Titanium oxide powder and method for producing same
By synthesizing and drying anatase-type titanium oxide powder under a specific atmosphere, the problems of dispersion and composition management in the prior art were solved, and high-performance titanium oxide powder suitable for electronic devices were prepared.
Patent Information
- Application Number
- CN202380022725.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2025-08-29
- Estimated Expiration
- 2043-12-27
AI Technical Summary
It is difficult to prepare anatase-type titanium oxide powder with high specific surface area and high dispersion in the prior art, and the silicon, phosphorus and other elements in the dispersant affect the performance of electronic devices, making it difficult to meet the strict composition management and dispersion requirements of electronic device materials.
Anatase-type titanium oxide is synthesized in the presence of urea, ammonium compounds, inorganic acids or organic acids, and dried under an atmosphere with an initial relative humidity of 70 to 100%, thereby inhibiting particle aggregation, and obtaining a titanium oxide powder with high specific surface area and high dispersion.
Anatase-type titanium oxide powder with high specific surface area, good dispersion and stability is suitable for electronic device materials and avoids the negative impact of dispersants on performance.
Smart Images

Figure BDA0005001346360000141 
Figure BDA0005001346360000171
Abstract
Description
Technical Field
[0001] The present invention relates to titanium oxide powder and a method for producing the same. Background Art
[0002] Titanium (IV) oxide (TiO2) is a chemically stable material used industrially in a wide range of fields, including as a white pigment. Furthermore, titanium (IV) oxide reacts with barium carbonate to form barium titanate. Barium titanate is known to be effectively used as a material for multilayer ceramic capacitors, which are components of smartphones and other applications.
[0003] As the crystal structures that titanium oxide can take, the three main known ones are anatase phase, brookite phase, and rutile phase. In particular, anatase-type titanium oxide has more hydroxyl groups on the surface than other crystalline phases, so it has high hydrophilicity and high dispersibility. In addition, since anatase-type titanium oxide has more hydroxyl groups on the surface, it has high surface reactivity with other metal elements and is in high demand as a raw material for dielectric materials and battery materials. In recent years, in order to achieve higher functions in these applications, anatase-type microparticles of titanium oxide with a high specific surface area have been sought.
[0004] On the other hand, as particles become finer, their surface free energy increases, and therefore, the particles tend to aggregate with each other, deteriorating their dispersibility. In order to suppress the aggregation of particles, a method has been reported, such as Patent Document 1, in which the particle surface is modified with a modifier such as a silane agent and the particles are dispersed in a dispersion containing an amine agent to stabilize the particles.
[0005] Owing to generally use the method that mixes with aqueous solvent, alcohol solvent when mixing nanoparticle, therefore can use the method that improves the compatibility with solvent by the hydrophilicity that improves particle surface.As the method that the hydrophilicity of particle surface is improved, there is the method that particle surface is modified with the polymer that comprises silicon etc. as patent documentation 2, patent documentation 3.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 2008-247712
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 2015-212355
[0010] Patent Document 3: Japanese Patent Application Laid-Open No. 2010-95392 Summary of the Invention
[0011] However, in the manufacture method of patent document 1, although a dispersion liquid of nanoparticles can be obtained, it is very difficult to manage the concentration during manufacture and storage in the form of the dispersion liquid. Therefore, the dispersion liquid obtained by adopting the manufacture method disclosed in patent document 1 is not suitable for making titanium oxide for electronic device applications such as dielectric materials and battery materials that require strict composition management. In addition, the silicon and phosphorus contained in the dispersant have a significant impact on the main properties such as the dielectric constant and electrical conductivity of the electronic device application material, and are therefore not suitable as electronic device materials.
[0012] Furthermore, the titanium oxide described in Patent Documents 2 and 3 also contains a large amount of silicon and is therefore not suitable as an electronic device material.
[0013] Therefore, when used as an electronic device material, highly dispersible anatase-type titanium oxide ultrafine particles are sought in the form of a dry powder that can be uniformly mixed with other raw materials based on a rigorously calculated composition. Furthermore, to prevent degradation of the properties of the electronic device material, the anatase-type titanium oxide microparticle powder must not contain semimetallic elements such as silicon and phosphorus, metallic elements such as sodium and magnesium, or high-molecular organic acid chains such as polyols.
[0014] An object of the present invention is to provide anatase-type titanium oxide powder having a high specific surface area and high dispersibility, and a method for producing the same.
[0015] The inventors have discovered that by synthesizing anatase-type titanium oxide through the hydrolysis of titanium tetrachloride in the presence of a dispersant such as urea, ammonium compounds, inorganic acids, or organic acids, and drying the synthesized titanium oxide in an atmosphere with an initial relative humidity of 70 to 100%, dense aggregation and grain growth of particles can be suppressed, and dry powder can be obtained without inactivating the hydroxyl groups on the particle surface, thereby obtaining anatase-type titanium oxide powder with a high specific surface area, high affinity with solvents, and high dispersibility.
[0016] The present invention for achieving the above-mentioned object is constructed as follows.
[0017] (1) The titanium oxide powder according to one embodiment of the present invention has a BET specific surface area of 300 m 2 / g and above 480m 2 / g or less, the anatase content of the crystalline phase measured by XRD measurement is 90% or more, and the spin-spin relaxation time T2 measured by pulse NMR on a 5 wt% suspension prepared using ion-exchanged water is 46 ms or more and 103 ms or less.
[0018] (2) In the titanium oxide powder described in (1) above, the carbon content may be 0.5 mass % or less.
[0019] (3) In the titanium oxide powder described in (1) or (2) above, the chlorine content may be 0.1 mass % or less, the silicon content may be 0.1 mass % or less, and the sulfur content may be 0.1 mass % or less.
[0020] (4) In the titanium oxide powder described in any one of (1) to (3) above, the half-value width of the diffraction peak at a diffraction angle 2θ of 24.5° to 26.0° may be 1.10° to 2.00°.
[0021] (5) The titanium oxide powder according to any one of (1) to (4) above may have a zeta potential of -63 mV or more and -40 mV or less.
[0022] (6) A method for producing titanium oxide powder according to one embodiment of the present invention comprises:
[0023] A synthesis step of mixing an aqueous solution containing urea and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the urea / Ti (molar ratio) becomes 0.001 to 0.058, and precipitating titanium oxide; and
[0024] The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
[0025] (7) A method for producing titanium oxide powder according to one embodiment of the present invention comprises:
[0026] A synthesis step of mixing an aqueous solution containing an ammonium compound and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the ammonium compound / Ti (molar ratio) is 0.001 to 0.029, and precipitating titanium oxide; and
[0027] The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
[0028] (8) In the method for producing titanium oxide powder described in (6) or (7) above, the pH of the aqueous solution containing at least one of urea and an ammonium compound may be less than 12.0.
[0029] (9) A method for producing titanium oxide powder according to one embodiment of the present invention comprises:
[0030] A synthesis step of mixing an aqueous solution containing an inorganic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the inorganic acid / Ti (molar ratio) becomes 0.001 to 0.030, and precipitating titanium oxide; and
[0031] The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
[0032] (10) A method for producing titanium oxide powder according to one embodiment of the present invention comprises:
[0033] A synthesis step of mixing an aqueous solution containing an organic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the acidic functional group of the organic acid / Ti (molar ratio) is 0.001 to 0.037, and precipitating titanium oxide; and
[0034] The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
[0035] (11) In the method for producing titanium oxide powder described in (10) above, the organic acid may be an α-hydroxycarboxylic acid.
[0036] (12) In the method for producing titanium oxide powder described in (10) or (11) above, the molecular weight of the organic acid or inorganic acid in the aqueous solution may be 300 or less.
[0037] (14) The method for producing titanium oxide powder described in (6) to (13) above may further include a purification step of purifying titanium oxide using any one or more of an ultrafiltration membrane, a reverse osmosis membrane, an ion exchange resin, and an electrodialysis membrane.
[0038] According to the present invention, an anatase-type titanium oxide powder having a high specific surface area and high dispersibility and a method for producing the same can be provided. DETAILED DESCRIPTION
[0039] Hereinafter, an example of an embodiment of the present invention will be described. However, the present invention is not limited to the following example.
[0040] In this embodiment, unless otherwise specified, "titanium oxide" refers to titanium (IV) oxide (TiO2). In addition, "Ti concentration" refers to the concentration obtained by dividing (the amount of Ti atoms in all components containing titanium atoms, such as titanium compounds, ions containing titanium, and complexes) by (the volume of the solution containing Ti).
[0041] <1. Titanium Oxide Powder>
[0042] The titanium oxide powder according to one embodiment of the present invention has a BET specific surface area of 300 m 2 / g and above 480m 2 / g or less, the anatase content of the crystalline phase measured by XRD measurement is 90% or more, and the spin-spin relaxation time T2 measured by pulse NMR (Nuclear Magnetic Resonance) on a 5% by mass suspension prepared using ion-exchanged water is 46 ms or more and 103 ms or less.
[0043] (BET specific surface area)
[0044] As described above, the BET specific surface area of the titanium oxide powder according to one embodiment of the present invention is 300 m 2 / g or more. If 300m 2 / g or more, when titanium oxide is reacted with other substances, an ultrafine material represented by a 0201 size multilayer ceramic capacitor material can be obtained. From the same point of view, from the perspective of obtaining an ultrafine material with a finer particle size, the BET specific surface area of titanium oxide powder is preferably 350m 2 / g or more, more preferably 380m 2 / g or above.
[0045] As described above, the BET specific surface area of the titanium oxide powder according to one embodiment of the present invention is 480 m 2 / g or less. If 480m 2 / g or less, even when reacting with barium carbonate at high temperature, the abnormal particle growth of titanium oxide can be suppressed, and the particle size distribution of the obtained material, i.e., barium titanate, can be made uniform. From the same point of view, from the perspective of obtaining a material with a more uniform particle size distribution, the BET specific surface area of titanium oxide powder is preferably 430 m 2 / g or less, more preferably 400m 2 / g or less.
[0046] (Anatase content)
[0047] The anatase phase content of the titanium oxide powder of this embodiment, as measured by XRD, is 90% or greater. When reacting other substances with titanium oxide, a high anatase phase content in the titanium oxide powder increases reactivity, which is advantageous. From the same perspective, the anatase phase content is more preferably 95% or greater, and even more preferably 99% or greater.
[0048] (Spin-spin relaxation time)
[0049] Unlike high-resolution NMR, pulsed NMR does not provide chemical shift information. Instead, it can rapidly measure the 1H nuclear relaxation time (spin-lattice relaxation time T1 and spin-spin relaxation time T2), which is closely related to molecular mobility.
[0050] In recent years, the use of pulsed NMR has rapidly expanded. As measurement methods for pulsed NMR, the Hahn echo method, the solid-state echo method, the CPMG method, or 90° pulsed NMR can be listed, all of which can be appropriately used. However, the spin-spin relaxation time T2 in the present invention refers to the spin-spin relaxation time T2 of the 1H nucleus measured using the CPMG method.
[0051] The spin-spin relaxation time T2 of the 1H nuclei of the titanium oxide in this embodiment, measured using the CPMG method using pulsed NMR when dispersed in water, can be considered a property related to the state of water molecules bound to the titanium oxide surface. Specifically, it is believed that a smaller spin-spin relaxation time T2 indicates a greater number of water molecules bound to the titanium oxide surface (a thicker hydration layer), thereby improving the dispersibility of the titanium oxide and facilitating enhanced filtration performance.
[0052] The CPMG method of pulsed NMR is used to measure the suspension of 5% by mass of the titanium oxide powder of one embodiment of the present invention made with ion exchange water, and the spin-spin relaxation time T2 obtained is more than 46ms and less than 103ms. If the spin-spin relaxation time T2 of the above-mentioned suspension is more than 46ms, then when the titanium oxide powder is re-slurried to obtain barium titanate and is made into dispersion liquid, it will not become overdispersed, and is suppressed to appropriate viscosity, and the flow state is excellent, thus being advantageous when reacting with other substances. From the same viewpoint, the spin-spin relaxation time T2 is preferably more than 60ms, more preferably more than 70ms. If the spin-spin relaxation time T2 is less than 103ms, the water molecules bound by the titanium oxide surface become more (hydration layer thickness), so it can be considered that excellent dispersibility. From the same viewpoint, the spin-spin relaxation time T2 is preferably less than 90ms, more preferably less than 80ms.
[0053] (Elemental Analysis)
[0054] When the titanium oxide powder according to this embodiment is used as a raw material for a dielectric material, the presence of Cl (chlorine), Fe (iron), Al (aluminum), Si (silicon), and S (sulfur) is expected to reduce the dielectric constant. Therefore, the chlorine, aluminum, silicon, and sulfur contents of the titanium oxide powder according to this embodiment are each preferably 0.1% by mass or less, more preferably 0.05% by mass or less, and even more preferably 0.01% by mass or less. While the lower limit is not particularly limited, it is preferably 0.0001% by mass or more from the perspective of production process costs.
[0055] In order to suppress the precipitation of by-products derived from C (carbon), the carbon content of the titanium oxide according to one embodiment of the present invention is preferably 0.50 mass% or less, more preferably 0.30 mass% or less, and even more preferably 0.10 mass% or less. The lower limit is not particularly limited, but is preferably 0.001 mass% or more from the perspective of production process costs.
[0056] (Half-value width of diffraction peak in crystallinity X-ray diffraction measurement)
[0057] The titanium oxide powder of this embodiment preferably has a half-value width (FWHM) of a diffraction peak exhibiting a diffraction angle 2θ in the range of 24.5° to 26.0°, as measured by X-ray diffraction (XRD). In this case, the titanium oxide powder has a small FMHM and high crystallinity, which is preferred. However, when the reaction is carried out at a high temperature in order to make the FMHM very small, this also causes agglomeration of the titanium oxide powder, and the BET specific surface area tends to decrease. Therefore, from the perspective of obtaining a titanium oxide powder that is not very agglomerated, it is desirable to have the FMHM be above a certain value, preferably above 1.10°. From the same perspective, the FWHM is more preferably above 1.30°, and even more preferably above 1.50°.
[0058] The FWHM is preferably 2.00° or less. This is because the better the crystallinity of titanium oxide, the higher the crystallinity of the product produced using titanium oxide. From the same perspective, it is more preferably 1.90° or less, and even more preferably 1.80° or less.
[0059] The titanium oxide powder according to one embodiment of the present invention, having the above-described configuration, has a zeta potential of -63 mV to -40 mV. In other words, the absolute value of the zeta potential of the titanium oxide powder according to this embodiment is 40 mV to 63 mV. Thus, the titanium oxide powder according to one embodiment of the present invention has a high zeta potential, resulting in improved dispersibility. Furthermore, since the zeta potential is not excessive, it is possible to prevent overdispersion and excessive viscosity of the dispersion, which could lead to poor flow, when producing barium titanate.
[0060] <2. Method 1 for producing titanium oxide powder>
[0061] Hereinafter, a method for producing the titanium oxide powder according to the above embodiment will be described.
[0062] One embodiment of the present invention relates to a method for producing titanium oxide powder, comprising a synthesis step and a drying step. The synthesis step is a step of mixing an aqueous solution containing any one of urea, an ammonia compound, an organic acid, and an inorganic acid with an aqueous solution containing titanium tetrachloride and having a pH of less than 3, thereby precipitating titanium oxide. In the synthesis step, (i) when using an aqueous solution containing urea, mixing is performed so that the urea / Ti (molar ratio) is 0.001 to 0.058, (ii) when using an aqueous solution containing an ammonia compound, mixing is performed so that the urea / Ti (molar ratio) is 0.001 to 0.029, (iii) when using an aqueous solution containing an inorganic acid, mixing is performed so that the inorganic acid / Ti (molar ratio) is 0.001 to 0.030, and (iv) when using an aqueous solution containing an organic acid, mixing is performed so that the acidic functional group of the organic acid / Ti (molar ratio) is 0.001 to 0.037. In the drying step, the obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and powdered.
[0063] First, as Production Method 1, a method for producing titanium oxide powder using urea as an additive to a titanium tetrachloride aqueous solution will be described.
[0064] The method for producing titanium oxide powder involved in this embodiment includes: a synthesis step of mixing an aqueous solution containing urea and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 in such a manner that the urea [mol] / Ti [mol] (molar ratio) becomes greater than or equal to 0.001 and less than or equal to 0.058, and precipitating titanium oxide; and a drying step of drying the obtained titanium oxide in an atmosphere with an initial relative humidity of 70 to 100% and powderizing it.
[0065] <2-1. Synthesis Step>
[0066] As described above, an aqueous solution containing urea and an aqueous solution containing titanium tetrachloride are first mixed to obtain an aqueous solution. Hereinafter, the aqueous solution obtained by mixing is sometimes referred to as a mixed solution. During the synthesis step, hydrolysis of the titanium tetrachloride is performed. The pH of the aqueous solution containing titanium tetrachloride is less than 3. This is to facilitate the hydrolysis reaction. Furthermore, the pH of the aqueous solution containing titanium tetrachloride is preferably 2 or less, and even more preferably 1 or less, and for example, 0.1 or greater.
[0067] Urea acts as a reaction inhibitor. The addition of urea stabilizes the formation of titanium oxide particles, inhibits phase transition to the rutile phase, and suppresses aggregation.
[0068] The pH of the aqueous solution containing urea is preferably less than 12.0. This is because if the pH is less than 12.0, the hydrolysis reaction occurs rapidly, making it difficult to produce a heterogeneous phase including the brookite phase. In addition, titanium oxide slowly precipitates and is easily dispersed. From the same point of view, the pH is more preferably 11.5 or less, and even more preferably 11.0 or less. In addition, it is preferred that the pH value is greater than 10, that is, the pH value is greater than 10. This is to fully suppress the rate of the hydrolysis reaction and inhibit the phase transition to the rutile phase, which is the stable phase.
[0069] The Ti atomic concentration in the aqueous solution (mixed solution) obtained by mixing an aqueous solution containing urea and an aqueous solution containing titanium tetrachloride is preferably 0.01 mol / L or higher. This is to facilitate the hydrolysis reaction. From the same viewpoint, the Ti atomic concentration is more preferably 0.03 mol / L or higher, and even more preferably 0.05 mol / L or higher.
[0070] The Ti atomic concentration in the mixed solution is preferably 1.00 mol / L or less. This is to prevent the precipitation of the rutile phase as a stable phase by suppressing the Ti concentration. From the same viewpoint, it is more preferably 0.50 mol / L or less, and further preferably 0.20 mol / L or less.
[0071] Regarding the urea content in the mixed solution, the ratio of the amount of urea to the amount of Ti in the mixed solution (urea [mol] / Ti [mol]) is 0.001 or greater. This is to sufficiently reduce the rate of the hydrolysis reaction and suppress the phase transition to the rutile phase, which is a stable phase. To further suppress the phase transition to the rutile phase, the above ratio (urea [mol] / Ti [mol]) is preferably 0.013 or greater, and more preferably 0.030 or greater. The above ratio (urea [mol] / Ti [mol]) is 0.058 or less, and preferably 0.050 or less. This is to prevent the hydrolysis reaction from being excessively inhibited.
[0072] The mixed solution is preferably heated in order to precipitate titanium oxide. From the viewpoint of productivity, the heating of the mixed solution is preferably carried out at a high heating rate. On the other hand, in order to suppress the precipitation of amorphous titanium oxide and improve the crystallinity, it is preferred to suppress the rapid progress of the reaction and suppress the heating rate so that the crystal growth is fully carried out. Therefore, the heating of the mixed solution until the target temperature, i.e., the synthesis temperature, is reached is preferably carried out at a heating rate of 0.1°C / min or more and 1.5°C / min or less, more preferably at a heating rate of 0.3°C / min or more and 1.0°C / min or less, and further preferably at a heating rate of 0.6°C / min or more and 1.0°C / min or less.
[0073] The synthesis temperature is preferably 50° C. or higher, more preferably 60° C. or higher. This is to allow the hydrolysis reaction to proceed advantageously. The synthesis temperature is preferably 100° C. or lower. This is to suppress the phase transition to the stable rutile phase.
[0074] The holding time of the mixed solution at the synthesis temperature can be set arbitrarily. The temperature can be lowered without holding the mixture, or the mixture can be held for a predetermined time. From the perspective of fully proceeding the reaction, the holding time of the mixed solution at the synthesis temperature is preferably 15 minutes or longer. After the reaction is completed, the mixture is preferably cooled naturally to room temperature.
[0075] <2-2. Refining process>
[0076] The method for producing titanium oxide powder according to one embodiment of the present invention preferably includes a purification step for purifying the titanium oxide. In this purification step, for example, one or more of an ultrafiltration membrane, a reverse osmosis membrane, an ion exchange resin, or an electrodialysis membrane is used. By further including this purification step, the method for producing titanium oxide powder according to one embodiment of the present invention can remove Cl (chlorine), S (sulfur), Si (silicon), Fe (iron), Al (aluminum), and the like from the titanium oxide slurry obtained in the synthesis step.
[0077] The purification step is performed after the synthesis step. Since the purification step is performed with titanium oxide dispersed in a liquid, it is preferably performed before the drying step.
[0078] <2-3. Dehydration process>
[0079] The method for producing titanium oxide powder according to one embodiment of the present invention may further include a dehydration step for dehydrating the slurry using a filter press or the like to obtain a solid component. The dehydration step is performed, for example, after the synthesis step and before the drying step. If the method for producing titanium oxide powder includes a purification step, the dehydration step is performed after the purification step. Dehydration allows for efficient drying.
[0080] <2-4. Drying Process>
[0081] A method for producing titanium oxide powder according to one embodiment of the present invention includes drying the obtained titanium oxide in an atmosphere having an initial relative humidity of 70 to 100% to form a powder (drying step). The initial relative humidity refers to the relative humidity at the start of the drying step.
[0082] The drying atmosphere may be air or an inert gas atmosphere.
[0083] The titanium oxide may be dried in the state of a slurry dispersed or dissolved in water, or may be dried in a state of titanium oxide dehydrated using a filter press or the like.
[0084] In the drying process, in order to suppress the deactivation of the hydroxyl groups on the surface of the titanium oxide and remove moisture, drying is carried out in an atmosphere with an initial relative humidity of 70% or more and 100% or less. From the same point of view, the humidity is preferably 75% or more, more preferably 80% or more, and further preferably 90% or more. In addition, the initial relative humidity in the drying process can be set to 99% or less, or 97% or less. After drying for a certain period of time in an atmosphere with an initial relative humidity of 70% or more, drying in the atmosphere after a certain period of time will promote drying, so it is preferred. The process of maintaining an initial relative humidity of 70% or more is also called aging treatment. The aging treatment time is preferably 3 to 48 hours, more preferably 5 to 30 hours.
[0085] In the drying step, the sample is dried until its water content reaches 2% to 15% by mass, thereby obtaining a solid portion of titanium oxide. The obtained solid portion of the oxide is pulverized in a mortar or the like to obtain titanium oxide powder.
[0086] <3. Method 2 for producing titanium oxide powder>
[0087] Next, as Production Method 2, a method for producing titanium oxide powder using an ammonium compound as an additive to a titanium tetrachloride aqueous solution will be described.
[0088] A titanium oxide powder production method (Production Method 2) according to another embodiment of Production Method 1 of the present invention includes: a synthesis step of mixing an aqueous solution containing an ammonium compound and an aqueous solution containing titanium tetrachloride with a pH of less than 3 so that the ammonium compound [mol] / Ti [mol] (molar ratio) is 0.001 to 0.029, thereby precipitating titanium oxide; and a drying step of drying the resulting titanium oxide in an atmosphere with an initial relative humidity of 70 to 100% to powderize the mixture. The initial relative humidity in the drying step is preferably 70% or higher. This titanium oxide powder production method differs from the titanium oxide powder production method of the aforementioned embodiment (Production Method 1) in terms of the synthesis step conditions. In this titanium oxide powder production method, steps other than the synthesis step can be the same as those of the titanium oxide powder production method of the aforementioned embodiment. That is, in Production Method 2, one or both of a purification step and a dehydration step can be performed between the synthesis step and the drying step. Preferred conditions for the purification step, dehydration step, and drying step may be the same as those in Production Method 1. The following describes conditions for the synthesis step of the titanium powder production method of this embodiment that differ from those in Production Method 1.
[0089] The ammonium compound acts as a reaction inhibitor. Adding the ammonium compound stabilizes the formation of titanium oxide particles, suppressing phase transition to the rutile phase and aggregation. Preferred ammonium compounds include ammonia, ammonium chloride, and ammonium carbonate, with ammonium carbonate being particularly preferred. Ammonium carbonate is easily adjusted to the desired pH value, enabling the production of titanium oxide powder under ideal conditions.
[0090] Regarding the content of ammonium compound in the aqueous solution (mixed solution) obtained by mixing an aqueous solution containing an ammonium compound and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3, the ratio of the amount of substance of the ammonium compound in the mixed solution to the amount of substance of Ti (ammonium compound [mol] / Ti [mol]) is preferably 0.001 or more. This is to make the speed of the hydrolysis reaction sufficiently low and suppress the phase transition to the rutile phase as a stable phase. From the viewpoint of further suppressing the phase transition to the rutile phase, the above-mentioned amount ratio is more preferably 0.005 or more, and further preferably 0.013 or more. The above-mentioned amount ratio (ammonium compound [mol] / Ti [mol]) is preferably 0.029 or less. This is to prevent the hydrolysis reaction from being excessively suppressed. From the same viewpoint, it is further preferably 0.020 or less.
[0091] <4. Method 3 for producing titanium oxide powder>
[0092] Next, as Production Method 3, a method for producing titanium oxide powder using an aqueous solution containing an inorganic acid as an additive to the titanium tetrachloride aqueous solution will be described.
[0093] One embodiment of the present invention relates to a method for producing titanium oxide powder, which differs from Methods 1 and 2. The method comprises: a synthesis step of mixing an aqueous solution containing an inorganic acid and an aqueous solution containing titanium tetrachloride with a pH of less than 3 so that the inorganic acid [mol] / Ti [mol] (molar ratio) is 0.001 to 0.030, thereby precipitating titanium oxide; and a drying step of drying the resulting titanium oxide in an atmosphere with an initial relative humidity of 70 to 100% to powderize the mixture. The initial relative humidity in the drying step is preferably 70% or higher, more preferably 75% or higher, and even more preferably 80% or higher. The method for producing titanium oxide powder in this embodiment differs from the method for producing titanium oxide powder in the aforementioned embodiment (Method 1) in terms of the synthesis step conditions. In this method for producing titanium oxide powder, steps other than the synthesis step can be the same as those in the aforementioned method for producing titanium oxide powder. Specifically, in Method 3, one or both of a purification step and a dehydration step can be performed between the synthesis step and the drying step. Preferred conditions for the purification step, dehydration step, and drying step may be the same as those in Production Method 1. The following describes conditions for the synthesis step of the titanium oxide powder production method of this embodiment that differ from those in Production Method 1.
[0094] <4-1. Synthesis Step>
[0095] The pH of the aqueous solution containing titanium tetrachloride is less than 3. This is to allow the hydrolysis reaction to proceed advantageously. Furthermore, the pH is more preferably 2 or less, and even more preferably 1 or less.
[0096] The inorganic acid stabilizes the surface of the generated titanium oxide particles by adhering to them, acting as a phase transition inhibitor that suppresses the phase transition from the anatase phase to the rutile phase. The inorganic acid modifies the titanium oxide surface. Furthermore, it also has the effect of suppressing the aggregation of particles. The inorganic acid is preferably a strong inorganic acid, and sulfuric acid (molecular weight 98.08) is preferred from the perspective of suppressing the phase transition to the rutile phase.
[0097] The molecular weight of the inorganic acid is preferably 300 or less. If an excessively high molecular weight inorganic acid is added, then relative to the titanium oxide precipitated, the molecules of the inorganic acid are large, so it is difficult to uniformly modify the titanium oxide surface, and sometimes the particles are not fully dispersed. In such a case, it is possible to cause the particles to condense with each other and to undergo a phase transition to the rutile phase with the condensation surface as a starting point. By making the molecular weight of the inorganic acid be 300 or less, the inorganic acid can uniformly modify the titanium oxide surface and improve the dispersibility of the particles. From the same viewpoint, the molecular weight of the inorganic acid is preferably 250 or less, more preferably 200 or less. In addition, the molecular weight of the inorganic acid is, for example, more than 30.
[0098] The Ti concentration in the mixed solution obtained by mixing an aqueous solution containing an inorganic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 is preferably 0.01 mol / L or higher. This is to facilitate the hydrolysis reaction. From the same viewpoint, the Ti concentration is more preferably 0.05 mol / L or higher, and even more preferably 0.30 mol / L or higher.
[0099] The Ti concentration in the mixed solution is preferably 2.00 mol / L or less. This is to suppress the phase transition to the rutile phase. From the same viewpoint, it is more preferably 1.50 mol / L or less, and even more preferably 1.00 mol / L or less.
[0100] About the content of the acidic compound in the mixed solution obtained by mixing an aqueous solution comprising an inorganic acid and an aqueous solution comprising titanium tetrachloride and having a pH value less than 3, the ratio of the amount of substance of the inorganic acid to the amount of substance of titanium (inorganic acid [mol] / Ti [mol]) (molar ratio) is 0.001 or more and 0.037 or less. This is to suppress the phase transition from the anatase phase to the rutile phase. From the same viewpoint, it is more preferably 0.010 or more, and further preferably 0.015 or more. The ratio of the amount of the above-mentioned substance (inorganic acid [mol] / Ti [mol]) is preferably 0.030 or less. This is because, if the inorganic acid is added in excess, it is easy to cause reaction obstruction.
[0101] <5. Method 4 for producing titanium oxide powder>
[0102] Next, as Production Method 4, a method for producing titanium oxide powder using an aqueous solution containing an organic acid as an additive to an aqueous titanium tetrachloride solution will be described.
[0103] The method for producing titanium oxide powder according to this embodiment differs from the method for producing titanium oxide powder according to the above embodiment (production method 1) in terms of the conditions of the synthesis process. In the method for producing titanium oxide powder according to this embodiment, the processes other than the synthesis process can be the same as those in the method for producing titanium oxide powder according to the above embodiment. That is, in production method 3, one or both of the refining process and the dehydration process can be performed between the synthesis process and the drying process. In addition, the preferred conditions for the refining process, the dehydration process, and the drying process can also be the same as those in production method 1. The following describes the conditions of the synthesis process in the method for producing titanium oxide powder according to this embodiment that are different from those in production method 1.
[0104] One embodiment of the present invention relates to a method for producing titanium oxide powder, which differs from methods 1 to 3. The method comprises a synthesis step and a drying step. In the synthesis step, an aqueous solution containing an organic acid and an aqueous solution containing titanium tetrachloride having a pH of less than 3 are mixed so that the molar ratio of acidic functional groups of the organic acid [mol] / Ti [mol] is 0.001 to 0.037, thereby precipitating titanium oxide. In the drying step, the obtained titanium oxide is dried and powdered in an atmosphere having an initial relative humidity of 70 to 100%. The initial relative humidity in the drying step is preferably 70% or higher, more preferably 75% or higher, and even more preferably 80% or higher.
[0105] <5-1. Synthesis Step>
[0106] The pH of the aqueous solution containing titanium tetrachloride is less than 3. This is to allow the hydrolysis reaction to proceed advantageously. Furthermore, the pH is more preferably 2 or less, and even more preferably 1 or less.
[0107] The organic acid stabilizes the surface of the generated titanium oxide particles by adhering to them, acting as a phase transition inhibitor that inhibits the phase transition from the anatase phase to the rutile phase. It also has the effect of inhibiting the aggregation of particles. The organic acid is preferably an α-hydroxycarboxylic acid, and from the perspective of inhibiting the phase transition to the rutile phase, malic acid (molecular weight 134.09) and citric acid (molecular weight 192.12) are more preferred.
[0108] For the same reasons as inorganic acid, the molecular weight of the organic acid is preferably below 300. That is, if an organic acid with excessively high molecular weight is added, then relative to the titanium oxide particles precipitated, the molecules of the acidic compound are large, so it is difficult to uniformly modify the titanium oxide surface, and sometimes the particles are not fully dispersed. In such a case, on the contrary, the particles are condensed with each other and the phase transition to the rutile phase is carried out with the condensation surface as the starting point. By making the molecular weight of the organic acid be below 300, the organic acid can uniformly modify the titanium oxide surface, improve the dispersibility of the particles. From the same viewpoint, the molecular weight of the acidic compound is preferably below 250, more preferably below 200. In addition, the molecular weight of the organic acid is, for example, more than 30, preferably more than 40.
[0109] The Ti concentration in the mixed solution obtained by mixing an aqueous solution containing an organic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 is preferably 0.01 mol / L or higher. This is to facilitate the hydrolysis reaction. From the same viewpoint, the Ti concentration is more preferably 0.05 mol / L or higher, and even more preferably 0.30 mol / L or higher.
[0110] The Ti concentration is preferably 2.00 mol / L or less. This is to suppress the phase transition to the rutile phase. From the same viewpoint, it is more preferably 1.50 mol / L or less, and even more preferably 1.00 mol / L or less.
[0111] With regard to the content of the acidic functional groups of the organic acid in the mixed solution obtained by mixing an aqueous solution containing an organic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3, the ratio of the amount of substance of the acidic functional groups of the organic acid in the mixed solution to the amount of substance of Ti (acidic functional groups of organic acid [mol] / Ti [mol]) (molar ratio) is preferably 0.001 or more and 0.037 or less. This is to suppress the phase transition from the anatase phase to the rutile phase. From the same viewpoint, it is more preferably 0.010 or more, and further preferably 0.015 or more. The above-mentioned ratio of the amount of substance (amount of substance of the acidic functional groups of organic acid [mol] / Ti [mol]) is preferably 0.037 or less. This is because if the organic acid is added in a very excessive amount, it is easy to cause reaction obstruction. From the same viewpoint, it is further preferably 0.030 or less.
[0112] Here, the amount of the substance containing the acidic functional groups of the organic acid in the mixed solution refers to the sum of the amounts of the substance containing the acidic functional groups of the organic acid contained in the mixed solution. For example, if the organic acid contained in the mixed solution is only 1 mol of citric acid, since citric acid has three acidic functional groups, the amount of the substance containing the acidic functional groups of the organic acid in the mixed solution is 3 mol.
[0113] According to the above embodiment, anatase-type titanium oxide is synthesized by hydrolyzing titanium tetrachloride in the presence of a dispersant such as urea, ammonium compounds, inorganic acids, and organic acids, and the synthesized titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100%. This can inhibit the dense aggregation and particle growth of the particles, and obtain a dry powder without inactivating the hydroxyl groups on the surface of the particles, thereby providing anatase-type titanium oxide powder with a high specific surface area, high affinity with solvents, and high dispersibility.
[0114] Example
[0115] Hereinafter, examples and comparative examples of the present invention will be described, but they do not limit the technical scope of the present invention.
[0116] <Example 1>
[0117] To an aqueous titanium tetrachloride solution (pH: 0.8) with a Ti concentration of 15% by mass (titanium tetrachloride concentration of 59% by mass) maintained at 20°C was added an aqueous urea solution adjusted to a pH of 11 with aqueous ammonia, yielding a mixed solution having a Ti molar concentration of 0.096 mol / L and a urea molar ratio of 0.026. The solution temperature was maintained at 20°C throughout this preparation step.
[0118] Next, the mixed solution was transferred to a glass reactor.
[0119] Next, while the mixed liquid was stirred at 60 rpm using a stirrer, the temperature was raised to 60° C. using an external heater at a temperature increase rate of 0.4° C. / min and maintained at that temperature for 30 minutes.
[0120] Then, the reaction solution was naturally cooled to room temperature (25° C.) to obtain a slurry.
[0121] The naturally cooled slurry was neutralized with aqueous ammonia, filtered and recovered using an ultrafiltration membrane ("Microsa UF (registered trademark)" manufactured by Asahi Kasei Corporation), and washed with ion-exchanged water.
[0122] The washed slurry was dehydrated using a filter press to a solid content of 30% by mass.
[0123] The titanium oxide solid obtained by dehydration was placed in a container set to an air atmosphere with an initial relative humidity of 80%, aged for 24 hours, and then dried in the air to a moisture content of 10% by mass to obtain a titanium oxide solid component. This solid component was pulverized in a mortar to obtain titanium oxide powder.
[0124] <Example 2>
[0125] Titanium oxide powder was obtained under the same conditions as in Example 1 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the urea amount [mol] / Ti amount [mol] became 0.042.
[0126] <Example 3>
[0127] Titanium oxide powder was obtained under the same conditions as in Example 1 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the urea amount [mol] / Ti amount [mol] became 0.053.
[0128] <Example 4>
[0129] An aqueous solution of ammonium carbonate adjusted to a pH of 11 was added to an aqueous titanium tetrachloride solution (pH 0.8) having a Ti concentration of 15% by mass (titanium tetrachloride concentration of 59% by mass) maintained at 20°C, thereby obtaining a mixed solution having a Ti molar concentration of 0.096 mol / L and a ratio of the amount of ammonium compound (mol) to the amount of Ti (mol) of 0.010. During this preparation step, the solution temperature was always maintained at 20°C.
[0130] Next, the mixed solution was transferred to a glass reactor.
[0131] The mixture was then heated to 60°C at a rate of 0.4°C / min using an external heater while being stirred at 60 rpm. The temperature was then maintained at 60°C for 30 minutes. The reaction mixture was then cooled to room temperature (25°C) to obtain a slurry.
[0132] Next, the naturally cooled slurry was neutralized with aqueous ammonia, filtered and recovered using an ultrafiltration membrane ("Microsa UF (registered trademark)" manufactured by Asahi Kasei Corporation), and washed with ion-exchanged water.
[0133] The washed slurry was dehydrated using a filter press to a solid content of 30% by mass.
[0134] The titanium oxide solid obtained by dehydration was placed in a container set to an air atmosphere with an initial relative humidity of 80%, aged for 24 hours, and then dried in the air to a moisture content of 10% by mass to obtain a titanium oxide solid component. This solid component was pulverized in a mortar to obtain titanium oxide powder.
[0135] <Example 5>
[0136] Titanium oxide powder was obtained under the same conditions as in Example 4 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the amount of substance of the ammonium compound [mol] / the amount of substance of Ti [mol] became 0.016.
[0137] <Example 6>
[0138] Aqueous sulfuric acid solution was added to an aqueous titanium tetrachloride solution (pH: 0.7) having a Ti concentration of 15% by mass (titanium tetrachloride concentration of 59% by mass) maintained at 20°C, to prepare a mixed solution having a Ti molar concentration of 0.074 mol / L and a ratio of the amount of inorganic acid (mol) to the amount of Ti (mol) of 0.026. The solution temperature was maintained at 20°C throughout this preparation step.
[0139] Next, the mixed solution was transferred to a glass reactor.
[0140] The mixture was then heated to 80°C at a rate of 0.2°C / min using an external heater while being stirred at 60 rpm. The temperature was then maintained at 80°C for 30 minutes. The reaction mixture was then cooled to room temperature (25°C) to obtain a slurry.
[0141] Next, the naturally cooled slurry was neutralized with aqueous ammonia, filtered and recovered using an ultrafiltration membrane ("Microsa UF (registered trademark)" manufactured by Asahi Kasei Corporation), and washed with ion-exchanged water.
[0142] Next, the washed slurry was dehydrated using a filter press to a solid content of 30% by mass.
[0143] Next, the titanium oxide solid obtained by dehydration was placed in a container set to an air atmosphere with an initial relative humidity of 80%, aged for 24 hours, and then dried in the atmosphere to a moisture content of 10% by mass to obtain a titanium oxide solid component. This solid component was pulverized in a mortar to obtain titanium oxide powder.
[0144] <Example 7>
[0145] Titanium oxide powder was obtained under the same conditions as in Example 6 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the inorganic acid amount [mol] / Ti amount [mol] became 0.027.
[0146] <Example 8>
[0147] Titanium oxide powder was obtained under the same conditions as in Example 6 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the inorganic acid amount [mol] / Ti amount [mol] became 0.029.
[0148] <Example 9>
[0149] In the preparation step, a citric acid aqueous solution was used instead of sulfuric acid, and the mixed solution was prepared so that the Ti molar concentration was 0.074 mol / L and the amount of substance of the acidic functional group of the organic acid [mol] / the amount of substance of Ti [mol] was 0.022. In addition, the initial relative humidity of the container when the titanium oxide solid obtained by dehydration was dried to obtain the solid component of titanium oxide was changed to 95%. Titanium oxide powder was obtained by the same method as in Example 6, except that the above methods were repeated.
[0150] <Example 10>
[0151] Titanium oxide powder was obtained under the same conditions as in Example 9 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the amount of substance of the acidic functional group of the organic acid [mol] / the amount of substance of Ti [mol] became 0.034.
[0152] <Example 11>
[0153] Titanium oxide powder was obtained by the same method as in Example 9, except that malic acid was used instead of citric acid in the preparation step, and the mixed solution was prepared so that the Ti molar concentration was 0.074 mol / L and the amount of substance of the acidic functional group of the organic acid [mol] / the amount of substance of Ti [mol] was 0.026.
[0154] <Example 12>
[0155] Titanium oxide powder was obtained under the same conditions as in Example 11 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the amount of substance of the acidic functional group of the organic acid [mol] / the amount of substance of Ti [mol] became 0.036.
[0156] <Comparative Example 1>
[0157] Titanium oxide powder was obtained in the same manner as in Example 1 except that the urea aqueous solution was not used in the preparation step and that a titanium tetrachloride aqueous solution (Ti molar concentration: 0.096 mol / L) having a Ti concentration of 15 mass % (titanium tetrachloride concentration: 59 mass %) was used instead of the mixed solution.
[0158] <Comparative Example 2>
[0159] Titanium oxide powder was obtained under the same conditions as in Example 1 except that the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution did not change and the urea amount [mol] / Ti amount [mol] became 0.063.
[0160] <Comparative Example 3>
[0161] Titanium oxide powder was obtained under the same conditions as in Example 4, except that the titanium tetrachloride aqueous solution used for mixing was changed to a titanium tetrachloride aqueous solution having a pH of 0.9, and the conditions of the preparation step were changed so that the Ti molar concentration in the mixed solution remained unchanged and the amount of substance of the ammonium compound [mol] / the amount of substance of Ti [mol] became 0.033.
[0162] <Comparative Example 4>
[0163] In the preparation step, the same method as in Example 6 was used to obtain titanium oxide powder, except that no urea aqueous solution was used, and a titanium tetrachloride aqueous solution (Ti molar concentration: 0.074 mol / L) with a Ti concentration of 15 mass% (titanium tetrachloride concentration: 59%) was used instead of the mixed liquid. In addition, the initial relative humidity of the container when the titanium oxide solid obtained by dehydration was wet-dried to obtain the solid component of titanium oxide was changed to 80%.
[0164] <Comparative Example 5>
[0165] Titanium oxide powder was obtained under the same conditions as in Example 6 except that the initial relative humidity of the container was changed to 0% when the titanium oxide solid obtained by dehydration was dried to obtain the titanium oxide solid component. That is, in Comparative Example 5, the titanium oxide solid obtained by dehydration was dry-dried.
[0166] <Comparative Example 6>
[0167] Titanium oxide powder was obtained under the same conditions as in Example 6 except that the initial relative humidity of the container when the titanium oxide solid obtained by dehydration was wet-dried to obtain the titanium oxide solid component was changed to 30%.
[0168] <Comparative Example 7>
[0169] Titanium oxide powder was obtained under the same conditions as in Example 6, except that the conditions of the preparation process were changed so that the Ti molar concentration in the mixed liquid did not change and the amount of substance of the inorganic acid [mol] / the amount of substance of Ti [mol] became 0.031. In addition, the initial relative humidity of the container when the titanium oxide solid obtained by dehydration was wet-dried to obtain the solid component of titanium oxide was changed to 80%.
[0170] <Comparative Example 8>
[0171] Titanium oxide powder was obtained in the same manner as in Example 9 except that the citric acid aqueous solution was not used in the preparation step and that a titanium tetrachloride aqueous solution (Ti molar concentration 0.096 mol / L) having a Ti concentration of 15 mass % (titanium tetrachloride concentration 59%) was used instead of the mixed solution.
[0172] <Comparative Example 9>
[0173] Titanium oxide powder was obtained under the same conditions as in Example 9 except that the initial relative humidity of the container when the titanium oxide solid obtained by dehydration was dried to obtain the titanium oxide solid component was changed to 0%.
[0174] <Comparative Example 10>
[0175] When obtaining the solid component of titanium oxide by drying the titanium oxide solid obtained by dehydration, the initial relative humidity of the container was changed to 30%, and titanium oxide powder was obtained under the same conditions as in Example 9 except for this.
[0176] <Comparative Example 11>
[0177] The conditions of the preparation process were changed so that the Ti molar concentration in the mixed solution remained unchanged and the amount of substance [mol] of the acidic functional group of the organic acid / the amount of substance [mol] of Ti became 0.038. Except for this, titanium oxide powder was obtained under the same conditions as in Example 9.
[0178] <Comparative Example 12>
[0179] When obtaining the solid component of titanium oxide by drying the titanium oxide solid obtained by dehydration, the initial relative humidity of the container was changed to 0%, and titanium oxide powder was obtained under the same conditions as in Example 11 except for this.
[0180] <Comparative Example 13>
[0181] When obtaining the solid component of titanium oxide by drying the titanium oxide solid obtained by dehydration, the initial relative humidity of the container was changed to 30%, and titanium oxide powder was obtained under the same conditions as in Example 11 except for this.
[0182] <Comparative Example 14>
[0183] The conditions of the preparation process were changed so that the Ti molar concentration in the mixed solution remained unchanged and the amount of substance [mol] of the acidic functional group of the organic acid / the amount of substance [mol] of Ti became 0.045. Except for this, titanium oxide powder was obtained under the same conditions as in Example 11.
[0184] The production conditions of the titanium oxide powders of the above Examples 1 to 12 and Comparative Examples 1 to 14 are summarized in Table 1. In Table 1, in the comparative examples where the additive type is indicated by "-", no additive was used, and an aqueous titanium tetrachloride solution was used instead of the mixed solution. For the sake of convenience in explanation, Comparative Example 1 is described at multiple places as the same experimental data.
[0185] The same applies to Comparative Example 7.
[0186] <第
[0187] For the titanium oxide powders of the above Examples 1 to 12 and Comparative Examples 1 to 14, the following evaluation methods were used for evaluation.
[0188] <BET specific surface area>
[0189] The specific surface area of titanium oxide powder was calculated from nitrogen adsorption-desorption curves using the BET method according to JIS Z8830:2013. The specific surface area (BET specific surface area) was measured using a Quantachrome QUADRASORV evo, after pretreatment by heating the sample to 180°C and flowing nitrogen for 20 minutes. The BET method was applied within a range of P / P0 = 0.00 to 0.95.
[0190] <Anatase Content, Rutile Content>
[0191] Powder X-ray diffraction analysis of titanium oxide powder was performed to calculate the anatase content based on the peak intensity corresponding to anatase crystals (Ia), the peak intensity corresponding to brookite crystals (Ib), and the peak intensity corresponding to rutile crystals (Ir). The anatase content (anatase ratio) of the titanium oxide powder's crystalline phase was calculated using the following formula.
[0192] Anatase content [%] = {Ia / (Ia+Ib+Ir)}×100
[0193] In addition, the rutile content (Rutile ratio) of the crystal phase of the titanium oxide powder was calculated using the following formula.
[0194] Rutile content [%] = {Ir / (Ia+Ib+Ir)}×100
[0195] Powder X-ray diffraction measurement was performed using SmartLab SE manufactured by Rigaku Corporation, using Cu-Kα1 radiation with a copper target, under the conditions of tube voltage 45 kV, tube current 40 mA, measurement range 2θ = 20 to 35 [deg], sampling width 0.0167 [deg], and scanning speed 0.0192 [deg / s].
[0196] Ia: Intensity of the peak corresponding to anatase crystal (2θ = 24.5° to 26.0°)
[0197] Ir: Intensity of the peak corresponding to rutile crystals (2θ = 26.6° to 28.1°)
[0198] Ib: Intensity of the peak corresponding to brookite crystals (2θ = 30.8° to 32.3°)
[0199] <Half-value width of diffraction peak in crystallinity X-ray diffraction measurement>
[0200] For titanium oxide powder, SmartLab SE manufactured by Rigaku Corporation was used, using Cu-Kα1 radiation with a copper target, under the conditions of tube voltage 45 kV, tube current 40 mA, measurement range 2θ = 24.5 to 26.0 [deg], sampling width 0.0167 [deg], and scanning speed 0.0192 [deg / s] to analyze the FWHM of the main peak of the anatase phase near 2θ = 25°.
[0201] During analysis, the diffraction pattern of the sample was corrected by measuring the background when only the glass cell was present and subtracting the background diffraction intensity from the diffraction intensity measured using a sample containing titanium oxide and the glass cell.
[0202] <Spin-spin relaxation time>
[0203] A slurry containing 5% by mass of titanium oxide was prepared using ion-exchanged water and filled into a Dispo NMR sample tube AS1NMR manufactured by Aswan Co., Ltd. Immediately after the slurry was filled into the sample tube, pulsed NMR measurement was performed using an Acorn Area manufactured by XiGo Nanotools.
[0204] The spin-spin relaxation time T2 of the titanium oxide powder was measured by pulse NMR measurement. The measurement was performed under the following conditions.
[0205] Measurement frequency: 13.1 MHz, measurement core: irradiation with a 90° single pulse followed by irradiation with a 180° pulse at 0.5 mS intervals, repeated four times. Measurement method: CPMG pulse sequence method, sample volume: 0.5 ml, temperature: 23°C, specific surface relaxation (Ka): 0.0075 g / m 2 / ms.
[0206] <Elemental Analysis>
[0207] Ti, Cl, Si, Al, and Fe in the raw materials were measured by mixing the sample with an aqueous hydrogen fluoride solution, completely dissolving the sample using the Microwave Sample Pretreatment System ETHOS EASY manufactured by Microstone Zeneral Co., Ltd., and then using the Hitachi Z-2300 atomic absorption spectrometer. The Ti, Cl, Si, Al, and Fe contents in the finished titanium oxide powder were similarly measured by mixing the sample with an aqueous hydrogen fluoride solution, completely dissolving the sample in the solution, and then using the same system.
[0208] C (carbon) and S (sulfur) in the titanium oxide powder were measured using a carbon-sulfur analyzer CS744 (manufactured by LECO Corporation).
[0209] <Moisture content measurement>
[0210] Using the MX50 heating and drying type moisture meter manufactured by A&D Company, after raising the temperature of 2 g of titanium oxide powder to 200 °C, infrared heating was carried out at 120 °C until the weight change became 0.01 mass% or less to measure the moisture content of the titanium oxide powder.
[0211] <Zeta potential measurement>
[0212] Ion-exchanged water was used to prepare a slurry with 0.1 mass% titanium oxide. It was filled into a sapphire cell, and the Zeta potential of this slurry was measured using the ELZ-2000 manufactured by Otsuka Electronics Co., Ltd.
[0213]
[0214] Table 2 is a table summarizing the physical properties of the titanium oxide powders of Examples 1 to 12 and Comparative Examples 1 to 14. In the content rates in Table 2, where the symbol "<" is used, it indicates less than the value immediately following "<". For example, the Fe content rate of Comparative Example 1 is less than 0.002 mass%.
[0215] As shown in Table 2, for the titanium oxide powders of Examples 1 to 12, the absolute value of the Zeta potential is 42 to 63 mV. In this range, the dispersion of titanium oxide is good and it does not become over-dispersed, and poor flow does not occur. Therefore, it is suitable for the synthesis of dielectric materials and battery materials.
[0216] On the other hand, for the titanium oxide powders of Comparative Examples 1 to 6 and Comparative Examples 8 to 13, the absolute value of the Zeta potential is 39 mV or less. It is known that if the absolute value of the Zeta potential is small, the dispersion is poor and the particles are likely to aggregate, and the dispersion of these titanium oxides is poor. For the titanium oxide powders of Comparative Examples 7 and Comparative Examples 14, the absolute value of the Zeta potential is 66 mV or more. It is known that if the absolute value of the Zeta potential is too large, it becomes over-dispersed and the viscosity of the dispersion liquid rises too much, thus causing poor flow. These titanium oxides are, for example, not suitable for use as a raw material for barium titanate in synthesis.
[0217] In addition, the spin-spin relaxation time T2 of Examples 1 to 12 and Comparative Examples 1 to 14 was compared, and it was confirmed that: in Examples 1 to 14, the spin-spin relaxation time was 42 to 99 ms, and when re-slurrying was carried out to prepare a dispersion liquid, titanium oxide powder that did not become over-dispersed was produced.
[0218] Through the comparison of the above Examples and Comparative Examples, it was confirmed that: according to the present invention, it is possible to provide anatase-type titanium oxide powder with a high specific surface area and high dispersibility.
Claims
1. A titanium oxide powder having a BET specific surface area of 300 m2 as measured by nitrogen adsorption. 2 / g and above 480m 2 / g or less, the anatase content of the crystalline phase measured by XRD measurement is 90% or more, and the spin-spin relaxation time T2 measured by pulse NMR on a 5 mass % suspension prepared using ion-exchanged water is 46 ms or more and 103 ms or less.
2. The titanium oxide powder according to claim 1, The carbon content is 0.5 mass% or less.
3. The titanium oxide powder according to claim 1 or 2, The chlorine content is 0.1 mass % or less, the silicon content is 0.1 mass % or less, and the sulfur content is 0.1 mass % or less.
4. The titanium oxide powder according to claim 1 or 2, The half-value width of the diffraction peak at a diffraction angle 2θ of 24.5° to 26.0° is 1.10° to 2.00°.
5. The titanium oxide powder according to claim 1 or 2, It has a zeta potential of not less than -63 mV and not more than -40 mV.
6. A method for producing titanium oxide powder, comprising: A synthesis step of mixing an aqueous solution containing urea and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the urea / Ti molar ratio is 0.001 to 0.058, thereby precipitating titanium oxide; and The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100%, and then subjected to a heat treatment step for powderization.
7. A method for producing titanium oxide powder, comprising: A synthesis step of mixing an aqueous solution containing an ammonium compound and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the ammonium compound / Ti molar ratio is 0.001 to 0.029, and precipitating titanium oxide; and The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
8. The method for producing titanium oxide powder according to claim 6 or 7, The pH of the aqueous solution containing at least any one of urea and the ammonium compound is less than 12.
0.
9. A method for producing titanium oxide powder, comprising: A synthesis step of mixing an aqueous solution containing an inorganic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the inorganic acid / Ti molar ratio is 0.001 to 0.030, thereby precipitating titanium oxide; and The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
10. A method for producing titanium oxide powder, comprising: A synthesis step of mixing an aqueous solution containing an organic acid and an aqueous solution containing titanium tetrachloride and having a pH value of less than 3 so that the molar ratio of the acidic functional group of the organic acid to Ti is 0.001 to 0.037, thereby precipitating titanium oxide; and The obtained titanium oxide is dried in an atmosphere with an initial relative humidity of 70 to 100% and subjected to a drying step for powdering.
11. The method for producing titanium oxide powder according to claim 10, The organic acid is an α-hydroxycarboxylic acid.
12. The method for producing titanium oxide powder according to any one of claims 9 to 11, The molecular weight of the organic acid or inorganic acid in the aqueous solution is 300 or less.
13. The method for producing titanium oxide powder according to any one of claims 9 to 11, The method further includes a purification step of purifying titanium oxide using at least one of an ultrafiltration membrane, a reverse osmosis membrane, an ion exchange resin, and an electrodialysis membrane.
Citation Information
Patent Citations
Method for producing titanate nanosheet dispersion liquid
JP2008247712A
Organosiloxane oligomer-modified inorganic oxide ultrafine particles
JP2010095392A
Titanium oxide-containing coating composition and coated article
JP2015212355A
Titanium oxide and method of producing the same
CN108367938A
Highly heat-resistant anatarse-type titanium oxide and method for producing same
CN113874325A