Semiconductor laser with light field expansion layer and preparation method thereof

By inserting N-type and P-type optical field extension layers into a semiconductor laser, the optical field distribution is changed, the problem of fast-axis far-field divergence angle is solved, and small divergence angle and high-efficiency electro-optic conversion are achieved.

CN121507549APending Publication Date: 2026-02-10Shandong Huaguang Optoelectronics Co. Ltd.
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511527746.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-24
Publication Date
2026-02-10

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively reduce the fast-axis far-field divergence angle of semiconductor lasers. Thick waveguide layers increase voltage and affect electro-optic conversion efficiency, while asymmetric waveguide structures are prone to high-order mode lasing and deterioration of the divergence angle.

Method used

An N-type optical field extension layer is inserted between the N-type confinement layer and the N-type waveguide layer, and a P-type optical field extension layer is inserted between the P-type confinement layer and the P-type waveguide layer. The optical field is extended by varying the refractive index, thereby increasing the range of optical field distribution.

Benefits of technology

This reduces the fast-axis far-field divergence angle of semiconductor lasers, improves electro-optic conversion efficiency, and avoids higher-order mode lasing and increased internal losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121507549A_ABST
    Figure CN121507549A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor laser with a light field expansion layer and a preparation method thereof, and the semiconductor laser sequentially comprises a substrate, a buffer layer, an N-type limiting layer, an N-type waveguide layer, an active layer, a P-type waveguide layer, a P-type limiting layer, and an ohmic contact layer along the epitaxial growth direction. Wherein an N-type light field expansion layer with gradually-changed components is inserted between an N-type limiting layer and an N-type waveguide layer, and a P-type light field expansion layer with gradually-changed components is inserted between a P-type waveguide layer and a P-type limiting layer, so that the distribution of a light field in a device is regulated and controlled, and the light field distribution range in the laser is enlarged; therefore, the semiconductor laser can obtain a lower fast-axis far-field divergence angle on the basis of using a thinner waveguide layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a semiconductor laser with an optical field extension layer and its fabrication method, belonging to the field of semiconductor laser technology. Background Technology

[0002] Semiconductor lasers are widely used in optical communication, fiber optic sensing, and medical aesthetics. In recent years, the requirements for signal transmission distance have been increasing, and the precision of laser surgery has been continuously improving. In order to achieve higher fiber coupling efficiency and energy density, the market's requirements for semiconductor laser specifications are increasingly focused on the parameter of smaller fast-axis far-field divergence angle. Therefore, effectively reducing the fast-axis far-field divergence angle of semiconductor lasers has very important commercial value.

[0003] Existing technologies typically employ thick waveguide layers to reduce the fast-axis far-field divergence angle of semiconductor lasers. Thicker waveguide layers broaden the distribution range of the optical field within the device, effectively reducing the fast-axis far-field divergence angle. However, since waveguide layers are generally lightly doped or undoped, excessively thick waveguide layers significantly increase the voltage of the semiconductor laser, affecting its electro-optical conversion efficiency. Another approach uses asymmetric waveguide structures to reduce losses and the fast-axis far-field divergence angle. However, as the asymmetry of the semiconductor laser waveguide layer increases, the mode gain of higher-order modes also increases, making the device prone to higher-order mode lasing. When higher-order mode lasing occurs in the semiconductor laser, the fast-axis far-field divergence angle deteriorates significantly, internal losses increase sharply, and output power and electro-optical conversion efficiency decrease accordingly. Therefore, effectively reducing the fast-axis far-field divergence angle of semiconductor lasers remains a current research focus. This invention addresses this issue. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a semiconductor laser with an optical field extension layer and its fabrication method, thereby solving the problem of effectively reducing the fast-axis far-field divergence angle of semiconductor lasers.

[0005] Terminology Explanation: MOCVD refers to metal-organic chemical vapor deposition; MO refers to metal-organic compounds.

[0006] TMGa, TMAl, and TMIn refer to trimethylgallium, trimethylaluminum, and trimethylindium, respectively, and are all raw materials for epitaxial growth, along with AsH3.

[0007] Example of expressing doping concentration: Doping concentration 1E16 cm⁻¹ -3 ~5E18 cm -3 This refers to a doping concentration of 1×10 16 cm -3 ~5 ×10 18 cm-3 .

[0008] Substrate angle: refers to the deviation of the normal direction of the (100) crystal plane from the substrate angle. <111> The angle of crystal orientation.

[0009] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a semiconductor laser with an optical field spreading layer, comprising, sequentially along the epitaxial growth direction, a substrate, a buffer layer, an N-type confinement layer, an N-type waveguide layer, an active layer, a P-type waveguide layer, a P-type confinement layer, and an ohmic contact layer, wherein a P-type ohmic electrode is disposed above the ohmic contact layer, and an N-type ohmic electrode is disposed below the substrate, characterized in that: An N-type optical field spreading layer is inserted between the N-type confinement layer and the N-type waveguide layer. The N-type optical field spreading layer is composed of Al. x3 Ga 1-x3 As material is formed, where x3 changes linearly between 0 and 0.35, from low to high values; A P-type optical field spreading layer is inserted between the P-type waveguide layer and the P-type confinement layer. The P-type optical field spreading layer is composed of Al. x7 Ga 1-x7 As material is formed, where x7 changes linearly between 0 and 0.35, from high to low values.

[0010] According to a preferred embodiment of the present invention, x3 in the N-type optical field extension layer is linearly varied from 0.2 to 0.3.

[0011] According to a preferred embodiment of the present invention, the N-type optical field extension layer is N-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18cm -3 Further preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm -3 The most preferred doping concentration is 3E16 cm⁻¹. -3 .

[0012] According to the present invention, the thickness of the N-type optical field extension layer is preferably 0.1 μm to 0.5 μm; more preferably, the thickness is 0.2 μm to 0.4 μm; and most preferably, the thickness is 0.33 μm.

[0013] According to a preferred embodiment of the present invention, x7 in the P-type optical field extension layer is linearly varied from 0.3 to 0.2.

[0014] According to a preferred embodiment of the present invention, the P-type optical field spreading layer is P-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18cm -3 Further preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm-3 The most preferred doping concentration is 3E16 cm⁻¹. -3 .

[0015] According to the present invention, the thickness of the P-type optical field extension layer is preferably 0.1 μm to 0.5 μm; more preferably, the thickness is 0.2 μm to 0.4 μm; and most preferably, the thickness is 0.33 μm.

[0016] According to a preferred embodiment of the present invention, the substrate material is GaAs, and the substrate angle is 0°, 10°, or 15°; more preferably, the substrate angle is 0°.

[0017] According to a preferred embodiment of the present invention, the buffer layer is made of Al x1 Ga 1-x1 As material is formed, wherein 0 ≤ x1 ≤ 0.05, N-type doped, and the doping concentration is 1E18 cm⁻¹. -3 ~5E18 cm -3 The thickness is 100 nm to 300 nm; more preferably, 0 ≤ x1 ≤ 0.03, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 200 nm to 300 nm; the most preferred value is x1=0, and the doping concentration is 1E18 cm⁻¹. -3 The thickness is 300nm.

[0018] According to a preferred embodiment of the present invention, the N-type confinement layer is made of Al x2 Ga 1-x2 As material is formed, wherein 0.35 ≤ x² ≤ 1, N-type doped, and the doping concentration is 5E¹⁷ cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 2 μm; more preferably, 0.35 ≤ x2 ≤ 0.5, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 1 μm to 1.5 μm; the most preferred value is x2 = 0.40, with a doping concentration of 1E18 cm⁻¹. -3 The thickness is 1.3 μm.

[0019] According to a preferred embodiment of the present invention, the N-type waveguide layer is made of Al x4 Ga 1-x4 As material is formed, wherein 0 ≤ x ≤ 0.4, N-type doped, and the doping concentration is 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0 ≤ x 4 ≤ 0.3, and the doping concentration is 1E16 cm⁻¹. -3~8E16 cm -3 The thickness is 0.1 μm to 0.3 μm; the most preferred value is x4 = 0.2, with a doping concentration of 3E16 cm⁻¹. -3 The thickness is 0.12 μm.

[0020] According to a preferred embodiment of the present invention, the active layer is composed of Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 The Al is composed of overlapping quantum well layers with an overlap period of 1 to 5, wherein 0 ≤ x5 ≤ 0.4, 0 ≤ y1 ≤ 0.5, and the Al x5 Ga 1-x5 As the band gap of the quantum barrier layer is greater than In y1 Ga 1-y1 As is the bandgap width of the quantum well layer; more preferably, the overlap period is 1~3, 0.1≤x5≤0.3, 0.1≤y1≤0.2; most preferably, the overlap period is 1, x5=0.2, y1=0.14; Preferably, the Al x5 Ga 1-x5 The thickness of the As quantum barrier layer is 1nm~50nm, and it can be undoped, p-type doped, or n-type doped. y1 Ga 1-y1 The thickness of the As quantum well layer is 1 nm to 10 nm, and it is undoped; more preferably, the Al... x5 Ga 1- x5 The thickness of the As quantum barrier layer is 10nm~30nm, and it is undoped. y1 Ga 1-y1 The thickness of the As quantum well layer is 4nm~10nm; most preferably, the Al... x5 Ga 1-x5 The thickness of the As quantum barrier layer is 20 nm, and the In y1 Ga 1-y1 The thickness of the As quantum well layer is 7 nm.

[0021] According to a preferred embodiment of the present invention, the P-type waveguide layer is made of Al x6 Ga 1-x6 As material is formed, wherein 0 ≤ x6 ≤ 0.4, p-type doped, and the doping concentration is 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0.1 ≤ x6 ≤ 0.3, and the doping concentration is 1E16 cm⁻¹. -3 ~5E16 cm -3The thickness is 0.1 μm to 0.3 μm; the most preferred value is x6=0.2, and the doping concentration is 3E16 cm⁻¹. -3 The thickness is 0.12 μm.

[0022] According to a preferred embodiment of the present invention, the P-type confinement layer is made of Al x8 Ga 1-x8 As material is formed, wherein 0.35 ≤ x 8 ≤ 1, p-type doped, and the doping concentration is 5E17 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 1.5 μm; more preferably, 0.35 ≤ x 8 ≤ 0.5, and the doping concentration is 8E17cm. -3 ~4E18 cm -3 The thickness is 1 μm to 1.5 μm; the most preferred value is x8 = 0.40, with a doping concentration of 1E18cm. -3 The thickness is 1.3 μm.

[0023] According to a preferred embodiment of the present invention, the ohmic contact layer is formed of GaAs material, p-type doped, with a doping concentration of 9E18cm⁻¹. -3 ~5E19 cm -3 The thickness is 20 nm to 400 nm; more preferably, the doping concentration is 1E19 cm⁻¹. -3 ~5E19 cm -3 The thickness is 100 nm to 300 nm; most preferably, the doping concentration is 4.5E19 cm⁻¹. -3 The thickness is 200 nm.

[0024] According to a preferred embodiment of the present invention, the P-type ohmic electrode is formed of Ni / Au, Cr / Au, Pt / Au or Ni / Al material; more preferably, the P-type ohmic electrode is formed of Ni / Au material.

[0025] According to a preferred embodiment of the present invention, the N-type ohmic electrode is formed of Al / Au, Cr / Au, or Ti / Al / Ti / Au material; more preferably, the N-type ohmic electrode is formed of Cr / Au material.

[0026] Secondly, the present invention also provides a method for fabricating the above-mentioned semiconductor laser with an optical field extension layer.

[0027] A method for fabricating a semiconductor laser with an optical field spreading layer includes the following steps: S1. In the MOCVD reactor, the substrate is heated to 710-750°C in an H2 environment for baking, and then AsH3 is introduced for high-temperature heat treatment to remove foreign matter and water and oxygen from the substrate surface. S2. The temperature is lowered to 700-720℃, and TMAl, TMGa and AsH3 are introduced to grow a buffer layer on the substrate. S3. The temperature is lowered to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow an N-type confinement layer on the buffer layer. S4. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type optical field extension layer on the N-type confinement layer; S5. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type waveguide layer on the N-type optical field extension layer. S6. The temperature is lowered to 540–580°C, and TMAl, TMGa, and AsH3 are introduced to grow Al on the N-type waveguide layer. x5 Ga 1- x5 As a quantum barrier layer, then TMI, TMGa, and AsH3 are introduced into Al. x5 Ga 1-x5 As quantum barrier layer grown In y1 Ga 1-y1 As a quantum well layer, repeat the above process, overlapping Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 As a quantum well layer forms an active layer; S7. The temperature is raised to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow a P-type waveguide layer on the active layer. S8. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type optical field extension layer on the P-type waveguide layer. S9. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type confinement layer on the P-type optical field extension layer. S10, the temperature is lowered to 540-560℃, TMGa and AsH3 are introduced, and an ohmic contact layer is grown on the P-type confinement layer; S11. A P-type ohmic electrode is deposited on the ohmic contact layer to thin the substrate, and an N-type ohmic electrode is deposited below the substrate.

[0028] The beneficial effects of this invention are: The semiconductor laser of this invention inserts an N-type optical field extension layer between an N-type confinement layer and an N-type waveguide layer, and a P-type optical field extension layer between a P-type confinement layer and a P-type waveguide layer. By changing the gradually varying refractive indices of the N-type and P-type optical field extension layers, the distribution state of the optical field is altered, causing the optical field confined within the N-type and P-type waveguide layers to extend into the N-type and P-type optical field extension layers, thereby increasing the distribution range of the optical field within the device. This reduces the fast-axis far-field divergence angle of the semiconductor laser, achieving a small fast-axis far-field divergence angle output. Attached Figure Description

[0029] Figure 1 This is a schematic diagram of the epitaxial structure of the semiconductor laser of the present invention; in the figure: 101, N-type ohmic electrode; 102, substrate; 103, buffer layer; 104, N-type confinement layer; 105, N-type optical field extension layer; 106, N-type waveguide layer; 107, active layer; 108, P-type waveguide layer; 109, P-type optical field extension layer; 110, P-type confinement layer; 111, ohmic contact layer; 112, P-type ohmic electrode.

[0030] Figure 2 The diagram shows the refractive index and optical field distribution of the semiconductor laser used in this invention as a comparative example. The dashed line represents the refractive index distribution; the solid line represents the optical field intensity distribution; the vertical axis (left) represents the refractive index, the vertical axis (right) represents the intensity (au), and the horizontal axis represents the relative position (μm).

[0031] Figure 3 This is a diagram showing the refractive index and optical field distribution of the semiconductor laser in Embodiment 1 of the present invention. The dashed line represents the refractive index distribution; the solid line represents the optical field intensity distribution; the vertical axis (left) represents the refractive index, the vertical axis (right) represents the intensity (au), and the horizontal axis represents the relative position (μm).

[0032] Figure 4 This is a comparison diagram of the fast-axis far-field divergence angles of the semiconductor lasers in Embodiment 1 and the comparative example of the present invention. The vertical axis (left) represents intensity (au), and the horizontal axis represents angle (°). Detailed Implementation

[0033] The present invention will be further described below with reference to embodiments and accompanying drawings, but is not limited thereto. The described embodiments are some embodiments of the present invention. Based on these embodiments, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] In the description of this invention, it should be noted that the terms "upper," "lower," "left," "right," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and should not be construed as limiting the invention. Furthermore, in this embodiment, "semiconductor laser device" has the same meaning as "semiconductor laser device," "device," and "laser."

[0035] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. Unless otherwise specified in the embodiments of the present invention, all techniques existing in the art can be used.

[0036] One embodiment of the present invention, such as Figure 1 As shown, a semiconductor laser with an optical field extension layer includes, in sequence along the epitaxial growth direction, a substrate 102, a buffer layer 103, an N-type confinement layer 104, an N-type optical field extension layer 105, an N-type waveguide layer 106, an active layer 107, a P-type waveguide layer 108, a P-type optical field extension layer 109, a P-type confinement layer 110, and an ohmic contact layer 111. A P-type ohmic electrode 112 is disposed above the ohmic contact layer 111, and an N-type ohmic electrode 101 is disposed below the substrate 102.

[0037] The material of the N-type optical field extension layer 105 is Al. x3 Ga 1-x3 As, where x3 linearly varies between 0 and 0.35, from a low value to a high value. Preferably, x3 linearly varies from 0.2 to 0.3.

[0038] The N-type optical field extension layer is N-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm -3 The thickness is 0.2 μm to 0.4 μm; most preferably, the doping concentration is 3E16 cm⁻¹. -3 The thickness is 0.33 μm.

[0039] The material of the P-type optical field extension layer 109 is Al. x7 Ga 1-x7 As, where x7 linearly varies between 0 and 0.35, from a high value to a low value; preferably, x7 linearly varies from 0.3 to 0.2.

[0040] The P-type optical field extension layer is P-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18 cm -3The thickness is 0.1 μm to 0.5 μm; more preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm -3 The thickness is 0.2 μm to 0.4 μm; most preferably, the doping concentration is 3E16 cm⁻¹. -3 The thickness is 0.33 μm.

[0041] The substrate 102 is made of GaAs, and the substrate angle is 0°, 10°, or 15°. Preferably, the substrate 102 has an angle of 0°.

[0042] The material of the buffer layer 103 is Al. x1 Ga 1-x1 As, where 0 ≤ x1 ≤ 0.05, is an N-type doped material with a doping concentration of 1E18 cm⁻¹. -3 ~5E18 cm -3 The thickness is 100 nm to 300 nm; more preferably, 0 ≤ x1 ≤ 0.03, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 200 nm to 300 nm; the most preferred value is x1=0, and the doping concentration is 1E18 cm⁻¹. -3 The thickness is 300nm.

[0043] The material of the N-type confinement layer 104 is Al. x2 Ga 1-x2 As, where 0.35 ≤ x² ≤ 1, is N-type doped with a doping concentration of 5E¹⁷ cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 2 μm; more preferably, 0.35 ≤ x2 ≤ 0.5, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 1 μm to 1.5 μm; the most preferred value is x2 = 0.40, with a doping concentration of 1E18 cm⁻¹. -3 The thickness is 1.3 μm.

[0044] The material of the N-type waveguide layer 106 is Al. x4 Ga 1-x4 As, where 0 ≤ x⁴ ≤ 0.4, is an N-type doped material with a doping concentration of 1E¹⁶ cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0 ≤ x 4 ≤ 0.3, and the doping concentration is 1E16cm. -3 ~8E16 cm -3The thickness is 0.1 μm to 0.3 μm; the most preferred value is x4 = 0.2, with a doping concentration of 3E16cm. -3 The thickness is 0.12 μm.

[0045] The active layer is composed of Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 The Al is composed of overlapping quantum well layers with an overlap period of 1 to 5, wherein 0 ≤ x5 ≤ 0.4, 0 ≤ y1 ≤ 0.5, and the Al x5 Ga 1-x5 As the band gap of the quantum barrier layer is greater than In y1 Ga 1- y1 As is the bandgap width of the quantum well layer; more preferably, the overlap period is 1~3, 0.1≤x5≤0.3, 0.1≤y1≤0.2; most preferably, the overlap period is 1, x5=0.2, y1=0.14; Preferably, the Al x5 Ga 1-x5 The thickness of the As quantum barrier layer is 1nm~50nm, and it can be undoped, p-type doped, or n-type doped. y1 Ga 1-y1 The thickness of the As quantum well layer is 1 nm to 10 nm, and it is undoped; more preferably, the Al... x5 Ga 1- x5 The thickness of the As quantum barrier layer is 10nm~30nm, and it is undoped. y1 Ga 1-y1 The thickness of the As quantum well layer is 4nm~10nm; most preferably, the Al... x5 Ga 1-x5 The thickness of the As quantum barrier layer is 20 nm, and the In y1 Ga 1-y1 The thickness of the As quantum well layer is 7 nm.

[0046] The material of the P-type waveguide layer 108 is Al. x6 Ga 1-x6 As, where 0 ≤ x6 ≤ 0.4, is a P-type doped material with a doping concentration of 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0.1 ≤ x6 ≤ 0.3, and the doping concentration is 1E16cm. -3 ~5E16 cm -3 The thickness is 0.1 μm to 0.3 μm; the most preferred value is x6=0.2, and the doping concentration is 3E16cm.-3 The thickness is 0.12 μm.

[0047] The material of the P-type confinement layer 110 is Al. x8 Ga 1-x8 As, where 0.35 ≤ x8 ≤ 1, is a P-type doped material with a doping concentration of 5E17 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 1.5 μm; more preferably, 0.35 ≤ x 8 ≤ 0.5, and the doping concentration is 8E17cm. -3 ~4E18 cm -3 The thickness is 1 μm to 1.5 μm; the most preferred value is x8 = 0.40, with a doping concentration of 1E18cm. -3 The thickness is 1.3 μm.

[0048] The ohmic contact layer 111 is made of GaAs, p-type doped, with a doping concentration of 9E18 cm⁻¹. -3 ~5E19 cm -3 The thickness is 20 nm to 400 nm; more preferably, the doping concentration is 1E19 cm⁻¹. -3 ~5E19 cm -3 The thickness is 100 nm to 300 nm; most preferably, the doping concentration is 4.5E19 cm⁻¹. -3 The thickness is 200 nm.

[0049] The material of the P-type ohmic electrode 112 is Ni / Au, Cr / Au, Pt / Au, or Ni / Al. Preferably, the material of the P-type ohmic electrode 112 is Ni / Au.

[0050] The material of the N-type ohmic electrode 101 is Al / Au, Cr / Au, or Ti / Al / Ti / Au. Preferably, the material of the N-type ohmic electrode 101 is Cr / Au.

[0051] The method for fabricating the semiconductor laser with the aforementioned optical field spreading layer includes the following steps: S1. In the MOCVD reactor, the substrate is heated to 710-750°C in an H2 environment for baking, and then AsH3 is introduced for high-temperature heat treatment to remove foreign matter and water and oxygen from the substrate surface. S2. The temperature is lowered to 700-720℃, and TMAl, TMGa and AsH3 are introduced to grow a buffer layer on the substrate. S3. The temperature is lowered to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow an N-type confinement layer on the buffer layer. S4. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type optical field extension layer on the N-type confinement layer; S5. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type waveguide layer on the N-type optical field extension layer. S6. The temperature is lowered to 540–580°C, and TMAl, TMGa, and AsH3 are introduced to grow Al on the N-type waveguide layer. x5 Ga 1- x5 As a quantum barrier layer, then TMI, TMGa, and AsH3 are introduced into Al. x5 Ga 1-x5 As quantum barrier layer grown In y1 Ga 1-y1 As a quantum well layer, repeat the above process, overlapping Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 As a quantum well layer forms an active layer; S7. The temperature is raised to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow a P-type waveguide layer on the active layer. S8. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type optical field extension layer on the P-type waveguide layer. S9. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type confinement layer on the P-type optical field extension layer. S10, the temperature is lowered to 540-560℃, TMGa and AsH3 are introduced, and an ohmic contact layer is grown on the P-type confinement layer; S11. A P-type ohmic electrode is deposited on the ohmic contact layer to thin the substrate, and an N-type ohmic electrode is deposited below the substrate.

[0052] The present invention will now be described in more detail with reference to specific embodiments.

[0053] Example 1 A semiconductor laser with an optical field spreading layer, such as Figure 1 As shown, along the epitaxial growth direction, the structure sequentially includes a substrate 102, a buffer layer 103, an N-type confinement layer 104, an N-type optical field extension layer 105, an N-type waveguide layer 106, an active layer 107, a P-type waveguide layer 108, a P-type optical field extension layer 109, a P-type confinement layer 110, and an ohmic contact layer 111. A P-type ohmic electrode 112 is disposed above the ohmic contact layer 111, and an N-type ohmic electrode 101 is disposed below the substrate 102.

[0054] The material of the N-type optical field extension layer 105 is Al. x3 Ga 1-x3 As, where x3 linearly varies from 0.2 to 0.3. The N-type optical field extension layer 105 is N-type doped with a doping concentration of 3E16 cm⁻¹. -3 The thickness is 0.33 μm.

[0055] The material of the P-type optical field extension layer 109 is Al. x7 Ga 1-x7 As, where x7 linearly varies from 0.3 to 0.2. The P-type optical field extension layer 109 is P-type doped with a doping concentration of 3E16 cm⁻¹. -3 The thickness is 0.33 μm.

[0056] The substrate 102 is made of GaAs and has a substrate angle of 0°.

[0057] The material of the buffer layer 103 is Al. x1 Ga 1-x1 As, where x1=0, N-type doped, doping concentration is 1E18 cm⁻¹ -3 The thickness is 300nm.

[0058] The material of the N-type confinement layer 104 is Al. x2 Ga 1-x2 As, where x2 = 0.4, N-type doped, with a doping concentration of 1E18cm⁻¹. -3 The thickness is 1.3 μm.

[0059] The material of the N-type waveguide layer 106 is Al. x4 Ga 1-x4 As, where x4 = 0.2, N-type doped, with a doping concentration of 3E16cm. -3 The thickness is 0.12 μm.

[0060] The active layer 107 is composed of Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 The Al is composed of overlapping quantum well layers with an overlap period of 1, where x5 = 0.2 and y1 = 0.14. x5 Ga 1-x5 The As quantum barrier layer is 20 nm thick and undoped. The In... y1 Ga 1-y1 The As quantum well layer is 7 nm thick and undoped. The Al... x5 Ga 1-x5 As the band gap of the quantum barrier layer is greater than that of In y1 Ga1-y1 As the bandgap of the quantum well layer.

[0061] The material of the P-type waveguide layer 108 is Al. x6 Ga 1-x6 As, where x6 = 0.2, is a P-type doped compound with a doping concentration of 3E16cm⁻¹. -3 The thickness is 0.12 μm.

[0062] The material of the P-type confinement layer 110 is Al. x8 Ga 1-x8 As, where x8 = 0.40, is a P-type doped compound with a doping concentration of 1E18 cm⁻¹. -3 The thickness is 1.3 μm.

[0063] The ohmic contact layer 111 is made of GaAs, p-type doped, with a doping concentration of 4.5E19 cm⁻¹. -3 The thickness is 200nm.

[0064] The material of the P-type ohmic electrode 112 is Ni / Au.

[0065] The material of the N-type ohmic electrode 101 is Cr / Au.

[0066] The method for fabricating the semiconductor laser with the aforementioned optical field spreading layer includes the following steps: S1. In the MOCVD reactor, the substrate is heated to 730°C in an H2 environment for baking, and then AsH3 is introduced for high-temperature heat treatment to remove foreign matter and water and oxygen from the substrate surface. S2. The temperature is lowered to 710℃, and TMAl, TMGa and AsH3 are introduced to grow a buffer layer on the substrate. S3. The temperature is lowered to 660℃, and TMAl, TMGa and AsH3 are introduced to grow an N-type confinement layer on the buffer layer. S4. Maintain the temperature at 660℃, introduce TMAl, TMGa and AsH3, and grow an N-type optical field extension layer on the N-type confinement layer; S5. Maintain the temperature at 660℃, introduce TMAl, TMGa and AsH3, and grow an N-type waveguide layer on the N-type optical field extension layer. S6. The temperature is lowered to 560℃, and TMAl, TMGa, and AsH3 are introduced to grow Al on the N-type waveguide layer. x5 Ga 1-x5 As a quantum barrier layer, then TMI, TMGa, and AsH3 are introduced into Al. x5 Ga 1-x5 As quantum barrier layer grown In y1 Ga 1-y1As a quantum well layer, repeat the above process, overlapping Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 As a quantum well layer forms an active layer; S7. The temperature is raised to 660℃, and TMAl, TMGa and AsH3 are introduced to grow a P-type waveguide layer on the active layer. S8. Maintain the temperature at 660℃, introduce TMAl, TMGa and AsH3, and grow a P-type optical field extension layer on the P-type waveguide layer. S9. Maintain the temperature at 660℃, introduce TMAl, TMGa and AsH3, and grow a P-type confinement layer on the P-type optical field extension layer. S10, the temperature is lowered to 550℃, TMGa and AsH3 are introduced to grow an ohmic contact layer on the P-type confinement layer; S11. A P-type ohmic electrode is deposited on the ohmic contact layer to thin the substrate, and an N-type ohmic electrode is deposited below the substrate.

[0067] Example 2 A semiconductor laser with an optical field spreading layer, as described in Example 1, except that: In the N-type optical field extension layer 105, x3 linearly varies from 0.1 to 0.3, and it is N-type doped with a doping concentration of 2E16cm⁻¹. -3 The thickness is 0.4 μm.

[0068] In the P-type optical field extension layer 109, x7 linearly decreases from 0.35 to 0.15, and it is P-type doped with a doping concentration of 2E16cm⁻¹. -3 The thickness is 0.4 μm.

[0069] The other steps and conditions are the same as in Example 1.

[0070] Comparative example: Semiconductor laser without a field spreading layer A semiconductor laser without an optical field extension layer comprises, from top to bottom, a substrate 102, a buffer layer 103, an N-type confinement layer 104, an N-type waveguide layer 106, an active layer 107, a P-type waveguide layer 108, a P-type confinement layer 110, and an ohmic contact layer 111. A P-type ohmic electrode 112 is disposed above the ohmic contact layer 111, and an N-type ohmic electrode 101 is disposed below the substrate 102.

[0071] The other steps and conditions are the same as in Example 1.

[0072] Test case The refractive index of the semiconductor lasers in Example 1 and the comparative example was measured and modeled; the results are as follows: Figure 2 , Figure 3 As shown, Figure 2 The diagram shows the refractive index and optical field distribution of a semiconductor laser as a comparison. Figure 3 The diagram shows the refractive index and optical field distribution of the semiconductor laser in Example 1. Figure 2 and Figure 3 It can be concluded that, compared with the comparative example, the internal optical field of the semiconductor laser in Embodiment 1 of this application is affected by the N-type optical field extension layer and the P-type optical field extension layer, which extends further into the optical field extension layer, changes the distribution state of the optical field, increases the distribution range of the optical field, and helps to reduce the fast axis far-field divergence angle of the semiconductor laser.

[0073] The fast-axis far-field divergence angles of the semiconductor lasers in Example 1 and the comparative example were measured respectively, and the comparison figures are shown in the figure below. Figure 4 As shown, from Figure 4 As can be seen, compared with the comparative example, the fast-axis far-field divergence angle of the semiconductor laser in Example 1 is smaller, indicating that the optical field extension layer of the present invention can effectively reduce the fast-axis far-field divergence angle of the semiconductor laser.

[0074] Other embodiments obtained by those skilled in the art based on the embodiments provided in this application by combining, splitting, or reorganizing the embodiments of this application do not exceed the protection scope of this application.

[0075] The above detailed embodiments have provided a detailed explanation of the purpose, technical solutions, and beneficial effects of the embodiments of this application. The above are merely specific embodiments of the embodiments of this application and are not intended to limit the protection scope of the embodiments of this application. That is, any modifications, equivalent substitutions, improvements, etc., made on the basis of the embodiments of this application should be included within the protection scope of the embodiments of this application.

Claims

1. A semiconductor laser with an optical field spreading layer, comprising, sequentially along the epitaxial growth direction, a substrate, a buffer layer, an N-type confinement layer, an N-type waveguide layer, an active layer, a P-type waveguide layer, a P-type confinement layer, and an ohmic contact layer, wherein a P-type ohmic electrode is disposed above the ohmic contact layer and an N-type ohmic electrode is disposed below the substrate, characterized in that: An N-type optical field extension layer is inserted between the N-type confinement layer and the N-type waveguide layer. The N-type optical field extension layer is composed of Al. x3 Ga 1-x3 As material is formed, where x3 changes linearly between 0 and 0.35, from low to high values; A P-type optical field spreading layer is inserted between the P-type waveguide layer and the P-type confinement layer. The P-type optical field spreading layer is composed of Al. x7 Ga 1- x7 As material is formed, where x7 changes linearly between 0 and 0.35, from high to low values.

2. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, In the N-type optical field extension layer, x3 gradually changes from 0.2 to 0.

3.

3. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, The N-type optical field extension layer is N-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18 cm -3 Further preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm -3 .

4. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, The thickness of the N-type optical field extension layer is 0.1 μm to 0.5 μm; more preferably, the thickness is 0.2 μm to 0.4 μm.

5. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, In the P-type optical field extension layer, x7 gradually changes from 0.3 to 0.

2.

6. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, The P-type optical field extension layer is P-type doped with a doping concentration of 1E16 cm⁻¹. -3 ~5E18 cm -3 Further preferably, the doping concentration is 1E16 cm⁻¹. -3 ~1E17 cm -3 .

7. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, The thickness of the P-type optical field extension layer is 0.1 μm to 0.5 μm; more preferably, the thickness is 0.33 μm.

8. The semiconductor laser with an optical field spreading layer according to claim 1, characterized in that, Includes one or more of the following conditions: a. The substrate is formed of GaAs material; b. The buffer layer is made of Al x1 Ga 1-x1 As material is formed, wherein 0 ≤ x1 ≤ 0.05, N-type doped, and the doping concentration is 1E18cm. -3 ~5E18 cm -3 The thickness is 100 nm to 300 nm; more preferably, 0 ≤ x1 ≤ 0.03, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 200 nm to 300 nm; c. The N-type confinement layer is made of Al x2 Ga 1-x2 As material is formed, wherein 0.35 ≤ x² ≤ 1, N-type doped, and the doping concentration is 5E¹⁷ cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 2 μm; more preferably, 0.35 ≤ x2 ≤ 0.5, and the doping concentration is 8E17cm. -3 ~3E18 cm -3 The thickness is 1 μm to 1.5 μm; d. The N-type waveguide layer is made of Al x4 Ga 1-x4 As material is formed, wherein 0 ≤ x ≤ 0.4, N-type doped, and the doping concentration is 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0 ≤ x 4 ≤ 0.3, and the doping concentration is 1E16 cm⁻¹. -3 ~8E16 cm -3 The thickness is 0.1 μm to 0.3 μm; e. The active layer is composed of Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 The Al is composed of overlapping quantum well layers with an overlap period of 1 to 5, wherein 0 ≤ x5 ≤ 0.4, 0 ≤ y1 ≤ 0.5, and the Al x5 Ga 1-x5 As the band gap of the quantum barrier layer is greater than In y1 Ga 1- y1 As is the bandgap width of the quantum well layer; more preferably, the overlap period is 1~3, 0.1≤x5≤0.3, 0.1≤y1≤0.2; f. The P-type waveguide layer is made of Al x6 Ga 1-x6 As material is formed, wherein 0 ≤ x6 ≤ 0.4, p-type doped, and the doping concentration is 1E16 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.1 μm to 0.5 μm; more preferably, 0.1 ≤ x6 ≤ 0.3, and the doping concentration is 1E16 cm⁻¹. -3 ~5E16 cm -3 The thickness is 0.1 μm to 0.3 μm; g. The P-type confinement layer is made of Al x8 Ga 1-x8 As material is formed, wherein 0.35 ≤ x 8 ≤ 1, p-type doped, and the doping concentration is 5E17 cm⁻¹. -3 ~5E18 cm -3 The thickness is 0.5 μm to 1.5 μm; more preferably, 0.35 ≤ x 8 ≤ 0.5, and the doping concentration is 8E17 cm⁻¹. -3 ~4E18 cm -3 The thickness is 1 μm to 1.5 μm; h. The ohmic contact layer is formed of GaAs material, p-type doped, with a doping concentration of 9E18 cm⁻¹. -3 ~5E19 cm -3 The thickness is 20 nm to 400 nm; more preferably, the doping concentration is 1E19 cm⁻¹. -3 ~5E19 cm -3 The thickness is 100 nm to 300 nm; i. The P-type ohmic electrode is formed of Ni / Au, Cr / Au, Pt / Au or Ni / Al material; more preferably, the material of the P-type ohmic electrode is Ni / Au; j. The N-type ohmic electrode is formed of Al / Au, Cr / Au or Ti / Al / Ti / Au material; more preferably, the N-type ohmic electrode is formed of Cr / Au material.

9. The semiconductor laser with an optical field spreading layer according to claim 8, characterized in that, The Al x5 Ga 1- x5 The thickness of the As quantum barrier layer is 1nm~50nm, and it can be undoped, p-type doped, or n-type doped. y1 Ga 1-y1 The thickness of the As quantum well layer is 1 nm to 10 nm, and it is undoped; more preferably, the Al... x5 Ga 1-x5 The thickness of the As quantum barrier layer is 10nm~30nm, and it is undoped. y1 Ga 1-y1 The thickness of the As quantum well layer is 4nm~10nm.

10. A method for fabricating a semiconductor laser with an optical field spreading layer as described in any one of claims 1-9, characterized in that, Includes the following steps: S1. In the MOCVD reactor, the substrate is heated to 710-750°C in an H2 environment for baking, and then AsH3 is introduced for high-temperature heat treatment to remove foreign matter and water and oxygen from the substrate surface. S2. The temperature is lowered to 700-720℃, and TMAl, TMGa and AsH3 are introduced to grow a buffer layer on the substrate. S3. The temperature is lowered to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow an N-type confinement layer on the buffer layer. S4. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type optical field extension layer on the N-type confinement layer; S5. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow an N-type waveguide layer on the N-type optical field extension layer. S6. The temperature is lowered to 540–580°C, and TMAl, TMGa, and AsH3 are introduced to grow Al on the N-type waveguide layer. x5 Ga 1-x5 As a quantum barrier layer, then TMI, TMGa, and AsH3 are introduced into Al. x5 Ga 1-x5 As quantum barrier layer grown In y1 Ga 1-y1 As a quantum well layer, repeat the above process, overlapping Al x5 Ga 1-x5 As quantum barrier layer and In y1 Ga 1-y1 As a quantum well layer forms an active layer; S7. The temperature is raised to 640-680℃, and TMAl, TMGa and AsH3 are introduced to grow a P-type waveguide layer on the active layer. S8. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type optical field extension layer on the P-type waveguide layer. S9. Maintain the temperature at 640-680℃, introduce TMAl, TMGa and AsH3, and grow a P-type confinement layer on the P-type optical field extension layer. S10, the temperature is lowered to 540-560℃, TMGa and AsH3 are introduced, and an ohmic contact layer is grown on the P-type confinement layer; S11. A P-type ohmic electrode is deposited on the ohmic contact layer to thin the substrate, and an N-type ohmic electrode is deposited below the substrate.