Graphene-diamond composite coating and preparation method thereof

By depositing a transition metal layer on the surface of a diamond coating and reacting it with liquid gallium, an intermetallic compound is generated, forming a graphene structure with both horizontal and vertical orientations. This solves the problems of weak interfacial bonding and high thermal resistance of graphene-diamond composite coatings under high load and high temperature environments, thereby improving friction performance and service life.

CN121046809AActive Publication Date: 2025-12-02NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202511605709.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-05
Publication Date
2025-12-02
Estimated Expiration
2045-11-05

AI Technical Summary

Technical Problem

Existing graphene-diamond composite coatings suffer from weak interfacial adhesion and high interfacial thermal resistance under high load and high temperature environments, which limits their service life and performance in high-load mechanical components, high-conductivity electrical contacts, and high-power heat dissipation substrates.

Method used

A transition metal layer is deposited on the diamond coating surface, and a Ni or Cu layer is formed by magnetron sputtering. The layer is then reacted with liquid gallium under vacuum annealing to generate an intermetallic compound, which improves the interfacial bonding force and promotes the growth of graphene, forming a graphene structure with both horizontal and vertical orientations.

Benefits of technology

The frictional properties of the graphene-diamond composite coating were improved, the coefficient of friction and wear rate were reduced, and the service life and wear resistance in seawater environment were enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121046809A_ABST
    Figure CN121046809A_ABST
Patent Text Reader

Abstract

The invention discloses a graphene-diamond composite coating and a preparation method thereof.The preparation method of the graphene-diamond composite coating comprises the steps that grinding and roughening treatment is conducted on the surface of a substrate, ultrasonic crystal planting is conducted on the roughened substrate, and then a diamond coating is formed through a CVD method; depositing a transition metal layer on the surface of the diamond coating through a magnetron sputtering method, wherein the transition metal layer is a Ni layer or a Cu layer; and metal gallium is dropwise added to the transition metal layer, and then vacuum annealing treatment is carried out to obtain the graphene-diamond composite coating. By means of the preparation method, the graphene-diamond composite coating with the high tribological performance can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of diamond coating technology, specifically relating to a graphene-diamond composite coating and its preparation method. Background Technology

[0002] Diamond coatings are considered ideal surface protection materials due to their extremely high hardness, wear resistance, and excellent chemical inertness (resistance to acid and alkali corrosion). However, in actual service, their high hardness is often accompanied by high brittleness, leading to brittle fracture under extreme conditions (such as high contact stress or high temperature environments), which in turn causes abrasive wear. These limitations severely restrict the widespread application of diamond coatings in demanding marine tribology fields such as high load and high speed. Graphene, as a typical two-dimensional carbon material, has attracted much attention due to its high electron mobility, excellent mechanical properties, high thermal conductivity, good chemical stability, and excellent lubrication properties.

[0003] Studies have shown that graphene exhibits excellent lubrication properties in micro-friction. This is because, at the microscopic level, carbon atoms within graphene sheets can achieve lubrication through sp... 2 Hybridization forms a stable six-membered ring framework structure, while the interlayers are bound together by relatively weak van der Waals forces. This structural characteristic results in extremely low shear resistance to be overcome during interlayer slippage, endowing graphene with excellent lubrication properties at the atomic scale.

[0004] However, during macroscopic friction, due to the significantly increased contact area and complex and variable stress distribution, graphene is prone to overall peeling, wrinkling, or transfer to the surface of the grinding ball, leading to rapid failure of its lubrication function. This limitation severely restricts the practical application of graphene under macroscopic friction conditions. It is worth noting that when graphene is introduced as a lubricating phase into a diamond coating system during macroscopic friction, the two can complement each other: the high hardness of diamond provides a stable load-bearing matrix for graphene, preventing it from being crushed under high loads; while the layered lubrication effect of graphene can effectively reduce interfacial frictional resistance, solving the problem of the high friction coefficient of a single diamond coating. Therefore, in recent years, researchers have generally focused on introducing graphene into diamond coatings through various processes (such as chemical vapor deposition and metal catalysis) to achieve a synergistic effect of "high load-bearing capacity and low friction," expanding its application scope in the field of tribology.

[0005] Currently, the preparation methods for graphene-diamond composite coatings depend on whether transfer is required. The transfer method, as the mainstream technology for constructing horizontally oriented graphene-diamond (Gr-MCD) heterostructures, has a relatively low preparation cost. However, it is affected by impurities such as residual polymers and moisture at the interface during the transfer process, and the prepared Gr-MCD coating has inherent defects such as weak interfacial adhesion and high interfacial thermal resistance. This severely limits its service life and performance in high-load mechanical components, high-conductivity electrical contacts, and high-power heat dissipation substrates.

[0006] Patent application CN202411100326 discloses a graphene-diamond composite coating, its preparation method, and its application, belonging to the field of materials technology. This graphene-diamond composite coating comprises a diamond coating and a graphene coating; the graphene sp2 bond structure and the diamond sp3 bond structure are covalently bonded; the graphene coating has a predominantly vertical, non-parallel graphene structure. The small lattice mismatch between diamond and graphene avoids volume expansion caused by frictional heating; the diamond coating provides a support layer for the graphene and forms strong C / C covalent bonds at the interface, significantly improving the adhesion strength of the graphene; the graphene prevents brittle fracture of the diamond and significantly improves the lubrication performance of the diamond coating surface. This composite coating exhibits excellent wear resistance, a low coefficient of friction, and superior oxidation resistance, and remains stable under high temperature and high load working conditions, thereby improving the service life and processing efficiency of wear-resistant parts. However, the preparation method disclosed in the patent application has poor wettability and uniformity between the liquid metal and the diamond surface, resulting in some diamonds being exposed and affecting the friction performance. Summary of the Invention

[0007] This invention provides a method for preparing a graphene-diamond composite coating, which can produce a graphene-diamond composite coating with high tribological properties.

[0008] This invention provides a method for preparing a graphene-diamond composite coating, comprising: The substrate surface is roughened by grinding, crystals are ultrasonically implanted on the roughened substrate, and then a diamond coating is formed by CVD. A transition metal layer, which is a Ni layer, a Ti layer, or a Cu layer, is deposited on the surface of a diamond coating by magnetron sputtering. Gallium metal was dropped onto the transition metal layer, and then vacuum annealing was performed to obtain a graphene-diamond composite coating.

[0009] Preferably, the transition metal layer is a Ni layer. The Ni layer provided by this invention not only improves the wettability of liquid gallium but also promotes the transfer of carbon source to sp244 on the surface of the diamond (MCD) coating. 2Hybrid carbon conversion lays the structural foundation for graphene nucleation, and the introduction of the Ni layer significantly improves the solubility of carbon in liquid gallium. Sufficient dissolved carbon source meets the carbon requirements for graphene nucleation and growth, not only improving carbon conversion efficiency but also accelerating graphene growth rate. In summary, the introduction of a Ni transition layer onto the MCD coating surface not only improves the wettability of liquid Ga through interfacial reactions but also provides a catalytic effect and carbon source guarantee for graphene growth, ultimately creating favorable conditions for the controllable growth of graphene structures with both horizontal and vertical orientations.

[0010] More preferably, the vacuum annealing process is as follows: under an argon atmosphere, the annealing temperature is 1100-1300℃, and the holding time is 4-7 hours. This invention, by controlling the annealing temperature and holding time, allows the Ni layer to introduce more free carbon atoms to form horizontally oriented graphene. Simultaneously, more free carbon atoms can dissolve in liquid gallium metal, providing a sufficient carbon source for graphene nucleation and growth. This facilitates the continuous diffusion of free carbon atoms to the interface between liquid gallium metal and the intermetallic compound. When the carbon concentration reaches a supersaturated state, Ga atoms in the intermetallic compound phase can catalyze the growth of carbon atoms along a direction perpendicular to the substrate surface by regulating the carbon diffusion path and nucleation direction, forming vertically oriented graphene.

[0011] More preferably, the flow rate of the argon gas is 35-45 sccm.

[0012] Preferably, the substrate is made of ceramic, hard alloy, or high-temperature alloy.

[0013] More preferably, the ceramic is silicon carbide, silicon nitride, aluminum oxide, or zirconium oxide.

[0014] Preferably, before grinding and roughening the substrate surface, it is ultrasonically treated with acetone or ethanol solution for 10-20 minutes.

[0015] Preferably, the substrate surface is roughened sequentially on the diamond grinding wheel surfaces of W10 and W5.

[0016] Preferably, the ultrasonic implantation method includes: The roughened substrate was placed in a suspension of diamond powder / ethanol with a mass percentage of 5%-8% and subjected to ultrasonic oscillation treatment for 15-30 min. The diamond particle size was 50 nm-2 μm.

[0017] Preferably, the CVD method is any one of MPCVD, HFCVD, or DC-CVD, and the prepared diamond coating can be one or a combination of microcrystalline, nanocrystalline, or ultrafine nanocrystalline materials.

[0018] More preferably, the process for preparing micron-sized diamond includes: Four tantalum wires with a diameter of 0.35 mm were fixed to the substrate. The process parameters were precisely controlled as follows: methane flow rate 10–35 sccm, hydrogen flow rate 350–400 sccm, chamber pressure 1.8–2.5 kPa, hot filament temperature 1100–1300℃, and deposition time 6–10 h. An MCD coating was successfully deposited on the substrate surface.

[0019] Preferably, the method for preparing the transition metal layer includes: Using a 99.99% high-purity Ni target, the parameters of the magnetron sputtering method include: vacuum degree < 1 × 10⁻⁶. -4 Pa, power 100-150 W, gas pressure 0.8-1.5 Pa, argon flow rate 20 sccm-35 sccm, sputtering temperature maintained at 50-250℃, sputtering time 10 min-60 min; Alternatively, a 99.99% high-purity Cu target can be used, and the magnetron sputtering parameters include: vacuum degree < 1 × 10⁻⁶. -4 Pa, power 80-120 W, gas pressure 0.8-1.2 Pa, argon flow rate 15 sccm-30 sccm, sputtering temperature maintained at 0-150 ℃, sputtering time 5 min-75 min.

[0020] Preferably, after vacuum annealing, the obtained sample is placed in concentrated hydrochloric acid solution and left to stand for 4-7 hours to remove residual liquid gallium metal.

[0021] On the other hand, the present invention also provides a graphene-diamond composite coating, which is prepared by the method described above, wherein the graphene-diamond composite coating includes a horizontal graphene and a vertical graphene stacked structure.

[0022] Preferably, the vertical graphene is located on the horizontal graphene, and the height of the vertical graphene is 550-1000.

[0023] More preferably, the height of the vertical graphene is 700-1000.

[0024] The vertical graphene provided by this invention can be uniformly dispersed on the interface and has a high height, which minimizes the exposure of diamond, enhances friction performance, and minimizes the pear groove phenomenon.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention deposits a transition metal layer on the surface of a diamond coating. During the contact process, liquid gallium metal and the transition metal layer undergo an alloying reaction to generate an intermetallic compound. This intermetallic compound can effectively destroy the oxide layer on the surface of liquid gallium, while enhancing the interfacial bonding energy between liquid gallium and the diamond-transition metal substrate. This reduces the solid-liquid interfacial tension, optimizes wettability, and ensures more complete contact between the diamond-transition metal substrate and liquid gallium, thereby improving the conversion efficiency of graphene.

[0026] The graphene-diamond composite coating provided by this invention includes a horizontal graphene and vertical graphene cross structure. The graphene sheets in this structure achieve a more complete wrapping of the wear debris, that is, the graphene sheets tightly cover the surface of the wear debris, forming a composite structure similar to a "nano-scroll". This structure can promote the transformation of the friction interface from a pure sliding mode to a "sliding-rolling" hybrid mode, and further reduce the interface friction coefficient by replacing part of the sliding friction with rolling friction. Attached Figure Description

[0027] Figure 1 A flowchart illustrating the preparation method of the graphene-diamond composite coating provided in Example 1 of this invention; Figure 2 The diagrams show the wetting behavior of the MCD-Ni interface and the MCD interface with liquid gallium provided in Embodiment 1 of the present invention. Figure 2 (a) in the figure shows the wetting behavior of the MCD interface with liquid gallium. Figure 2 (b) in the figure shows the wetting behavior of the MCD-Ni interface with liquid gallium. Figure 3 The images show the surface morphology, cross-sectional morphology, and Raman spectra of Gr-MCD, Gr-MCD(Ga), and Gr-MCD(Ni,Ga) prepared in Example 1 of this invention; wherein, Figure 3 (a), (b), and (c) in the figure represent the surface morphology, cross-sectional morphology, and Raman spectrum of the Gr-MCD, respectively. Figure 3 In the figure, (d), (e) and (f) are the surface morphology, cross-sectional morphology and Raman spectrum of Gr-MCD(Ga), respectively; Figure 3 In the figure, (g), (h) and (i) are the surface morphology, cross-sectional morphology and Raman spectrum of Gr-MCD(Ni,Ga), respectively; Figure 4 The images show transmission images of Gr-MCD(Ga) and Gr-MCD(Ni,Ga) prepared in Example 1 of this invention, the interface structure diagram between the graphene layer and the diamond lattice, the growth morphology of graphene in the vertical direction, and a schematic diagram of the structure of Gr-MCD(Ni,Ga). Figure 4In the diagram, (a), (b), and (c) are the transmission spectrum of Gr-MCD(Ga), the interface structure between the graphene layer and the diamond lattice, and the growth morphology of graphene in the vertical direction, respectively. Figure 4 In the diagram, (d), (e), and (f) are the transmission spectrum of Gr-MCD(Ni,Ga), the interface structure between the graphene layer and the diamond lattice, and the growth morphology of graphene in the vertical direction, respectively. Figure 4 (g) in the figure is a schematic diagram of the structure of Gr-MCD(Ni,Ga); Figure 5 This is a schematic diagram illustrating the growth mechanism of the diamond-graphene composite coating prepared in Example 1 of the present invention. Figure 6 The graphs show the friction coefficient variation curves and wear performance diagrams for Gr-MCD, Gr-MCD(Ga), and Gr-MCD(Ni,Ga) prepared in Example 1 of this invention. Figure 6 (a) in the figure represents the curve showing the change in the coefficient of friction. Figure 6 (b) in the diagram is the wear performance diagram; Figure 7 The images show the overall morphology of the wear tracks, magnified SEM images of localized areas, and images of the wear marks on the Gr-MCD, Gr-MCD(Ga), and Gr-MCD(Ni,Ga) prepared in Example 1 of this invention after friction. Figure 7 Images (a), (b), and (c) in the figure show the overall morphology of the wear track after friction, a magnified SEM image of a local area, and an image of the wear scar on the wear pair using Gr-MCD. Figure 7 In the figure, (d), (e) and (f) are the overall morphology of the wear track of Gr-MCD(Ga) after friction, the magnified SEM image of a local area, and the wear mark image of the wear pair; Figure 7 In the figure, (g), (h) and (i) represent the overall morphology of the wear track of Gr-MCD(Ni,Ga) after friction, the magnified SEM image of a local area, and the wear mark image of the wear pair. Figure 8 A schematic diagram illustrating the friction mechanism of Gr-MCD and Gr-MCD(Ni,Ga) prepared in Example 1 of this invention. Figure 9 The images show the surface morphology, cross-sectional morphology, and Raman spectrum of the Gr-MCD (Cu,Ga) prepared in Example 2 of this invention; wherein, Figure 9 (a), (b), and (c) in the figure represent the surface morphology, cross-sectional morphology, and Raman spectrum of Gr-MCD(Cu,Ga), respectively. Detailed Implementation

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0029] Example 1 This embodiment provides a method for preparing a graphene-diamond composite coating, such as... Figure 1 As shown, it includes: Step 1: Preparation of the metallic diamond coating: Before preparing the graphene conversion coating, an MCD coating is first grown on a SiC substrate using an HFCVD device. The preparation process mainly includes the following steps: Substrate pretreatment: The surface of the SiC substrate is ground to increase the surface roughness and provide sufficient adhesion sites for subsequent diamond seed crystals.

[0030] Ultrasonic implantation: The polished SiC substrate is placed in a suspension of diamond powder and subjected to ultrasonic oscillation for 20 minutes. After treatment, the substrate surface is dried with high-purity nitrogen. This step aims to provide sufficient nucleation centers for uniform nucleation of the diamond coating.

[0031] HFCVD deposition of MCD coating: The SiC substrate after crystallization is placed in the HFCVD reaction chamber, and the gas mixture (CH4 / H2) is thermally decomposed by four parallel tantalum wires. The relevant deposition parameters are shown in Table 1.

[0032] Table 1: MCD Coating Deposition Parameters

[0033] Step 2: Preparation of diamond-graphene heterostructure coating: First, a nickel layer with a thickness of approximately 70 nm was deposited on the surface of a micron-sized diamond (MCD) coating using a magnetron sputtering device. The relevant deposition parameters are shown in Table 2.

[0034] Before graphene growth, the sample surface needs to be cleaned: it is ultrasonically treated in acetone, ethanol and deionized water for 10 minutes each, and then dried in a nitrogen stream.

[0035] After cleaning, the diamond-nickel composite coating is placed in a square ceramic boat, liquid gallium metal is added as a catalyst, and then the ceramic boat is transferred into a tube furnace for vacuum annealing.

[0036] The annealing process parameters were: argon (Ar) flow rate 40 sccm, annealing temperature 1200℃, and holding time 5 h. After annealing, the tube furnace was allowed to cool naturally to room temperature. The sample was then removed and placed in a concentrated hydrochloric acid solution at 80℃ for 8 h to remove residual liquid metal from the surface, finally obtaining the target product Gr-MCD (Ni, Ga) coating.

[0037] Table 2: Ni coating deposition parameters

[0038] Field emission scanning electron microscopy (FESEM) and energy-dispersive X-ray spectroscopy (EDS) were used to comprehensively characterize the microstructure of the prepared samples. Raman spectroscopy, transmission electron microscopy (TEM), and laser confocal microscopy were used to characterize the structural information of the coating before and after friction. To reduce experimental errors, each experiment was repeated three times.

[0039] Coating friction and wear test: The Gr-MCD(Ni,Ga) coating, MCD coating, and diamond-graphene (Gr-MCD(Ga)) coating prepared in Example 1 were subjected to friction and wear tests on a high-pressure, high-speed simulated mechanical seal vibration test bench equipped with a corrosion testing module. The MCD preparation parameters are shown in Table 1. Gr-MCD(Ga) is graphene with a vertical surface catalyzed only by liquid Ga; Ga is commercially available from Dongguan Dingyi Metal Co., Ltd. Gr-MCD(Ni,Ga) is the diamond coating prepared in Example 1, then a Ni coating is deposited on the surface, followed by a Ga layer. The Ni layer was sputtered using a 99.99% high-purity target from Zhongnuo New Materials; Ga is commercially available. In the friction test, silicon carbide (SiC) ceramic balls with a diameter of 6 mm were used as the mating material, and the friction test temperature in a seawater environment was 0°C. During the friction test, the applied load was fixed at 5 Newtons, the test duration was 2.5 hours, the average sliding speed for all tests was 50 mm / s, and the stroke length was 5 mm. The wear rate was calculated using the formula W = V / FL, where V, F, and L represent the cumulative wear volume (mm²). 3 The applied normal load (N) and total sliding distance (m) were used. To reduce error, all experiments were repeated at least three times.

[0040] Performance Analysis: like Figure 2 As shown, the wetting behavior of Ga on the surface of the MCD coating and the nickel-plated microcrystalline diamond (MCD-Ni) composite coating provided in Example 1 is compared. The contact angle characterization intuitively reflects the influence of different substrates on the wettability of liquid Ga.

[0041] As shown in Figure 2(a), liquid Ga exhibits a typical superhydrophobic state on the surface of a pure MCD coating, with a static contact angle of approximately 150° and extremely poor wettability. The essence of this phenomenon lies in the fact that when liquid Ga is exposed to air, its surface rapidly oxidizes to form a dense gallium oxide (Ga₂O₃) film approximately 2 nm thick. This oxide layer has high chemical stability, significantly increasing the solid-liquid interfacial tension between liquid Ga and the MCD substrate, hindering effective interfacial contact and interaction, ultimately leading to deteriorated wettability. In stark contrast, the wettability of liquid Ga on the surface of the MCD-Ni composite coating is improved.

[0042] As shown in Figure 2(b), the static contact angle decreased to approximately 110°, a reduction of 40° compared to the pure MCD coating. The core mechanism of this improved wettability lies in the introduction of the Ni transition layer, which triggers an interfacial chemical reaction. During the contact process, liquid Ga and Ni undergo an alloying reaction to generate Ni-Ga intermetallic compound (IMC). This IMC phase can effectively disrupt the Ga2O3 oxide layer on the surface of liquid Ga, while simultaneously enhancing the interfacial bonding energy between liquid Ga and the MCD-Ni substrate, thereby reducing the solid-liquid interfacial tension and optimizing wettability. Furthermore, Ni, as a highly efficient catalyst in the field of carbon material growth, can not only regulate wettability but also provide support for subsequent graphene growth through two pathways: on the one hand, Ni can reduce the sp(s) content in diamond. 3 The bond energy barrier of hybrid carbon promotes the transfer of carbon source to sp from the MCD coating surface. 2 Hybrid carbon conversion lays the structural foundation for graphene nucleation. On the other hand, based on a metal alloying control strategy, the introduction of Ni can significantly improve the solubility of carbon in liquid Ga. Previous literature indicates that the carbon solubility of Ni at 1000℃ is approximately 1.3 at.%, far higher than that of Ga. Sufficient dissolved carbon sources can meet the carbon requirements for graphene nucleation and growth, not only improving carbon conversion efficiency but also accelerating the graphene growth rate. In summary, introducing a Ni transition layer onto the MCD coating surface can improve the wettability of liquid Ga through interfacial reactions and provide a catalytic effect and carbon source guarantee for graphene growth, ultimately creating favorable conditions for the controllable growth of graphene structures with both horizontal and vertical orientations.

[0043] Figure 3 The images show the surface morphology, Raman spectra, and cross-sectional morphology of the MCD samples before and after the growth of the top layer of graphene. Figure 3 (a) in the middle, Figure 3 (b) shows that the prepared MCD coating has a grain size between 3 and 6 μm, a coating thickness of approximately 9.2 nm, and a thickness of 1334.1 cm⁻¹. -1A strong peak was observed at the location ( Figure 3 (c) indicates that the MCD coating has been successfully prepared.

[0044] Figure 3 Image (d) shows the surface morphology of the coating after gallium direct catalysis of MCD. The image indicates that a rose petal-like structure appears on the MCD coating surface after gallium direct catalysis. Figure 3 As shown in (e), the height of the vertical graphene sheet after conversion is approximately 520 nm, according to the Raman spectrum. Figure 3 (f) indicates that, compared to the original MCD coating, the diamond peak on the surface of the catalytically catalyzed coating disappears, while three new peaks appear: the D peak (1331.5 cm⁻¹). -1 ), G peak (1581.2cm) -1 ) and 2D peak (2712.9cm) -1 The D peak is caused by the disordered structure of graphene. The G peak is related to the disordered polycrystalline and nanocrystalline graphitic carbon inside the coating and is one of the characteristic peaks of graphene. The 2D peak, as another characteristic peak of graphene, is one of the important standards for judging the growth quality of graphene. By performing peak fitting on the Raman peaks after growth, it can be seen that the I peak of the prepared coating is... D / I G A value of 0.165 indicates that the prepared graphene sheets have a low degree of disorder and good graphene quality. 2D / I G A value of 0.685 < 1 indicates that the prepared graphene sheet has a multilayer structure. It is worth noting that... Figure 3 (d) shows that after gallium metal directly catalyzes MCD, there are still large areas of exposed diamond coating on the coating surface. This is because the mutual wetting effect between the diamond coating and liquid gallium metal is poor, and some diamond coatings fail to fully contact gallium, ultimately resulting in a low efficiency of diamond to graphene conversion.

[0045] like Figure 3 As shown in (g), compared to direct liquid gallium catalysis for MCD coating, the MCD is catalyzed after nickel plating, resulting in more uniform vertical graphene growth on the coating surface, increased graphene sheet height (725-962 nm), and the formation of horizontally structured graphene. Figure 3 (h) in the middle. Figure 3 (i) Raman spectroscopy shows that the surface of the catalytically catalyzed coating reaches 1354.9 cm⁻¹. -1 1581.3 cm -1 2702.8 cm -1 It exhibits a strong peak. And the coating's I... D / I G The value is 0.148, which shows a decrease in disorder compared to the direct catalytic coating surface of graphene. 2D / I G The value of 0.634 < 1 indicates that the prepared graphene multilayer structure has increased. In summary, it can be concluded that Ni,Ga bimetallic catalysis not only facilitates the growth of vertically structured graphene, but also enables the preparation of graphene sheets with both horizontal and vertical structures.

[0046] To investigate the interfacial structure between diamond and graphene, the prepared Gr-MCD coated samples were analyzed using a high-resolution HRTEM instrument. The results are as follows: Figure 4 As shown. Figure 4 Images (a) and (d) in Figure 4 show transmission images of Gr-MCD(Ga) and Gr-MCD(Ni,Ga) coatings, respectively. The images reveal a distinct columnar structure in the prepared MCDs, with vertical growth heights of approximately 500 nm and 1000 nm, consistent with SEM observations. High-resolution images (b) and (e) in Figure 4 clearly demonstrate the interface structure between the graphene layer and the diamond lattice, showing that the graphene lattice is continuously epitaxially grown from the diamond lattice. This provides direct microscopic evidence for the in-situ growth of graphene from diamond catalyzed by Ni and Ga. Fourier transform (FFT) analysis of selected regions further confirmed the crystal structure at the interface. The lattice spacings measured before transformation (in the diamond region) were 0.202 nm and 0.206 nm, corresponding to the 111 crystal plane of diamond. After conversion (graphite region), the measured lattice spacings were 0.320 nm and 0.334 nm, corresponding to the 0001 crystal plane of graphene. Diamond and graphene can be almost perfectly bonded through the covalent bonds of diamond (111) and graphene (0001), with a lattice mismatch of only 2%.

[0047] like Figure 4 As shown in (e), the Gr-MCD (Ni, Ga) coating prepared in Example 1 exhibits a distinct horizontal and vertical stacking structure. To further demonstrate that the top layer of the prepared Gr-MCD coating is a vertical graphene sheet, the top vertical graphene sheet of the Gr-MCD coating was peeled off using an ultrasonic device. HRTEM analysis revealed that the thickness of the graphene sheet in the Gr-MCD (Ga) coating was approximately 5 layers, while the thickness in the Gr-MCD (Ni, Ga) coating was 9 layers. This indicates that the introduction of bimetallic catalysis not only facilitates the horizontal stacking of graphene but also promotes the vertical growth of graphene (e.g., ...). Figure 4 (As shown in (c) and (f)). Based on the combined observations of SEM and TEM images, a schematic diagram of the prepared Gr-MCD(Ni, Ga) coating structure is shown below. Figure 4 As shown in (g), vertically structured graphene and horizontally structured graphene are stacked sequentially on the surface of the diamond coating to form a unique graphene-diamond composite coating that combines both structures.

[0048] like Figure 5 As shown in the specific embodiments of the present invention, the growth mechanism of the diamond-graphene composite coating can be divided into three key stages, as follows: Initial nucleation stage of horizontally oriented graphene: Under a high-temperature reaction environment, the pre-deposited nickel (Ni) transition layer directly contacts the surface of the microcrystalline diamond (MCD) coating. Ni, as a typical metal catalyst, can preferentially reduce the sp(s) content in diamond. 3 The bond energy of hybrid carbon catalyzes the decomposition of carbon sources on the diamond surface into free carbon atoms. These free carbon atoms gradually form stable horizontally oriented graphene on the Ni layer surface through diffusion and reconstruction. The formation and wettability regulation stage of the intermetallic compound (IMC): When liquid gallium (Ga) comes into contact with the Ni layer, an interfacial reaction occurs at high temperature to generate a Ni-Ga intermetallic compound. On the one hand, the formation of IMC can significantly improve the wettability between liquid Ga and the MCD substrate. By reducing the solid-liquid interfacial tension, liquid Ga is uniformly spread on the substrate surface, providing a continuous and uniform reaction interface for the subsequent directional growth of vertical graphene. On the other hand, the presence of Ni can effectively increase the solubility of carbon in the system, promoting the dissolution of more free carbon atoms in the liquid metal medium, providing a sufficient carbon source for graphene nucleation and growth, thereby improving carbon conversion efficiency and graphene growth rate.

[0049] The growth and dual-structure formation stages of vertically oriented graphene: As the reaction continues, free carbon atoms dissolved in Ni-GaIMC diffuse towards the liquid Ga / IMC interface. When the carbon concentration reaches supersaturation, Ga atoms in the IMC phase can catalyze the growth of carbon atoms perpendicular to the substrate surface by controlling the carbon diffusion path and nucleation direction, thus forming vertically oriented graphene. Ultimately, through the synergistic effect of the initial nucleation of horizontal graphene and the subsequent growth of vertical graphene, a Gr-MCD coating with both horizontal and vertical dual-orientation structures is formed on the MCD coating surface.

[0050] To investigate the tribological properties of diamond-graphene composite coatings in a seawater environment, tribological tests were performed on MCD, Gr-MCD(Ga), and the Gr-MCD(Ni, Ga) coating prepared in Example 1. The results are as follows: Figure 6 As shown.

[0051] Figure 6Figure (a) shows the friction coefficient variation curves of various coatings in a seawater environment. It can be seen that there are significant differences in the friction behavior of different coatings: after approximately 2.5 hours of break-in, the friction coefficient of the MCD coating stabilizes at around 0.072; while the Gr-MCD(Ga) and Gr-MCD(Ni, Ga) coatings, due to their similar surface graphene structures, exhibit similar friction characteristics, with stable friction coefficients of 0.04 and 0.03, respectively. Compared with the MCD coating, the friction coefficients are reduced by 42.9% and 57.1%, respectively.

[0052] like Figure 6 As shown in (b), the MCD coating exhibits the highest wear rate, reaching 3.78 × 10⁻⁶. -6 mm 3 / (N·m); Gr-MCD(Ga) coating is second, at 1.81×10 -6 mm 3 / (N·m), the wear rate was reduced by 52.1%; the Gr-MCD(N,Ga) coating had the lowest wear rate, only 1.65 × 10 / (N·m). -6 mm 3 / (N·m), the wear rate decreased by 56.3%.

[0053] The wear rates of the grinding pairs showed similar trends: the grinding pairs with MCD coatings experienced the most severe wear, with a wear rate of 1.71 × 10⁻⁶. -4 mm 3 / (N·m); The wear rates of the mating pairs of Gr-MCD(Ga) and Gr-MCD(Ni, Ga) coatings were 1.66×10⁻⁶ / (N·m). -4 mm 3 / (N·m) and 1.02×10 -4 mm 3 The wear rate was reduced by 6.62% and 45.1% respectively, with the coefficient of friction / (N·m) / (N·m). Among them, the Gr-MCD(Ni, Ga) group showed the best tribological performance.

[0054] To further investigate the tribological behavior of diamond and diamond-graphene composite coatings in a seawater environment, Figure 7 SEM images of the worn surfaces of each coating and the wear morphology of the corresponding friction pairs are shown. As can be seen from the images, the wear track of the MCD coating is relatively wide after friction, while the wear track width is significantly reduced after vertical graphene is grown on its surface, and the number of grooves in the wear track area is also significantly reduced.

[0055] Figure 7Images (a) and (b) show the overall morphology of the wear track after friction and a magnified local SEM image of the MCD coating, respectively. It is evident that the MCD coating exhibits the widest wear track (1.26 mm) and numerous grooves on its surface, primarily due to the significant ploughing effect during friction. High-magnification images reveal that some diamond tips on the coating surface have been ground flat and are covered with a small amount of wear debris. EDS analysis indicates that the silicon content in the wear debris in this area is 1.99%, suggesting that the wear debris mainly originates from the SiC grinding pair. Figure 7 Image (c) shows the wear scar image of the friction pair corresponding to the MCD coating. The wear scar radius is 1634 μm, and there are obvious furrows on the surface, which further confirms that a severe furrowing effect and wear occurred between SiC and the MCD coating.

[0056] The wear morphology and magnified images of the Gr-MCD(Ga) coating are shown below. Figure 7 As shown in (d) and (e) in the image, compared to the MCD, the wear track width is slightly reduced to 1.14 mm. The furrows are shallower but still visible, indicating that the vertical graphene on the surface alleviates the furrowing effect to some extent. However, due to the presence of exposed diamond areas, the furrowing effect is not completely suppressed. A magnified local image shows that the wear debris is partially encapsulated by graphene. EDS results show that the silicon content at this location decreases to 1.43%, which may be related to the weakening of silicon characteristic signals caused by the graphene coverage. Figure 7 Image (f) shows the wear scar of the Gr-MCD(Ga) coated pair, with a wear scar radius of 1429 μm. The surface is relatively smooth, and the wear is less severe than that of the MCD friction pair.

[0057] The wear morphology of the Gr-MCD(Ni,Ga) coating prepared in Example 1 is as follows: Figure 7 As shown in (g), the wear track width is further reduced to only 1.08 mm, and the surface is smoother. Its high-magnification image shows that the wear debris is more completely encapsulated by graphene. For example... Figure 7 As shown in (h) and (i), the silicon content measured by EDS is the lowest, at only 0.99%. The corresponding wear scar radius of the friction pair is also the smallest, at 980 μm, and the surface is smooth. In summary, in a seawater environment, growing vertical graphene on a diamond surface can effectively reduce the ploughing effect between the coating and the friction pair, reduce the wear scar width, and thus improve the tribological properties of the coating.

[0058] like Figure 8 As shown, the different friction mechanisms of MCD and Gr-MCD(Ni, Ga) coatings in a seawater environment are illustrated. In a seawater environment, when the MCD coating rubs against a silicon carbide grinding ball, its significant conical structure induces a pronounced ploughing effect, resulting in a high coefficient of friction and severe abrasive wear.

[0059] The Gr-MCD(Ni,Ga) coating prepared in Example 1 exhibits a significantly different friction mechanism: during friction, on the one hand, the vertical graphene sheets on the surface are flattened and cover the diamond tip, effectively mitigating the ploughing effect caused by the tip by utilizing the excellent lubricity of graphene itself; on the other hand, the presence of the underlying horizontal graphene layer acts as a lubricating and barrier layer, further enhancing the overall lubrication performance of the coating, thereby significantly reducing the coefficient of friction. As friction continues, the softer SiC ball generates wear debris, and some graphene sheets break at the root, forming sheet-like graphite wear debris. These broken graphene sheets can adhere to the surface of the grinding ball, further reducing the ploughing effect; in addition, some graphene sheets adsorb onto the wear debris surface and curl, promoting the transformation of the friction interface from pure sliding to a sliding-rolling hybrid mode, thereby more effectively reducing the overall coefficient of friction.

[0060] Example 2 Diamond coating preparation: First, a hot-wire chemical vapor deposition (HFCVD) method was used to deposit an MCD coating onto a silicon carbide (SiC) substrate. The preparation process included the following steps: 1) Substrate pretreatment: The SiC substrate surface was mechanically roughened for 10 minutes using W40 diamond slurry to enhance the adhesion of the subsequent diamond coating. 2) Ultrasonic nucleation treatment: The SiC substrate was placed in a diamond powder suspension and subjected to ultrasonic oscillation for 20 minutes, followed by drying with a high-purity nitrogen stream. This treatment forms numerous nucleation sites, promoting uniform deposition of the diamond coating. 3) MCD coating deposition: The pretreated SiC substrate was placed in the HFCVD reaction chamber, and the MCD coating was deposited by decomposing a CH4 / H2 mixture using four parallel tantalum wires. Specific deposition parameters are detailed in Table 3.

[0061] Preparation of graphene-diamond composite coating The in-situ preparation process of the graphene-diamond composite coating is as follows: First, a copper layer approximately 300 nm thick is deposited on the MCD coating using physical vapor deposition (PVD). Before graphene growth, the sample is ultrasonically cleaned sequentially in acetone, ethanol, and deionized water (10 minutes each), and then dried under a nitrogen atmosphere. After cleaning, the diamond-nickel composite coating is placed in a square quartz container, and gallium is added as a catalyst. The quartz container is then transferred to a tube furnace for vacuum annealing. An in-situ conversion reaction is carried out at 1200 °C for 5 hours under an argon flow rate of 40 sccm to convert diamond into graphene. After the reaction, the coating is slowly cooled to room temperature. The resulting surface is covered with a uniform Ga film, which is then etched with hydrochloric acid at 80 °C for 8 hours to remove residual metal, thus completing the preparation of the Gr-MCD coating. The detailed preparation process of the graphene-diamond composite coating is as follows: Figure 1 As shown, the deposition parameters corresponding to the Cu layer are shown in Table 4.

[0062] Table 3: MCD Coating Deposition Parameters

[0063] Table 4: Cu coating deposition parameters

[0064] like Figure 9 As shown in (a), compared to direct liquid gallium catalysis of MCD coating, the MCD is catalyzed after nickel plating, resulting in more uniform vertical graphene growth on the coating surface, an increased graphene sheet height of 556 nm, and the formation of horizontally structured graphene. Figure 9 (b) in the middle. Figure 9 (c) Raman spectra show that, where the ordinate represents intensity and the abscissa represents Raman shift, the surface of the catalytically catalyzed coating reaches a value of 1350.1 cm⁻¹. -1 1580.1 cm -1 2701.4 cm -1 It exhibits a strong peak. In summary, it can be concluded that Cu,Ga bimetallic catalysis not only facilitates the growth of vertically structured graphene, but also enables the preparation of graphene sheets with both horizontal and vertical structures.

Claims

1. A method for preparing a graphene-diamond composite coating, characterized in that, include: The substrate surface is roughened by grinding, crystals are ultrasonically implanted on the roughened substrate, and then a diamond coating is formed by CVD. A transition metal layer, which is a Ni layer, a Ti layer, or a Cu layer, is deposited on the surface of a diamond coating by magnetron sputtering. Gallium metal was dropped onto the transition metal layer, and then vacuum annealing was performed to obtain a graphene-diamond composite coating.

2. The method for preparing the graphene-diamond composite coating according to claim 1, characterized in that, The transition metal layer is a Ni layer.

3. The method for preparing the graphene-diamond composite coating according to claim 1 or 2, characterized in that, The vacuum annealing process is as follows: under an argon atmosphere, the annealing temperature is 1100-1300℃, and the holding time is 4-7h.

4. The method for preparing the graphene-diamond composite coating according to claim 3, characterized in that, The flow rate of the argon gas is 35-45 sccm.

5. The method for preparing the graphene-diamond composite coating according to claim 1, characterized in that, The substrate is made of ceramic, hard alloy, or high-temperature alloy.

6. The method for preparing the graphene-diamond composite coating according to claim 5, characterized in that, The ceramic is silicon carbide, silicon nitride, aluminum oxide, or zirconium oxide.

7. The method for preparing the graphene-diamond composite coating according to claim 1, characterized in that, Methods for preparing transition metal layers include: Using a Ni target, the parameters of the magnetron sputtering method include: vacuum degree < 1 × 10⁻⁶. -4 Pa, power 100-150 W, gas pressure 0.8-1.5 Pa, argon flow rate 20 sccm-35 sccm, sputtering temperature maintained at 50-250 ℃, sputtering time 10-60 min; Alternatively, a Cu target can be used, and the magnetron sputtering parameters include: vacuum level < 1 × 10⁻⁶. -4 Pa, power 80-120 W, gas pressure 0.8-1.2 Pa, argon flow rate 15 sccm-30 sccm, sputtering temperature maintained at 0-150 ℃, sputtering time 5 min-75 min.

8. The method for preparing the graphene-diamond composite coating according to claim 1, characterized in that, After vacuum annealing, the prepared sample is placed in concentrated hydrochloric acid solution and left to stand for 4-7 hours to remove residual liquid gallium.

9. A graphene-diamond composite coating, characterized in that, The graphene-diamond composite coating is prepared by the method according to any one of claims 1-8, wherein the graphene-diamond composite coating comprises a horizontal graphene and a vertical graphene stacked structure.

10. The graphene-diamond composite coating according to claim 9, characterized in that, The vertical graphene is located on the horizontal graphene, and the height of the vertical graphene is 550~1000 nm.

Citation Information

Patent Citations

  • Graphene-diamond covalent heterostructure connected through covalent bond and preparation method thereof

    CN113582173A

  • Batch preparation method of graphene-diamond covalent heterostructure particles

    CN116969454A

  • Graphene-diamond composite coating as well as preparation method and application thereof

    CN118996371A

  • Compound heat conduction membrane of diamond / graphite alkene and cooling system

    CN207775345U

  • AA stacked graphene-diamond hybrid material by high temperature treatment of diamond and the fabrication method thereof