Metal composite material and preparation method and application thereof
By combining TiC steel-bonded cemented carbide and low-carbon steel with vacuum sintering and heat treatment processes, the problem of insufficient impact toughness and wear resistance of steel-bonded cemented carbide has been solved, realizing a metal composite material with high wear resistance and impact resistance, which is suitable for wear-resistant hammers and other applications.
Patent Information
- Application Number
- CN202511408732.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-29
- Publication Date
- 2026-01-09
AI Technical Summary
Existing steel-bonded cemented carbide materials are insufficient in terms of impact toughness and wear resistance, and are prone to deformation or fracture during sintering, which limits their application range.
A metal composite material with high wear resistance and the ability to withstand impact loads was prepared by using TiC steel-bonded cemented carbide as the working layer and low carbon steel as the matrix layer, through vacuum sintering and heat treatment processes, with a transition zone of 0.05mm to 0.8mm at the interface.
It improves the overall impact toughness and wear resistance of the material, solves the deformation problem of single steel-bonded cemented carbide during sintering, expands its application range, and shows a significant extension of service life, especially in wear-resistant hammer plates.
Smart Images

Figure CN121289478A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite materials, specifically to a metal composite material, its preparation method, and its application. Background Technology
[0002] Steel-bonded cemented carbide is a hard material produced using a liquid-phase sintering method with TiC carbide as the hard phase and high-manganese steel as the binder phase. This material possesses the high hardness and wear resistance of cemented carbide, but its impact toughness is relatively low, and it experiences significant shrinkage during sintering, making it prone to deformation or fracture when producing large workpieces. Currently, it is typically only produced as small round bars or granules as inserts for easily worn parts of various hammerheads. Steel-bonded cemented carbide cannot be used in applications requiring both wear resistance and impact resistance simultaneously, significantly limiting its application. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a metal composite material containing TiC steel-bonded cemented carbide, which has high wear resistance and can withstand impact loads. The present invention also includes the preparation method and application of the metal composite material.
[0004] The technical solution adopted by the present invention to solve its technical problem is as follows: a metal composite material, comprising a working layer and a matrix layer; the working layer and the matrix layer are metallurgically bonded; there is a transition zone with a thickness of 0.05mm to 0.8mm at the interface between the working layer and the matrix layer; the main component of the working layer is TiC steel-bonded hard alloy; the main component of the matrix layer is low carbon steel; The TiC steel-bonded cemented carbide comprises the following components by mass percentage: 40%–50% titanium carbide, 0.6%–0.9% carbon, 6%–9% manganese, 0.9%–1.2% molybdenum, 1.0%–1.5% nickel, and the balance being iron and unavoidable impurities; In the low-carbon steel, the mass percentage of carbon does not exceed 0.25%; The working layer accounts for 20% to 60% of the total volume of the composite material.
[0005] Based on the same inventive concept, this invention also provides a method for preparing the aforementioned metal composite material: pressing TiC steel-bonded cemented carbide raw material into a powder with a density of 4.3 g / cm³ using conventional powder metallurgy methods. 3 ~4.6g / cm 3 The powder block blank is then bonded to low carbon steel and vacuum sintered. After vacuum sintering, heat treatment is performed to obtain a metal composite material. The high-temperature section of the vacuum sintering process has a temperature of 1390℃~1450℃; The heat treatment method is as follows: first, the temperature is raised to 1050℃~1100℃, and then the temperature is rapidly cooled; the cooling rate of the rapid cooling process is greater than 80℃ / min.
[0006] Preferably, the vacuum degree of the vacuum sintering is 1 Pa to 10 Pa.
[0007] Preferably, the raw materials for TiC steel-bonded cemented carbide include TiC powder and binder phase material powder.
[0008] Preferably, after the raw material of TiC steel-bonded cemented carbide is granulated, the particle size meets the following condition: it can pass through a 60-mesh sieve.
[0009] Preferably, the powder block blank also contains 0.2% to 0.4% vinyl acetate by mass.
[0010] Preferably, the pressure for pressing the powder block blank is 100MPa~300MPa.
[0011] Preferably, the vacuum sintering process is as follows: the temperature is increased from room temperature to 250℃~350℃ at a heating rate of 4℃ / min~6℃ / min, and held for 20min~60min; then the temperature is increased to 400℃~500℃ at a heating rate of 8℃ / min~10℃ / min, and held for 20min~60min; then the temperature is increased to 900℃~1100℃ at a heating rate of 8℃ / min~11℃ / min, and held for 20min~60min; subsequently, the temperature is increased to 1390℃~1450℃ at a heating rate of 3℃ / min~5℃ / min, and held for 60min~90min; after the holding period, the temperature is cooled to 780℃~820℃ in the furnace, and then removed from the furnace and air-cooled to room temperature.
[0012] Preferably, the heat treatment process is as follows: the temperature is raised to 300℃~350℃ at a heating rate of 50℃ / h~60℃ / h and held for 2~3.5 hours; then the temperature is raised to 650℃~700℃ at a heating rate of 50℃ / h~60℃ / h and held for 1~2.5 hours; then the temperature is raised to 1050℃~1100℃ at a heating rate of 80℃ / h~100℃ / h, with a holding time of 50min~70min for every 20mm of billet thickness; after the holding time is completed, the billet is removed from the furnace and quickly immersed in a cooling medium for rapid cooling.
[0013] Preferably, during the heat treatment process, the cooling medium used for the rapid cooling process is water.
[0014] Preferably, during the heat treatment process, the time from exiting the furnace to immersion in the cooling medium during rapid cooling should not exceed 30 seconds.
[0015] Preferably, during the heat treatment process, after the rapid cooling treatment is completed, the temperature of the cooling medium used in the rapid cooling treatment is below 60°C.
[0016] Based on the same inventive concept, the present invention also provides the application of the metal composite material or the metal composite material prepared by the method of preparing the metal composite material in wear-resistant hammer plates.
[0017] Preferably, the contact surface material between the wear-resistant hammer and the material is a working layer of metal composite material.
[0018] The present invention has the following beneficial effects: The metal composite material of the present invention combines TiC steel-bonded cemented carbide powder and low carbon steel. TiC steel-bonded cemented carbide has high hardness and excellent wear resistance. The low carbon steel matrix layer is easy to machine and has good weldability. The low carbon steel matrix layer provides the material with impact resistance as a whole, so that the material can withstand impact loads while having high wear resistance.
[0019] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The invention will now be described in further detail with reference to the accompanying drawings. Attached Figure Description
[0020] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a metallographic image of the working layer-matrix layer bonding interface after vacuum sintering during the preparation of the metal composite material in Embodiment 1 of the present invention; Figure 2 This is a metallographic image of the working layer-matrix layer interface after heat treatment during the preparation of the metal composite material in Embodiment 1 of the present invention. Detailed Implementation
[0021] To make the objectives, solutions, and beneficial technologies of this invention clearer, the invention will be further described in detail below with reference to embodiments and accompanying drawings. It should be noted that the embodiments described in this specification are merely illustrative of the invention and are not intended to limit the invention.
[0022] For simplicity, this paper only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, just as any upper limit can be combined with any other upper limit to form an undefined range. Furthermore, although not explicitly stated, every point or individual value between the endpoints of a range is included within that range. Therefore, each point or individual value can serve as its own lower or upper limit and be combined with any other point or individual value, or with other lower or upper limits, to form an undefined range.
[0023] In this description, it should be noted that, unless otherwise stated, "above" and "below" include the stated number, "multiple" in "one or more" means two or more, and "more than" in "one or more" means two or more.
[0024] An embodiment of the present invention provides a metal composite material, comprising a working layer and a matrix layer; the working layer and the matrix layer are metallurgically bonded; there is a transition zone with a thickness of 0.05 mm to 0.8 mm at the interface between the working layer and the matrix layer; the main component of the working layer is TiC steel-bonded cemented carbide; the main component of the matrix layer is low-carbon steel. The TiC steel-bonded cemented carbide comprises the following components by mass percentage: 40%–50% titanium carbide, 0.6%–0.9% carbon, 6%–9% manganese, 0.9%–1.2% molybdenum, 1.0%–1.5% nickel, and the balance being iron and unavoidable impurities; In the low-carbon steel, the mass percentage of carbon does not exceed 0.25%; The working layer accounts for 20% to 60% of the total volume of the composite material.
[0025] In some embodiments of the present invention, a transition zone with a thickness of 0.1 mm to 0.6 mm is present at the interface between the working layer and the substrate layer. The transition zone is a mutually soluble region formed by the mutual diffusion of the two metals at high temperatures.
[0026] In some embodiments of the present invention, the volume of the working layer accounts for 30% to 50% of the total composite material.
[0027] The embodiments of the present invention also include a method for preparing the aforementioned metal composite material: pressing the TiC steel-bonded cemented carbide raw material into a powder with a density of 4.3 g / cm³ using conventional powder metallurgy methods. 3 ~4.6g / cm 3 The powder block blank is then bonded to low carbon steel and vacuum sintered. After vacuum sintering, heat treatment is performed to obtain a metal composite material. The high-temperature section of the vacuum sintering process has a temperature of 1390℃~1450℃; The heat treatment method is as follows: first, the temperature is raised to 1050℃~1100℃, and then rapidly cooled; the cooling rate of the rapid cooling process is greater than 80℃ / min. Heat treatment can improve the toughness of TiC steel-bonded cemented carbide.
[0028] The conventional powder metallurgy process can be summarized as follows: wet grinding → drying → binder addition → granulation → molding.
[0029] TiC steel-bonded cemented carbide alone has poor impact toughness and suffers from large shrinkage during sintering, leading to significant deformation and limiting its size and applications. Typically, it can only be produced as round bars with a diameter of 20mm for use as inserts in various wear-resistant hammers. This invention uses low-carbon steel as the matrix layer, which can limit the deformation caused by the large shrinkage during sintering of the steel-bonded cemented carbide, reducing defects. The resulting metal composite material exhibits good interfacial bonding, minimal matrix layer deformation, and no cracks in the working layer, enabling the production of large-size TiC steel-bonded cemented carbide working layers. The method of this invention has a simple production process, and the overall impact toughness of the resulting metal composite material is significantly improved.
[0030] In an embodiment of the present invention, the vacuum degree of the vacuum sintering is 1 Pa to 10 Pa.
[0031] In embodiments of the present invention, the raw materials for TiC steel-bonded cemented carbide include TiC powder and binder phase material powder.
[0032] In an embodiment of the present invention, after the raw material of TiC steel-bonded cemented carbide is granulated, the particle size meets the following condition: it can pass through a 60-mesh sieve.
[0033] In an embodiment of the present invention, the powder blank further contains 0.2% to 0.4% vinyl acetate by mass. The vinyl acetate acts as a binder in powder metallurgy.
[0034] In an embodiment of the present invention, the pressure for pressing the powder block blank is 100MPa~300MPa.
[0035] In an embodiment of the present invention, the vacuum sintering process is as follows: the temperature is increased from room temperature to 250°C to 350°C at a heating rate of 4°C / min to 6°C / min, and held for 20 min to 60 min; then the temperature is increased to 400°C to 500°C at a heating rate of 8°C / min to 10°C / min, and held for 20 min to 60 min; then the temperature is increased to 900°C to 1100°C at a heating rate of 8°C / min to 11°C / min, and held for 20 min to 60 min; subsequently, the temperature is increased to 1390°C to 1450°C at a heating rate of 3°C / min to 5°C / min, and held for 60 min to 90 min; after the holding period, the temperature is cooled in the furnace to 780°C to 820°C, and then removed from the furnace and air-cooled to room temperature.
[0036] During vacuum sintering, the heat preservation in the 250℃~350℃ range plays a role in degreasing and promotes the discharge of binders.
[0037] In an embodiment of the present invention, the heat treatment process is as follows: the temperature is raised to 300℃~350℃ at a heating rate of 50℃ / h~60℃ / h and held for 2~3.5 hours; then the temperature is raised to 650℃~700℃ at a heating rate of 50℃ / h~60℃ / h and held for 1~2.5 hours; then the temperature is raised to 1050℃~1100℃ at a heating rate of 80℃ / h~100℃ / h, with a holding time of 50min~70min for every 20mm of billet thickness (e.g., if the thickness is 50mm, the holding time is 50 / 20×50min~50 / 20×70min, which equals 125min~175min); after the holding time is completed, the billet is removed from the furnace and quickly immersed in a cooling medium for rapid cooling.
[0038] During heat treatment, the heat preservation in the 300℃~350℃ range helps to relieve stress; the heat preservation in the 650℃~700℃ range can prevent the precipitation of carbides.
[0039] In an embodiment of the present invention, water is used as the cooling medium for the rapid cooling process during heat treatment.
[0040] In an embodiment of the present invention, during the heat treatment process, the rapid cooling process takes no more than 30 seconds from the time the material is taken out of the furnace to the time it is immersed in the cooling medium.
[0041] In an embodiment of the present invention, during the heat treatment process, after the rapid cooling process is completed, the temperature of the cooling medium used in the rapid cooling process is below 60°C.
[0042] In some embodiments of the present invention, the cooling rate of the rapid cooling process is greater than 100°C / min.
[0043] The embodiments of the present invention also include the application of the metal composite material or the metal composite material prepared by the method of preparing the metal composite material in wear-resistant hammer plates.
[0044] In an embodiment of the present invention, the contact surface material between the wear-resistant hammer and the material is a working layer of metal composite material.
[0045] Metal composite materials can be processed into wear-resistant hammer plates through conventional cutting methods. Wear-resistant hammer plates are generally long strips, and the working layer can be a plane, or a convex or concave shape with central symmetry. The mounting surface (base layer) can be processed according to the requirements of the rotor of the impact crusher.
[0046] An impact crusher is a crushing machine that uses impact energy to crush materials. It features a large crushing ratio, good particle shape and gradation of the crushed products, strong adaptability, simple structure, and convenient replacement of wearing parts, making it widely used in mining, construction, and road construction. The main problem with impact crushers is the rapid wear of the wear-prone hammer plates. Currently, hammer plates are mainly made of single-metal materials such as high-manganese steel and high-chromium cast iron, which have good impact resistance but insufficient wear resistance. The working layer facing the material directly impacts the material, resulting in severe wear when processing high-hardness materials, requiring frequent replacement. This invention uses a metal composite material to manufacture wear-resistant hammer plates. TiC steel-bonded cemented carbide serves as the working layer facing the material, directly impacting it. The low-carbon steel matrix layer is easy to machine, has good weldability, and can withstand impact loads, serving as the contact and fixing surface for mounting the hammer plates onto the rotor of the impact crusher. TiC has a microhardness of 3000~3200 HV and a density of 4.93 g / cm³. 3 In the metal composite material of the present invention, its volume fraction in the steel-bonded cemented carbide is more than 52%, which makes the TiC steel-bonded cemented carbide working layer, although not very hard (HRC about 60), very wear-resistant. The results of its use in a certain mine show that its service life is more than 4 times that of high-chromium cast iron hammer plates.
[0047] The combination of the working layer and the matrix layer in this invention's metal composite material significantly reduces costs. TiC steel-bonded cemented carbide powder costs approximately 70 yuan / kg, while low-carbon steel plate costs approximately 5 yuan / kg. Simultaneously, the low-carbon steel matrix layer possesses excellent machinability and weldability, solving the problems of difficult machining and poor weldability associated with single-layer steel-bonded cemented carbide. For example, as a wear-resistant hammer, it allows for easy machining of threaded holes, T-slots, welded screws, and connecting blocks during subsequent hammer installation and maintenance.
[0048] Example The following examples describe the disclosure of this invention in more detail. These examples are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight. Unless otherwise stated, all reagents used in the examples are available commercially or synthesized using conventional methods and are ready for use without further processing. Unless otherwise stated, all instruments used in the examples are available commercially.
[0049] Example 1 The metal composite material of this embodiment includes a working layer and a matrix layer; the working layer and the matrix layer are metallurgically bonded; there is a transition zone with a thickness of 0.1 mm to 0.6 mm at the interface between the working layer and the matrix layer; the main component of the working layer is TiC steel-bonded cemented carbide; the main component of the matrix layer is Q235 low carbon steel (carbon mass percentage is 0.19%). The TiC steel-bonded cemented carbide comprises the following components by mass percentage: 40% titanium carbide, 0.9% carbon, 9% manganese, 1.2% molybdenum, 1.5% nickel, and the balance being iron and unavoidable impurities; In this embodiment, the working layer is 20mm thick and the matrix layer is 40mm thick. The volume of the working layer accounts for one-third of the total composite material.
[0050] The preparation method of the metal composite material in this embodiment includes: pressing the TiC steel-bonded cemented carbide raw material into a powder with a density of 4.49 g / cm³ using conventional powder metallurgy methods. 3 The powder block blank is prepared; the low carbon steel is brought into contact with the powder block blank and vacuum sintered; after vacuum sintering is completed, heat treatment is performed to obtain a metal composite material. The process for producing the powder block blank is as follows: (1) Mix TiC powder (hard phase material) and binder phase material powders such as iron, manganese, carbon, molybdenum and nickel according to the mass percentage of TiC steel-bonded hard alloy composition; (2) Add the prepared raw materials to a ball mill, add anhydrous ethanol and grind for 36 hours; remove excess anhydrous ethanol to obtain a mixture with anhydrous ethanol content ≤5%; (3) Add 0.2% vinyl acetate (adhesive) by weight to the mixture and stir evenly; then dry (60℃, 60 hours). (4) Granulate and pass through a 60-mesh sieve to remove oversized particles; add to the mold. The size of a single mold is calculated based on the length and width of the finished product plus the shrinkage of the powder block by about 12%. The length is 448 mm and the width is 224 mm. 10 kg of powder is added to each mold and a 22.2 mm thick powder block blank is made under a pressure of 300 MPa.
[0051] A Q235 low-carbon steel plate with a length of 448mm, a width of 224mm, and a thickness of 40mm is used as the base steel plate. Blocks of the same material as the base steel plate are welded around the plate to fix the position of the powder block blank. The block thickness is 3mm, and it protrudes 20mm above the base surface. The oxide scale, oil, and impurities on the steel plate surface are cleaned. The powder block blank is then placed on the base steel plate and fixed in place by the block. It is then sent into the furnace for vacuum sintering.
[0052] The vacuum sintering process is as follows: the vacuum degree is set to 1 Pa; the temperature is increased from room temperature to 250℃ at a heating rate of 4℃ / min and held for 20 min; then the temperature is increased to 400℃ at a heating rate of 10℃ / min and held for 30 min; then the temperature is increased to 900℃ at a heating rate of 11℃ / min and held for 60 min; then the temperature is increased to 1390℃~1450℃ at a heating rate of 3℃ / min and held for 60 min; after the holding period, the temperature is cooled to 790℃ in the furnace and then removed from the furnace and air-cooled to room temperature. Figure 1 This is a metallographic image of the interface between the working layer and the substrate layer after vacuum sintering: the left side is the working layer, the right side is the substrate layer, and there is a relatively wide transition zone in the middle.
[0053] The heat treatment process is as follows: the temperature is raised to 300℃ at a heating rate of 60℃ / h and held for 3 hours; then the temperature is raised to 700℃ at a heating rate of 60℃ / h and held for 2 hours; then the temperature is raised to 1100℃ at a heating rate of 100℃ / h and held for 3 hours; after the holding period, the product is removed from the furnace and quickly (within 30 seconds) immersed in cold water with a temperature ≤30℃ for rapid cooling treatment, with a cooling rate greater than 100℃ / min, and the water temperature after treatment is below 60℃. Figure 2 This is a metallographic image of the interface between the working layer and the substrate layer after heat treatment: the left side is the working layer, the right side is the substrate layer, and there is a transition zone of about 300 μm in the middle.
[0054] TiC steel-bonded cemented carbide shrinks in volume during vacuum sintering, and the length and width of the matrix layer are larger than those of the working layer. Unwanted parts can be removed by conventional cutting methods.
[0055] The metal composite material of this embodiment is applied to the wear-resistant hammer: the metal composite material is cut into strips with dimensions of 400 mm (length) × 200 mm (width) × 60 mm (height). Threaded holes or slots for installation are machined on the substrate layer. The contact surface material between the wear-resistant hammer and the material is the working layer of the metal composite material. The final finished size of the steel-bonded cemented carbide layer of the composite wear-resistant hammer is 405 mm × 202 mm × 19.7 mm.
[0056] Example 2 The metal composite material of this embodiment includes a working layer and a matrix layer; the working layer and the matrix layer are metallurgically bonded; there is a transition zone with a thickness of 0.1 mm to 0.6 mm at the interface between the working layer and the matrix layer; the main component of the working layer is TiC steel-bonded cemented carbide; the main component of the matrix layer is Q235 low carbon steel (carbon mass percentage is 0.21%). The TiC steel-bonded cemented carbide comprises the following components by mass percentage: 50% titanium carbide, 0.6% carbon, 6.5% manganese, 0.9% molybdenum, 1.0% nickel, and the balance being iron and unavoidable impurities; In this embodiment, the working layer is 25mm thick and the matrix layer is 25mm thick. The volume of the working layer accounts for 50% of the total composite material.
[0057] The preparation method of the metal composite material in this embodiment includes: pressing the TiC steel-bonded cemented carbide raw material into a powder with a density of 4.37 g / cm³ using conventional powder metallurgy methods. 3 The powder block blank is prepared; the low carbon steel is brought into contact with the powder block blank and vacuum sintered; after vacuum sintering is completed, heat treatment is performed to obtain a metal composite material. The process for producing the powder block blank is as follows: (1) Mix TiC powder (hard phase material) and binder phase material powders such as iron, manganese, carbon, molybdenum and nickel according to the mass percentage of TiC steel-bonded hard alloy composition; (2) Add the prepared raw materials into a ball mill, add anhydrous ethanol and grind for 48 hours; remove excess anhydrous ethanol to obtain a mixture with anhydrous ethanol content ≤5%; (3) Add 0.4% vinyl acetate (adhesive) by weight to the mixture and stir evenly; then dry (65℃, 70 hours). (4) Granulate and pass through a 60-mesh sieve to remove oversized particles; add to the mold. The size of a single mold is calculated based on the length and width of the finished product plus the shrinkage of the powder block by about 11%. The length is 333 mm and the width is 111 mm. Add 4.6 kg of powder to each mold and make a powder block blank with a thickness of 28.5 mmr under a pressure of 200 MPa.
[0058] A Q235 low-carbon steel plate with a length of 333mm, a width of 111mm, and a thickness of 25mm is used as the base steel plate. Blocks of the same material as the base steel plate are welded around the plate to fix the position of the powder block blank. The block thickness is 5mm, and it protrudes 12.5mm above the base surface. The oxide scale, oil, and impurities on the steel plate surface are cleaned. The powder block blank is then placed on the base steel plate and fixed in place by the block, and then sent into the furnace for vacuum sintering.
[0059] The vacuum sintering process is as follows: the vacuum degree is set to 10 Pa; the temperature is increased from room temperature to 350℃ at a heating rate of 6℃ / min and held for 60 min; then the temperature is increased to 500℃ at a heating rate of 8℃ / min and held for 60 min; then the temperature is increased to 1100℃ at a heating rate of 8℃ / min and held for 30 min; then the temperature is increased to 1390℃~1450℃ at a heating rate of 5℃ / min and held for 90 min; after the holding period, the temperature is cooled to 820℃ in the furnace and then removed from the furnace and air-cooled to room temperature.
[0060] The heat treatment process is as follows: the temperature is raised to 350℃ at a heating rate of 50℃ / h and held for 2 hours; then the temperature is raised to 650℃ at a heating rate of 50℃ / h and held for 1 hour; then the temperature is raised to 1050℃ at a heating rate of 80℃ / h and held for 2 hours; after the holding period, the product is removed from the furnace and quickly (within 30 seconds) immersed in cold water with a temperature ≤30℃ for rapid cooling treatment, with a cooling rate greater than 100℃ / min, and the water temperature after treatment is below 60℃.
[0061] TiC steel-bonded cemented carbide shrinks in volume during vacuum sintering, and the length and width of the matrix layer are larger than those of the working layer. Unwanted parts can be removed by conventional cutting methods.
[0062] The metal composite material of this embodiment is applied to the wear-resistant hammer: the metal composite material is cut into strips with dimensions of 300 mm long × 100 mm wide × 50 mm high. Threaded holes or slots for installation are machined on the substrate layer. The contact surface material between the wear-resistant hammer and the material is the working layer of the metal composite material. The final finished size of the steel-bonded hard alloy layer of the composite wear-resistant hammer is 298 × 99 × 25.5 mm.
[0063] Performance testing of metal composite materials in Examples 1-2: (1) Take the steel-bonded cemented carbide layer of the metal composite material and measure its density using the Archimedes method; (2) Measure the microhardness of the steel-bonded cemented carbide layer using a microhardness tester; (3) Prepare a V-notch impact sample (10mm×10mm×55mm, a general shape and size, with the two phase interfaces perpendicular to the V-notch) of half steel-bonded cemented carbide and half carbon steel matrix, and determine the impact energy and calculate the impact toughness value of the composite material using the Charpy pendulum impact test method; (4) Prepare a V-notch impact sample (10mm×10mm×55mm, a general shape and size) of a single steel-bonded cemented carbide layer, and determine the impact energy and calculate the impact toughness value of the single steel-bonded cemented carbide layer using the Charpy pendulum impact test method.
[0064] The performance test results of the metal composite materials are shown in Table 1.
[0065] Table 1 Performance test results of the metal composite materials in the examples
Claims
1. A metal composite material, characterized in that, It includes a working layer and a substrate layer; the working layer and the substrate layer are metallurgically bonded; there is a transition zone with a thickness of 0.05mm to 0.8mm at the interface between the working layer and the substrate layer; the main component of the working layer is TiC steel-bonded cemented carbide; the main component of the substrate layer is low-carbon steel. The TiC steel-bonded cemented carbide comprises the following components by mass percentage: 40%–50% titanium carbide, 0.6%–0.9% carbon, 6%–9% manganese, 0.9%–1.2% molybdenum, 1.0%–1.5% nickel, and the balance being iron and unavoidable impurities; In the low-carbon steel, the mass percentage of carbon does not exceed 0.25%; The working layer accounts for 20% to 60% of the total volume of the composite material.
2. The method for preparing the metal composite material as described in claim 1, characterized in that: TiC steel-bonded cemented carbide raw materials were pressed into a powder with a density of 4.3 g / cm³ using conventional powder metallurgy methods. 3 ~4.6g / cm 3 The powder block blank is then bonded to low carbon steel and vacuum sintered. After vacuum sintering, heat treatment is performed to obtain a metal composite material. The high-temperature section of the vacuum sintering process has a temperature of 1390℃~1450℃; The heat treatment method is as follows: first, the temperature is raised to 1050℃~1100℃, and then the temperature is rapidly cooled; the cooling rate of the rapid cooling process is greater than 80℃ / min.
3. The method for preparing the metal composite material according to claim 2, characterized in that, The vacuum degree of the vacuum sintering is 1 Pa to 10 Pa.
4. The method for preparing the metal composite material according to claim 2, characterized in that, The raw materials for TiC steel-bonded cemented carbide include TiC powder and binder phase material powder; after granulation, the particle size of the raw materials for TiC steel-bonded cemented carbide meets the following condition: it can pass through a 60-mesh sieve.
5. The method for preparing the metal composite material according to claim 2, characterized in that, The powder block blank also contains 0.2% to 0.4% vinyl acetate by mass; the pressure for pressing the powder block blank is 100 MPa to 300 MPa.
6. The method for preparing the metal composite material according to any one of claims 2 to 5, characterized in that, The vacuum sintering process is as follows: the temperature is increased from room temperature to 250℃~350℃ at a heating rate of 4℃ / min~6℃ / min, and held for 20min~60min; then the temperature is increased to 400℃~500℃ at a heating rate of 8℃ / min~10℃ / min, and held for 20min~60min; then the temperature is increased to 900℃~1100℃ at a heating rate of 8℃ / min~11℃ / min, and held for 20min~60min; then the temperature is increased to 1390℃~1450℃ at a heating rate of 3℃ / min~5℃ / min, and held for 60min~90min; after the holding period, the temperature is cooled in the furnace to 780℃~820℃, and then removed from the furnace and air-cooled to room temperature.
7. The method for preparing the metal composite material according to claim 6, characterized in that, The heat treatment process is as follows: the temperature is raised to 300℃~350℃ at a heating rate of 50℃ / h~60℃ / h and held for 2~3.5 hours; then the temperature is raised to 650℃~700℃ at a heating rate of 50℃ / h~60℃ / h and held for 1~2.5 hours; then the temperature is raised to 1050℃~1100℃ at a heating rate of 80℃ / h~100℃ / h, with a holding time of 50min~70min for every 20mm of billet thickness; after the holding time is completed, the billet is removed from the furnace and quickly immersed in a cooling medium for rapid cooling.
8. The method for preparing the metal composite material according to claim 2 or 7, characterized in that, During the heat treatment process, the cooling medium used for the rapid cooling treatment is water; during the rapid cooling treatment, the time from taking off the furnace to immersing in the cooling medium does not exceed 30 seconds; after the rapid cooling treatment is completed, the temperature of the cooling medium used for the rapid cooling treatment is below 60°C.
9. The application of the metal composite material as described in claim 1 or the metal composite material prepared by any one of claims 2 to 8 in wear-resistant hammer plates.
10. The application according to claim 9, characterized in that, The contact surface material between the wear-resistant hammer and the material is a metal composite working layer.