration of chromate passivation plating solution is 3-5g / L.
[0044] Table 1 Chemical composition list of various embodiments of the present invention and comparative examples (wt%)
[0045] Table 2 List of main process parameters for preparing hot dip plating solutions of various embodiments of the present invention and comparative examples
[0046] Table 3 List of process parameter values for the main methods used in various embodiments and comparative examples of the present invention
[0047] Continued Table 3-1
[0048] Continued Table 3-2
[0049] Table 4 Mechanical properties test results of various embodiments of the present invention and comparative examples
[0050] As can be seen from Table 4, from the salt spray corrosion data, during the 1200h corrosion process, compared with the 210g / m2 pure zinc coating in Comparative Example 1, 2 , and 190 g / m 2 The mass loss was reduced to 100g / m after adding 5% Al content. 2 and 89 g / m 2 When Si, La and Ce elements were added, the mass loss was generally reduced to 80 g / m 2 the following.
[0051] From the comprehensive data of strength, elongation, and torsional performance of steel wire under different hot dip treatment times and temperatures, the ф5mm series steel wire has the best performance when hot dipped at 440-450℃ for 30-60s, with a tensile strength of 2148Mpa, an elongation of 4.95%, and a torsional number of 15 times; the ф7mm series steel wire has the best performance when hot dipped at 450-460℃ for 30-60s, with a tensile strength of 2160Mpa, an elongation of 5.53%, and a torsional number of 14 times. It can be seen that the components manufactured by the present invention have the best performance when hot dipped at 625℃ and 10 5 h service environment, its high-temperature endurance strength performance can reach more than 120 MPa, and the oxidation weight gain is significantly reduced and the oxidation resistance is significantly improved, which is a significant improvement compared with traditional 9%Cr heat-resistant steel materials.
[0052] This specific implementation is only the best example and is not a limitative implementation of the technical solution of the present invention.
Claims
1. A hot-dip plating solution for bridge cable steel wire, wherein the chemical composition and mass percentage content are: Al: 5-20%, RE: 0.05-1.0%, Si: 0.05-3.0%, and the remainder is Zn and unavoidable impurities; and the Si / RE ratio does not exceed 3.0; the RE is Ce and La, and the two are added in a ratio of 1:
1.
2. The hot-dip plating bath for bridge cable steel wire according to claim 1, characterized in that: Si / RE does not exceed 2.
5.
3. The hot-dip plating bath for bridge cable steel wire according to claim 1, characterized in that: The mass percentage content of RE is 0.07~0.75%.
4. The hot-dip plating bath for bridge cable steel wire according to claim 1, characterized in that: The Si mass percentage content is 0.07~2.25%.
5. The method for preparing a hot-dip plating solution for bridge cable steel wire according to claim 1, comprising the following steps: 1) Preheat the zinc ingot and aluminum block to 150-200°C, and control the moisture content of the preheated zinc ingot and aluminum block to no more than 0.02%; 2) Preheat the melting furnace to no less than 400°C; 3) Place the zinc ingot in the container and heat it to melt at 450-480°C until the ingot is completely melted, stirring during the melting process. 4) Add the aluminum in three batches: 50% of the total amount in the first batch, 30% in the second batch, and the remaining 20% in the third batch. While adding the aluminum, raise the temperature to 600-620°C and continue stirring until the aluminum is completely dissolved. 5) Add RE and silicon A. When the melt temperature drops to 550-570°C after adding the aluminum block, mix the set RE and silicon and add them all at once, and control the Si / RE ratio to not more than 3. Continue stirring during the addition process until the RE and silicon are completely dissolved; B. Add or pass impurity adsorbent into the completely dissolved RE and silicon mixture and keep warm for 10 to 30 minutes; add impurity adsorbent in an amount such that the impurities in the RE and silicon mixture are ≤0.005%; 6) Cool the hot dip bath naturally to 440-480°C and set aside.
6. The method for preparing a hot-dip plating solution for bridge cable steel wire according to claim 5, characterized in that: The impurity adsorbent is hexachloroethane or an inert gas.
7. A method for using the hot-dip plating solution for bridge cable steel wire according to claim 1, comprising the following steps: 1) Pretreatment stage of bridge cable wire A. First, perform alkaline degreasing cleaning: The temperature of the alkaline degreasing solution is controlled at 60-80°C and soaked at this temperature for 8-12 minutes; the alkaline degreasing solution is a NaOH solution containing 30-80g / L; B. Electrolytic degreasing: process parameters: voltage 3-12V, DC power supply 5-15 A / dm, electrolytic degreasing temperature 60-80℃; C. Carry out hydrochloric acid pickling and rust removal The mass concentration of hydrochloric acid pickling solution is 18-22%, the pickling temperature is 25-35℃, and the pickling time is 5-15min; D. For slow release, add 0.5-1.0% of hexamethylenetetramine as corrosion inhibitor; E. Water washing and neutralization Use three-stage countercurrent water washing, the conductivity does not exceed 50μS / cm, and the pH value is adjusted between 6.5 and 7.5; 2) Perform flux plating treatment A. Impregnation is performed, the immersion temperature is controlled at 60-70°C, the immersion solution is: ZnCl2 solution with a mass concentration of 500-600g / L, NH4Cl solution with a mass concentration of 80-100g / L, and CeCl3 solution with a mass concentration of 0.1-0.3%. The pH value of the immersion solution is 3.5-4.5, the immersion time is 1-2min, and a dense compound pre-plating layer of 10-15μm is formed; B. Drying, the drying temperature is 120 ~ 150 ℃, and the drying time does not exceed 30s; C. Heat the steel wire until the temperature difference between its surface and the zinc liquid does not exceed 50°C; 3) Hot dip galvanizing A. The temperature of the hot-dip plating solution is controlled at 440-480℃, and the temperature fluctuation is controlled at ±2℃; and the Fe content in the hot-dip plating solution is controlled to be less than 0.03%; B. Hot dip galvanizing The bridge cable wire enters the zinc pot at an angle of 5 to 10 degrees; According to the diameter of the bridge cable wire: When the bridge cable steel wire is ф5mm series, the hot dip coating temperature is 440~460℃, and the hot dip coating time is 30~60s; When the bridge cable steel wire is ф7.0mm series, the hot dip coating temperature is 450-460℃, and the hot dip coating time is 30-60s; C. Use nitrogen air knife pressure of 0.2~0.4MPa, 50~100mm away from zinc liquid surface, and control the coating thickness with an accuracy of 10μm; 4) Processing A. Perform graded cooling First, air-cool the sample from 450°C to 250-300°C at a cooling rate of 50°C / s; then naturally cool the sample to room temperature; B. Passivation is performed using a chromate passivation plating solution with a mass concentration of 3 to 5 g / L to form a brown passivation film with a thickness of 0.5 to 1 μm. The passivation time is 30 to 60 seconds. 5) For oil protection, use electrostatic spraying of anti-rust oil, control the oil film thickness at 2-5μm, and the friction coefficient at 0.08-0.12.
Citation Information
Patent Citations
Hot dipping method for zinc-aluminum coating of bridge cable
CN107557713A
Zinc-aluminum alloy steel wire coating double-immersion plating process for new bridge cable
CN111101084A
Cited By
Preparation method of corrosion-resistant steel wire mesh
CN121156150A