Direct regeneration method and application of invalid battery positive electrode material based on size regulation and control
By controlling the grain size and structure of failed lithium-ion battery cathode materials using the molten salt method, the problems of long regeneration processes and low efficiency were solved, resulting in high-performance single-crystal high-voltage cathode materials suitable for high-energy-density lithium-ion batteries.
Patent Information
- Application Number
- CN202511564260.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-30
- Publication Date
- 2026-01-30
AI Technical Summary
Existing technologies are insufficient for effectively recycling cathode materials from failed lithium-ion batteries, resulting in substandard electrochemical performance. Furthermore, traditional recycling processes are lengthy, economically inefficient, and have a significant environmental impact.
The molten salt method is used for size control to transform the cathode material of a failed battery into a single-crystal high-voltage cathode. By controlling the grain size and structure, mild lithium replenishment can be achieved, reducing energy consumption and cost, and improving electrochemical performance.
An efficient and environmentally friendly regeneration process was achieved, and the resulting single-crystal high-voltage cathode material exhibits excellent electrochemical performance and cycle stability under high voltage, making it suitable for high-energy-density lithium-ion batteries.
Smart Images

Figure CN121428646A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the field of electrochemistry and waste electronic product recycling, and particularly relates to a direct regeneration method for directly optimizing and regenerating a failed battery positive electrode into a single-crystal high-voltage positive electrode and application, and the material can be used as a lithium ion battery positive electrode active material. BACKGROUND
[0002] LiNi x Co y Mn z O2 (NCM) as a kind of lithium ion battery positive electrode material, because of its high energy density, high working voltage, low cost and environmental friendliness, it is vigorously promoted in the field of electric vehicles and energy storage. But because of its limited life, when the capacity is lower than 80%, it will be eliminated from electric vehicles, and when the capacity is lower than 50%, it will be eliminated from the field of energy storage. At present, a large number of failed batteries have emerged in the market, and the growth is explosive year by year. The failed batteries contain a large amount of transition metals and have economic benefits and environmental threats. Therefore, it is urgent to realize the recycling of waste lithium ion batteries with high economic benefits and low environmental threats. Direct optimization and regeneration is an ideal choice for recycling waste lithium battery positive electrodes due to its short process flow and high product added value The traditional direct regeneration process only considers the missing lithium in the material and performs lithium supplementation. Although the capacity is improved, the overall electrochemical performance is difficult to meet the increasing performance demand of lithium batteries. Lithium batteries are developing towards high energy density, which requires both capacity and voltage to be improved. However, with the increase of the cut-off voltage, the stress accumulated in the material due to H1-H2-H3 phase transition increases. This may cause lattice dislocation, particle breakage, and current collector peeling during the cycle process. Therefore, we achieve the two purposes of polycrystal to single crystal transformation and grain size control in the regeneration process. Effectively release the stress in the cycle process, reduce stress accumulation, avoid lattice dislocation, particle breakage, and current collector peeling during the cycle process, which affect the high voltage performance and cycle stability of the material. Therefore, for the regenerated NCM positive electrode material, single crystal structure and grain size are the key requirements for optimizing high voltage performance and realizing high energy density lithium ion battery energy storage.
[0003] The recycling process of NCM material mainly includes hydrometallurgy and direct regeneration. The hydrometallurgy process involves pretreatment, leaching, extraction, precipitation, separation, and drying, and has a long process flow, large amount of wastewater, and low economic benefit of the product. Direct regeneration can solve the above problems, but different regeneration methods have great differences in economic and environmental benefits due to different lithium supplementation temperatures and different electrochemical performances of the products. The molten salt method we use selects the appropriate proportion through the binary phase diagram to reduce the melting point temperature and achieve mild temperature lithium supplementation. By controlling the grain size, the high voltage performance of the regenerated product is improved, and the added value of the product is improved. Finally, the double high-efficiency regeneration of economy and benefit is realized. SUMMARY
[0004] The present application aims to provide a direct regeneration method and application for directly optimizing the failed battery positive electrode to single crystal high-voltage positive electrode through size regulation, which has simple operation, mild lithium supplement temperature, and cheap and easily available raw materials. The obtained regenerated positive electrode material is used as a high-voltage lithium ion battery positive electrode active material and shows good electrochemical performance, which can be used to solve the problems of harmless and high economic efficiency recovery of failed battery positive electrode material, and poor cycle stability and high pressure of regenerated positive electrode material.
[0005] To achieve the above-mentioned purpose, the present application provides a direct regeneration method for failed battery positive electrode material based on size regulation, comprising the following steps: (a) mixing lithium nitrate and lithium hydroxide according to a predetermined molar ratio to prepare a molten salt; (b) mixing the molten salt obtained in step (a) with the failed battery polycrystalline NCM positive electrode material according to a predetermined molar ratio and ball milling to obtain a uniform mixture; (c) pre-sintering treatment of the mixture obtained in step (b) in an oxygen-containing atmosphere to realize lithium supplement regeneration; (d) cooling, washing and drying the lithium-supplemented material obtained in step (c); (e) adding lithium source and tungsten source to the dried material obtained in step (d) and grinding to mix uniformly; (f) high-temperature annealing treatment of the mixture obtained in step (e) to realize grain size regulation and structure optimization, and obtain a single crystal high-voltage positive electrode material. Further, the molar ratio of lithium nitrate to lithium hydroxide in step (a) is 6:4. According to the binary phase diagram of lithium nitrate and lithium hydroxide, when the molar ratio of lithium nitrate to lithium hydroxide is 6:4, the melting point of the eutectic salt is about 176°C, which is much lower than the melting point of lithium nitrate (LiNO3) 264°C and the melting point of lithium hydroxide (LiOH) about 462°C. Lower melting point can save energy consumption in the regeneration process, reduce cost and carbon emission. The molar ratio of molten salt to waste polycrystalline NCM positive electrode material in step (b) is 4:1. The molten salt acts as a lithium supplement solvent. When the proportion of molten salt is too low, it cannot completely cover the electrode particles and cannot provide sufficient lithium source. On the contrary, when the proportion of molten salt is too high, it will cause excessive lithium residue on the surface of the electrode particles, which is not conducive to the electrode interface reaction. In addition, too much lithium salt is not economical and practical.
[0006] Further, the process conditions of the pre-sintering treatment in step (c) are as follows: in an air atmosphere, heating at a heating rate of 1-5°C / min to 300-500°C, and holding for 2-5 hours.
[0007] Further, the washing in step (d) is washing with water and ethanol in sequence, and the drying is drying at 50-80℃ for 2-10 hours.
[0008] Further, the lithium source in step (e) is one or more of lithium carbonate, lithium hydroxide and lithium nitrate, and the addition amount is 1-5 wt% of the total mass of the dried material; the tungsten source is tungsten trioxide (WO33), and the addition amount is 1-1.5 mol% of the total mass of the dried material. Compared with the traditional solid-phase sintering method, the solid-phase sintering method is a solid-solid reaction, and the reaction only occurs at the solid-solid interface, which is affected by the contact area. The molten salt method is a solid-liquid reaction, and the contact area between the solid electrode particles and the liquid molten salt is large, which is beneficial to improve the kinetics of the reaction. In addition, the molten salt has high lithium ion concentration and high ion transport capacity, which are all beneficial to the lithium supplement process and promote the conversion of the electrode particles from polycrystal to single crystal. Most importantly, the introduction of tungsten, which is a high-valence metal with +VI valence, can reduce the surface energy of the electrode particles, so that the size of the regenerated electrode particles is smaller.
[0009] Further, the process conditions of the high-temperature annealing treatment in step (f) are annealing at 700-900℃ for 3-8 hours.
[0010] Further, the ball milling time in step (b) is 1-5 hours.
[0011] The application provides a single-crystal high-voltage cathode material prepared by the above method, characterized in that the cathode material is a single-crystal particle with a layered structure, the grain size is 0.5-1μm, and the ratio of the diffraction peak intensity of the (003) crystal face to the (104) crystal face in the XRD pattern is greater than 1.2.
[0012] The application also provides a lithium ion battery, wherein the cathode active material comprises the single-crystal high-voltage cathode material according to claim 8.
[0013] Further, the working voltage window of the battery is 2.5V to 4.4V or 2.5V to 4.5V.
[0014] The application has the following beneficial effects: The direct regeneration method for directly optimizing the failed battery positive electrode to single crystal high-voltage positive electrode through size regulation has the following advantages: 1) high environmental benefits of the regeneration process, specifically including a short process flow, mild lithium supplement temperature, low energy consumption, and low waste water and waste gas generation; 2) high economic benefits of the regeneration process, specifically including a short process flow, low equipment requirements, low lithium source price for lithium supplement, low energy consumption in the regeneration process, and high added value of the obtained single crystal high-voltage positive electrode material product; 3) the high-voltage single crystal positive electrode material obtained by regeneration has a stable structure, and the single crystal particles with appropriate size obtained by regulation are beneficial to stress release in the cycle process, reduce stress accumulation, avoid lattice dislocation, particle breakage, and current collector peeling in the cycle process; 4) the high-voltage single crystal positive electrode material obtained by regeneration has excellent electrochemical performance, and the regenerated material shows high specific capacity, cycle stability and energy density due to the stable material structure, and is more suitable for high-voltage working conditions. It can be applied at a high cut-off voltage of 4.4 V and 4.5 V. When the raw material is waste NCM622, the regenerated product has a high reversible charge-discharge specific capacity (165 mAh g -1 ) at a current density of 0.5 C and a cut-off voltage of 2.5-4.4 V. In addition, the regeneration process of the present application is simple, the high-valence transition metal is adjusted to regulate the grain size through a simple molten salt method, the scale-up experiment can be quantitatively produced, and it is beneficial to market promotion. BRIEF DESCRIPTION OF DRAWINGS
[0015] Figure 1 The figure is a schematic diagram of the regeneration strategy of the present application.
[0016] Figure 2 The figure is an X-ray diffraction (XRD) spectrum of the high-voltage single crystal NCM positive electrode material obtained by size regulation and regeneration.
[0017] Figure 3 The figure is a Raman spectrum analysis (Raman) graph of the high-voltage single crystal NCM positive electrode material obtained by size regulation and regeneration. Figure 4 The figure is a scanning electron microscope (SEM) graph of the high-voltage single crystal NCM positive electrode material obtained by size regulation and regeneration.
[0018] Figure 5 The figure is a charge-discharge voltage distribution graph of the high-voltage single crystal NCM positive electrode material obtained by size regulation and regeneration at a current density of 0.5 C and a voltage window of 2.5-4.4 V.
[0019] Figure 6 The figure is a charge-discharge cycle graph of the high-voltage single crystal NCM positive electrode material obtained by size regulation and regeneration at a current density of 0.5 C.
[0020] Figure 7is a scanning electron microscope (SEM) image of a positive electrode material prepared by the comparative example. DETAILED DESCRIPTION
[0021] The technical solutions of the present application will be further described in detail below in conjunction with specific embodiments, but do not constitute any limitation on the present application.
[0022] Example 1: Regeneration of single crystal high pressure positive electrode with failed battery NCM622 positive electrode material as raw material Raw material pretreatment: Take the failed battery NCM622 positive electrode sheet of the retired electric vehicle, after disassembly and cutting, remove the aluminum foil current collector by ultrasonic stripping (solvent is N-methyl pyrrolidone) to obtain waste polycrystalline NCM622 powder (particle size 5-10 μm, capacity decay to 75% of initial capacity); Molten salt preparation: weigh 6 mol lithium nitrate (analytical pure, purity ≥ 99.0%) and 4 mol lithium hydroxide (analytical pure, purity ≥ 98.0%), put into agate mortar and grind for 10 min, mix uniformly to obtain binary molten salt; Raw material mixing and ball milling: according to the molar ratio of molten salt: failed battery NCM622 = 4:1, weigh 4 mol of the above molten salt and 1 mol of waste NCM622 powder, add into a planetary ball mill, ball-to-material ratio is 10:1, rotation speed is 300 r / min, ball mill for 1 h until mixed uniformly; Pre-sintering lithium supplement: transfer the ball-milled mixture into an α-alumina crucible, put into a muffle furnace, set air atmosphere, heating rate is 5 ℃ / min, heat to 400 ℃ and keep for 4 h; after the heat preservation is over, take out the crucible when the furnace temperature drops to 80 ℃; Washing and drying: transfer the pre-sintered material into a beaker, add 500 mL of deionized water, stir for 30 min and then filter; repeat water washing for 3 times, and then wash with 200 mL of anhydrous ethanol for 1 time, after filtration, transfer the filter cake into a 80 ℃ air oven and dry for 12 h until constant weight to obtain the pretreated regenerated material; Size control and annealing: add 5 wt% of lithium carbonate (analytical pure) and 1.5 mol% of tungsten trioxide (analytical pure) into the pretreated regenerated material, grind in an agate mortar for 30 min until no obvious particles; transfer the mixture into an alumina crucible, put into a muffle furnace, heat to 850 ℃ under air atmosphere and keep for 6 h; Product grinding: after the annealing is over, naturally cool to room temperature, take out the material, grind with a planetary ball mill at a speed of 200 r / min for 1 h to obtain white powder of single crystal high pressure NCM positive electrode material.
[0023] Performance test Crystal structure test: X-ray diffraction (XRD, Cu Kα rays) was used for testing. The results are shown in Figure 2. The XRD pattern of the recycled material is consistent with the standard NCM pattern of Fd-3m space group. (003) / (104)=1.68, indicating a low lithium-nickel mixing rate. Raman spectroscopy test: The test was conducted using a Raman spectrometer (excitation wavelength 532 nm), and the results are as follows: Figure 3 As shown, at 493cm -1 (Eg peak) and 587cm -1 The presence of a characteristic NCM peak at (A1g peak) confirms successful regeneration of the layered structure; Microscopic morphology testing: Observation was performed using a scanning electron microscope (SEM, accelerating voltage 20kV), and the results are as follows: Figure 4 As shown, the recycled material consists of single-crystal particles of 0.5-1 μm with a smooth surface. This differs from the cathode particles of failed batteries and traditional lithium-ion batteries, which are typically polycrystalline spherical particles with a diameter of 5 to 10 μm. The single-crystal particles with a grain size of 0.5-1 μm are beneficial for releasing stress during cycling, reducing stress accumulation, and preventing problems such as lattice dislocation, particle breakage, and current collector delamination during cycling.
[0024] Electrochemical performance testing: Recycled materials, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1 and coated onto aluminum foil to prepare a positive electrode. This positive electrode was then assembled into a coin cell with a lithium metal negative electrode, a Celgard 2400 separator, and a 1 mol / L LiPF6 / EC-DMC-EMC electrolyte (volume ratio 1:1:1). Tests were conducted at a current density of 0.5C and a voltage window of 2.5-4.4V. The results are as follows: Figure 5 , Figure 6 As shown, the initial charge-discharge specific capacity is 165 mAh / g, and the capacity retention rate after 100 cycles is 86%, demonstrating excellent high-voltage cycling stability. This is attributed to the fact that the regenerated material has a single-crystal structure and its grain size has been controlled, ranging from 0.5 to 1 μm. This facilitates the release of stress during cycling, reduces stress accumulation, and avoids problems such as lattice dislocation, particle breakage, and current collector delamination during cycling.
[0025] Comparative Example 1 The difference from Example 1 is that tungsten trioxide is replaced with alumina; the other processes are the same as in Example 1. (See attached...) Figure 7 As can be seen, the final material obtained is a polycrystalline spherical material.
[0026] Comparative Example 2: The difference from Example 1 is that WO3 is replaced by Nb2O5, and other processes are the same as those in Example 1. For example, the single-crystal NCM positive electrode material obtained in the example has a discharge specific capacity of 152 mAh / g at a current density of 0.5C, and a discharge specific capacity of 128 mAh / g after 100 cycles, with a capacity retention rate of 84%. Through analysis, it can be inferred that although Nb can regulate the grain, since Nb is a 5-valence metal and W is a 6-valence metal, the surface formation energy of the Nb-modified material is higher than that of W, so the size regulation is not in place. Stress accumulation still occurs during charging and discharging.
[0027] Comparative Example 3: The difference from Example 1 is that the addition amount of WO3 is 5 mol%, and other processes are the same as those in Example 1.
[0028] For example, the single-crystal NCM positive electrode material obtained in the example has a discharge specific capacity of 158 mAh / g at a current density of 0.5C, and a discharge specific capacity of 124 mAh / g after 100 cycles, with a capacity retention rate of 78%. Through analysis, it can be inferred that W is a 6-valence metal, Ni in the NCM material is 2-valence and 3-valence, and excessive W is introduced. In order to balance the charge, the 3-valence Ni will be converted into 2-valence nickel. The 2-valence nickel is similar in radius to lithium ions, and is easy to cause lithium-nickel mixing, so as to increase polarization, thereby affecting the electrochemical performance of the battery.
[0029] Comparative Example 4: The difference from Example 1 is that the addition amount of WO3 is 0.5 mol%, and other processes are the same as those in Example 1. For example, the single-crystal and polycrystal mixed NCM positive electrode material obtained in the example has a discharge specific capacity of 149 mAh / g at a current density of 0.5C, and a discharge specific capacity of 122 mAh / g after 100 cycles, with a capacity retention rate of 82%. Through analysis, it can be inferred that the doping amount is insufficient, and the advantages of doping cannot be reflected.
[0030] Finally, the method of the present application is only a preferred embodiment, and is not used to limit the protection scope of the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A method for direct regeneration of failed cathode material of a battery based on size regulation, characterized in that, The method comprises the following steps: (a) mixing lithium nitrate and lithium hydroxide in a predetermined molar ratio to prepare a molten salt; (b) mixing the molten salt obtained in step (a) with a spent battery polycrystalline NCM positive electrode material in a predetermined molar ratio and performing ball milling to obtain a uniform mixture; (c) performing a pre-sintering treatment on the mixture obtained in step (b) in an oxygen-containing atmosphere to realize lithium supplement regeneration; (d) cooling, washing and drying the lithium-supplemented material obtained in step (c); (e) adding a lithium source and a tungsten source to the dried material obtained in step (d) and grinding to mix uniformly; (f) performing a high-temperature annealing treatment on the mixture obtained in step (e) to realize grain size control and structure optimization, thereby obtaining a single-crystal high-voltage positive electrode material.
2. The method of claim 1, wherein, The molar ratio of lithium nitrate to lithium hydroxide in step (a) is 6:4; and the molar ratio of the molten salt to the spent battery polycrystalline NCM positive electrode material in step (b) is 4:
1.
3. The method of claim 1, wherein, The process conditions for the pre-sintering treatment in step (c) are as follows: heating to 300-500℃ at a heating rate of 1-5℃ / min in an air atmosphere, and maintaining the temperature for 2-5 hours.
4. The method of claim 1, wherein, The washing in step (d) is washing with water and ethanol in sequence, and the drying is drying at 50-80℃ for 2-10 hours.
5. The method of claim 1, wherein, The lithium source in step (e) is one or more of lithium carbonate, lithium hydroxide and lithium nitrate, and the addition amount is 1-5 wt% of the total mass of the dried material; and the tungsten source is tungsten trioxide (WO33), and the addition amount is 1-1.5 mol%.
6. The method of claim 1, wherein, The process conditions for the high-temperature annealing treatment in step (f) are as follows: annealing at 700-900℃ for 3-8 hours.
7. The method of claim 1, wherein, The ball milling time in step (b) is 1-5 hours.
8. A single-crystalline high-voltage cathode material prepared by the method of any one of claims 1 to 7, characterized in that, The positive electrode material is a single-crystal particle with a layered structure, the grain size is 0.5-1μm, and the ratio of the diffraction peak intensity of the (003) crystal face to the (104) crystal face in the XRD pattern is greater than 1.
2.
9. A lithium-ion battery, characterized by The positive electrode active material comprises the single-crystal high-voltage positive electrode material according to claim 8.
10. The lithium-ion battery of claim 9, wherein, The working voltage window of the battery is 2.5V to 4.4V or 2.5V to 4.5V.
Citation Information
Cited By
Direct regeneration method of ternary positive electrode waste material, regenerated ternary positive electrode material and lithium ion battery
CN122068163A