Catalyst for preparing 2, 5-furandicarboxylic acid and preparation method of 2, 5-furandicarboxylic acid

By mixing humic substances with non-precious metal salts to form a dot-network structure catalyst, and then subjecting it to carbonization and surface oxidation treatment, the problem of high cost of precious metal catalysts was solved, and efficient and low-cost preparation of 2,5-furandicarboxylic acid was achieved.

CN122057511APending Publication Date: 2026-05-19CHINESE TEXTILE ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411644582.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-18
Publication Date
2026-05-19

AI Technical Summary

Technical Problem

Existing precious metal catalysts are expensive and scarce, while non-precious metal catalysts are prone to agglomeration and have insufficient catalytic activity in the preparation of 2,5-furandicarboxylic acid, which affects their industrial application.

Method used

The humic substances produced during the preparation of 5-hydroxymethylfurfural are mixed with non-precious metal salts to form a dot-network structure catalyst. After carbonization and surface oxidation treatment, metal ions are fixed to form a catalyst with high specific surface area and abundant active sites.

Benefits of technology

This achieved high efficiency, stability, and activity of the catalyst, reduced production costs, increased the yield and production efficiency of 2,5-furandicarboxylic acid, and realized the high-value utilization of humic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005139363220000071
    Figure BDA0005139363220000071
  • Figure BDA0005139363220000131
    Figure BDA0005139363220000131
  • Figure BDA0005139363220000141
    Figure BDA0005139363220000141
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing 2, 5-furandicarboxylic acid and a preparation method of the 2, 5-furandicarboxylic acid, and the preparation method of the catalyst comprises the following steps: (1) mixing humus generated in the preparation process of 5-hydroxymethylfurfural with non-noble metal salt to form a dot net structure adsorbed with non-noble metal ions; and (2) carrying out carbonization and surface oxidation treatment to obtain the catalyst for preparing 2, 5-furandicarboxylic acid. According to the preparation method, the humus and the non-noble metal salt are mixed, so that metal ions are uniformly adsorbed on the surface of the humus to form a point net structure with high specific surface area and rich active sites, and then carbonization and surface oxidation treatment are performed to fix the metal ions and enhance the stability and activity of the catalyst; the preparation method has the advantages that the problems of high price and scarce resources of the traditional noble metal catalyst are solved, the high-value utilization of the humus is realized, the preparation cost of the catalyst is reduced, and meanwhile, the yield and the production efficiency of the 2, 5-furandicarboxylic acid (FDCA) are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical production technology, specifically, it relates to a catalyst for preparing 2,5-furandicarboxylic acid and a method for preparing 2,5-furandicarboxylic acid. Background Technology

[0002] 2,5-Furfurandicarboxylic acid (FDCA) is an important platform compound that can be used as a rigid monomer in the production of various polymer materials such as polyesters and polyamides, and has the potential to replace terephthalic acid (TPA) in the preparation of polyester materials. FDCA is typically produced by dehydrating biomass feedstock to prepare 5-hydroxymethylfurfural (HMF), followed by purification of HMF and subsequent oxidation under a catalyst.

[0003] However, 5-hydroxymethylfurfural (HMF) exhibits high reactivity and poor thermal stability. During preparation and reaction, it readily undergoes side reactions such as condensation, rehydration, rearrangement, and decomposition with raw materials, products, and itself, generating small-molecule acids like formic acid and levulinic acid, as well as large-molecule humic substances like humin. Humin has high viscosity, contains a large amount of organic solvent, and is difficult to handle, but its high carbon content and abundant metal ions make it an excellent raw material for preparing activated carbon and catalyst supports.

[0004] In the oxidation of 5-hydroxymethylfurfural (HMF) to 2,5-furandicarboxylic acid (FDCA), the selection of catalyst and oxidant is crucial. Commonly used catalysts include noble metal catalysts such as Pt / C, Pd / C, and Au / C. Ait Rass et al. (2013) studied the catalytic activity of Pt-Bi / C catalyst for HMF oxidation, achieving an FDCA yield as high as 99%, and found that the addition of bismuth could accelerate the reaction and prevent catalyst deactivation. Miao et al. (2015) prepared Pt / Ce nanoparticles supported on a cerium-bismuth support. 0.8 Bi 0.2 O 2-δ The catalyst achieved an FDCA yield of 98% within 30 minutes at room temperature, and the FDCA selectivity did not significantly decrease after five reuses. Casanova et al. (2009) prepared various gold-supported catalysts for HMF oxidation, and the results showed that the catalytic activity was optimal when the supports were TiO2 and CeO2, with an FDCA yield as high as 99%.

[0005] However, precious metal catalysts are expensive, significantly increasing the production cost of 2,5-furandicarboxylic acid (FDCA). Therefore, researchers have focused on developing non-precious metal catalysts for the oxidation of 5-hydroxymethylfurfural (HMF). Existing non-precious metal catalysts, such as MnOx–CeO2, MnO2, and CoOx-MC, have achieved HMF oxidation to some extent, but they suffer from problems such as easy aggregation and low catalytic activity, limiting their application in industrial production.

[0006] In view of this, the present invention is hereby proposed. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a catalyst for 2,5-furandicarboxylic acid. Through the rational treatment and utilization of humic substances, not only is the high-value utilization of waste achieved and the production cost reduced, but the performance and catalytic efficiency of the catalyst are also improved.

[0008] To solve the above-mentioned technical problems, the basic concept of the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a catalyst for the preparation of 2,5-furandicarboxylic acid, comprising:

[0010] (1) The humic substances generated during the preparation of 5-hydroxymethylfurfural are mixed with non-precious metal salts to form a dot network structure adsorbed with non-precious metal ions.

[0011] (2) The catalyst for preparing 2,5-furandicarboxylic acid was then obtained through carbonization and surface oxidation treatment.

[0012] During the preparation of 5-hydroxymethylfurfural (HMF), a large number of byproducts—humic substances (also known as humic acid)—are often generated. These humic substances are high-molecular-weight organic compounds formed by complex reactions between raw materials (such as cellulose, glucose, fructose, etc.), HMF itself, products, and byproducts. They have complex structures, contain a large number of aromatic rings, carboxyl groups, hydroxyl groups, and other functional groups, and have rich chemical reactivity.

[0013] Using humic substances (such as humin macromolecular humic substances) generated during the production of 5-hydroxymethylfurfural (HMF) as raw materials enables the high-value utilization of waste, reduces the pressure of waste treatment during the production process, and significantly reduces the preparation cost of catalysts.

[0014] Humic substances possess a complex macromolecular network structure with various functional groups between molecules, enabling coordination or adsorption with metal ions. This network structure provides numerous active sites for metal ion loading, facilitating the formation of highly dispersed metal active centers. This application mixes humic substances with non-precious metal salts, allowing metal ions to be uniformly adsorbed onto the humic substance surface, forming a dotted network structure with a high specific surface area and abundant active sites. Carbonization and surface oxidation treatments then immobilize the metal ions, enhancing the catalyst's stability and activity.

[0015] The catalyst prepared in this invention is a non-precious metal catalyst, avoiding the problems of high cost and scarce resources of traditional precious metal catalysts. This catalyst exhibits high activity and excellent cycling performance in the reaction using 5-hydroxymethylfurfural (HMF) as a raw material and sodium hypochlorite as an oxidant, thereby improving the yield and production efficiency of 2,5-furandicarboxylic acid (FDCA).

[0016] Furthermore, the weight ratio of the humic substance to the non-precious metal salt is 1:0.1-10, preferably 1:1-1.5.

[0017] Furthermore, the non-precious metal salt is selected from one or more of cobalt, manganese, copper, and nickel salts;

[0018] This method uses transition metals such as cobalt, manganese, copper, and nickel as the active components of the catalyst. These metals are abundant, inexpensive, and possess multiple valence states and complex redox properties, making them suitable for catalyzing oxidation reactions.

[0019] Preferably, the non-precious metal salt includes one or two of cobalt salt, nickel salt, and copper salt;

[0020] Preferably, the non-precious metal salt includes one or both of nickel sulfate hexahydrate and cobalt acetate tetrahydrate;

[0021] Preferably, the non-precious metal salt includes cobalt acetate tetrahydrate and copper salt;

[0022] Preferably, the cobalt salt is 5-30 parts by weight and the copper salt is 15-25 parts by weight;

[0023] Preferably, the cobalt salt is 10-30 parts by weight and the copper salt is 15-20 parts by weight.

[0024] Further, in step (1), the humic substances produced during the preparation of 5-hydroxymethylfurfural are mixed with water and non-precious metal salts to form a uniform mixture, and then subjected to ultrasonic treatment;

[0025] Preferably, the ultrasonic treatment time is 20-90 min, more preferably 20-30 min.

[0026] When ultrasound propagates in a liquid, it generates cavitation, creating a localized high-temperature, high-pressure microenvironment that promotes the dispersion and dissolution of solid particles. Ultrasonic treatment of mixtures of humic substances and non-precious metal salts can uniformly spread the macromolecular network structure of the humic substances, enhancing their capture and adsorption of metal ions and resulting in a uniform distribution of metal ions on the humic substance surface.

[0027] Further, in step (1), after ultrasonic treatment, an alkali agent is added, and the weight ratio of the humic substance to the alkali agent is 1:0.1-10;

[0028] Preferably, the alkaline agent is selected from one or more of metal hydroxides or carbonates;

[0029] Preferably, the alkaline agent is selected from one or more of sodium hydroxide, potassium hydroxide, barium hydroxide, sodium carbonate, and potassium carbonate.

[0030] Upon addition of an alkaline agent, the metal ions react with the alkali to form metal hydroxide or metal carbonate precipitates. These precipitates further interact with the functional groups on the surface of humic substances, forming stable complexes that are fixed within the network structure of the humic substances.

[0031] Furthermore, in step (2), carbonization includes: carbonization in an inert atmosphere by gradient heating;

[0032] Carbonization under an inert atmosphere forms a carbon-based material with a certain porous structure, increasing the specific surface area and providing more active sites for catalytic reactions. Simultaneously, metal hydroxides or carbonates decompose at high temperatures, forming metal oxide nanoparticles that are uniformly dispersed on the surface or within the pores of the carbon-based material. Furthermore, high-temperature carbonization makes the material's structure more stable, improving its resistance to high temperatures and acids / alkalis, and extending the catalyst's lifespan.

[0033] At high temperatures, organic matter and metal ions are easily oxidized in the air, leading to excessive combustion of materials or changes in the oxidation state of metals. Therefore, nitrogen is used as a protective gas to provide an inert atmosphere and prevent oxidation reactions from occurring.

[0034] Preferably, in step (2), carbonization includes: first rapidly heating to 300°C, then slowly heating to 550°C, and then holding at that temperature;

[0035] Increasing the carbonization temperature helps to improve the degree of graphitization in carbon materials, enhances electrical conductivity, and thus facilitates electron transfer and accelerates catalytic reactions.

[0036] Preferably, in step (2), the temperature is first raised to 300°C at a rate of 10°C / minute, and then raised to 550°C at a rate of 5°C / minute, and carbonized at 550°C.

[0037] The temperature is first increased to 300℃ at a rate of 10℃ / min. Residual moisture and low-boiling-point organic matter in the sample are gradually removed to prevent structural damage caused by rapid gas release during rapid heating. At the same time, some organic functional groups (such as carboxyl and hydroxyl groups) begin to undergo pyrolysis, laying the foundation for subsequent carbonization.

[0038] The temperature is then increased to 550℃ at a rate of 5℃ / min. Above 300℃, the pyrolysis reaction of organic matter intensifies, producing a large amount of gas and free radicals. The slower heating rate helps to control the pyrolysis process and prevent the sudden collapse of the material structure. At this stage, the aromatization and condensation reactions are enhanced, and a stable carbon skeleton is gradually formed, which is beneficial to improving the electrical conductivity and mechanical strength of carbon materials.

[0039] Furthermore, the material is kept at 550℃ for 1 hour. During this holding period, the organic matter is completely carbonized and volatile substances are completely eliminated, forming a stable carbonaceous material. At high temperatures, carbon atoms rearrange to form a more ordered graphite microcrystalline structure, improving the physicochemical properties of the carbon material.

[0040] Furthermore, in step (2), a sodium hypochlorite solution with an effective chlorine content of 4-30% is used for surface oxidation treatment;

[0041] Sodium hypochlorite (NaClO) is an oxidizing agent that can generate hypochlorous acid (HOCl) in aqueous solution, exhibiting strong oxidizing power. In surface oxidation treatment, sodium hypochlorite generates active oxides through the following reaction:

[0042] NaClO + H₂O → HOCl + NaOH;

[0043] Hypochlorous acid (HOCl) further decomposes to produce chlorine free radicals (-Cl) and other oxidizing species. These active oxide species can react with carbon-based materials on the catalyst surface to generate oxygen-containing functional groups, such as carboxyl groups (–COOH), hydroxyl groups (–OH), and carbonyl groups (–C=O).

[0044] Specifically, the chemical reactions that introduce oxygen-containing functional groups onto the catalyst surface mainly include:

[0045] Carboxylation reaction: The introduction of carboxyl groups can increase the acidic sites on the catalyst surface and enhance its interaction with reactant molecules;

[0046] C–H+O→C–OH,

[0047] C–OH+O→C=O;

[0048] Hydroxylation reaction: The introduction of hydroxyl groups helps to improve the hydrophilicity and dispersibility of the catalyst, and enhance its contact efficiency with reactants in solution;

[0049] C–H+O→C–OH;

[0050] Carbonylation reaction: The formation of carbonyl groups can provide additional catalytically active sites, promoting the oxidation reaction;

[0051] C–OH+O→C=O;

[0052] Through these chemical reactions, the catalyst surface is effectively functionalized, forming a rich network of oxygen-containing functional groups, which significantly enhances the activity and selectivity of the catalyst.

[0053] "Available chlorine content" refers to the percentage of active chlorine (Cl) species in a chlorine compound solution that provide oxidizing capabilities. Specifically, available chlorine content measures the proportion of free chlorine (such as hypochlorous acid, chloride ions, etc.) in the solution, which has oxidizing and disinfecting capabilities.

[0054] Preferably, a sodium hypochlorite solution with an effective chlorine content of 6-14% is used for surface oxidation treatment;

[0055] Preferably, a sodium hypochlorite solution with an effective chlorine content of 7.5% is used for surface oxidation treatment;

[0056] Sodium hypochlorite solution with an effective chlorine content of 7.5% has moderate oxidizing power and can fully introduce oxygen-containing functional groups without over-oxidizing the catalyst surface.

[0057] Preferably, the mass ratio of the humic substance to the sodium hypochlorite solution is 1:1-20.

[0058] Surface oxidation treatment using sodium hypochlorite solution can further oxidize the surface of carbon-based materials, increasing oxygen-containing functional groups such as carboxyl and hydroxyl groups. These functional groups can improve the hydrophilicity of the catalyst and its adsorption capacity for reactants, thereby enhancing the catalyst's activity.

[0059] Furthermore, in step (2), the carbonized product is first ground and sieved to obtain carbonized powder, and the carbonized powder is slowly added to sodium hypochlorite solution for surface oxidation treatment.

[0060] Controlling the addition rate of sodium hypochlorite solution prevents the oxidation reaction from becoming too vigorous and damaging the catalyst surface structure; slow addition helps to form a uniform layer of oxygen-containing functional groups on the catalyst surface.

[0061] Preferably, carbonized powder with a particle size of 200-400 mesh is obtained by sieving.

[0062] Furthermore, the humic substance is the humic substance produced during the preparation of 5-hydroxymethylfurfural using one or more of cellulose, glucose, fructose, starch, and sucrose as raw materials.

[0063] The raw materials for preparing the catalyst of 2,5-furandicarboxylic acid according to this invention include humic substances generated during the preparation of 5-hydroxymethylfurfural. The humic substances are mainly composed of some high-molecular organic compounds with significant aromatic structures and oxygen-containing functional groups, such as carboxyl groups, phenolic hydroxyl groups, and aldehyde groups. These functional groups enable the humic substances to have certain functions in catalysis, such as complexing metal ions, stabilizing metal catalysts, and promoting reaction activation. Specifically, it includes humic substances generated during the preparation of 5-hydroxymethylfurfural using one or more of cellulose, glucose, fructose, starch, and sucrose as raw materials.

[0064] This invention also provides a method for preparing 2,5-furandicarboxylic acid, comprising the following steps:

[0065] (1) Take sodium hypochlorite solution and disperse the catalyst prepared by any of the preparation methods described in claims 1-9 to obtain a dispersion;

[0066] (2) Add an alkaline agent to the obtained dispersion, and then add 5-hydroxymethylfurfural to react and prepare 2,5-furandicarboxylic acid.

[0067] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art.

[0068] In this invention, by mixing humic substances with non-precious metal salts, metal ions are uniformly adsorbed on the surface of the humic substances, forming a dot network structure with a high specific surface area and abundant active sites. After carbonization and surface oxidation treatment, the metal ions are fixed, enhancing the stability and activity of the catalyst. This avoids the problems of high price and scarce resources of traditional precious metal catalysts, realizes the high-value utilization of humic substances, reduces the preparation cost of the catalyst, and improves the yield and production efficiency of 2,5-furandicarboxylic acid (FDCA). Detailed Implementation

[0069] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments are described clearly and completely below. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0070] Example 1

[0071] (1) Catalyst preparation:

[0072] Add 20 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 ml of water, add 30 grams of nickel sulfate hexahydrate (NiSO4·6H2O), and stir until fully dissolved to obtain a mixture. The humic substances are produced during the preparation of 5-hydroxymethylfurfural (HMF) from fructose, and the carbon-to-oxygen ratio of the humic substances is 63.52:31.51, with a molecular weight of 835 Da.

[0073] The above mixture was subjected to ultrasonic treatment for 30 minutes to enhance the mixing uniformity.

[0074] Add 5 grams of sodium hydroxide (NaOH) to the mixture and continue stirring to allow the reaction to proceed fully.

[0075] After the reaction was completed, the solid material was filtered, collected, and dried in an oven at 105°C for 4 hours to obtain solid A.

[0076] The dried solid was placed in a quartz boat and placed in a tube furnace. Under nitrogen (N2) protection, the temperature was increased to 300°C at a rate of 10°C / min, and then increased to 550°C at a rate of 5°C / min. The temperature was then held at 550°C for 1 hour to obtain solid B.

[0077] (2) Activation treatment of catalyst:

[0078] Solid B is ground and sieved to obtain a uniform powder.

[0079] Slowly add the above powder to 100 ml of sodium hypochlorite solution (available chlorine content 7.5%), mix thoroughly with stirring to promote activation.

[0080] The mixture was filtered, the solids were collected, and the mixture was washed with deionized water until neutral.

[0081] The washed solid was dried in an oven to obtain a catalyst for the preparation of 2,5-furandicarboxylic acid (FDCA).

[0082] (3) Synthesis of 2,5-furandicarboxylic acid (FDCA):

[0083] Take 12.5 ml of sodium hypochlorite solution (available chlorine content 7.5%) and place it in an Erlenmeyer flask.

[0084] Add 0.5 g of the catalyst prepared above and shake well to disperse the catalyst evenly.

[0085] Add 0.4 g of sodium hydroxide (NaOH), mix well, and adjust the alkalinity of the solution.

[0086] Finally, add 0.63 g of 5-hydroxymethylfurfural (HMF) and react at 40°C for 1 hour, stirring constantly to ensure a complete reaction.

[0087] (4) Detection and analysis of products:

[0088] After the reaction is complete, stir the reaction solution evenly, take 3 grams of the reaction solution, add 15 ml of 4 mol / L sodium hydroxide solution to completely dissolve the generated 2,5-furandicarboxylic acid (FDCA).

[0089] Take a small sample and filter it with a 0.22-micron needle filter to remove solid impurities.

[0090] Dilute the filtrate appropriately so that its concentration falls within the range of the standard curve for high performance liquid chromatography (HPLC).

[0091] Analysis was performed using a VYDAC 214TP54 column (C18, 5 μm, 250 × 4.6 mm) connected to a UV detector.

[0092] The mobile phase was a mixture of 0.05 mol / L ammonium acetate solution and methanol at a volume ratio of 50:50, the flow rate was 0.6 mL / min, the detection wavelength was 265 nm, and the column temperature was maintained at 30 °C.

[0093] The yield of 2,5-furandicarboxylic acid (FDCA) was calculated using the following formula:

[0094]

[0095] The catalyst prepared by the above method was used for the oxidation reaction of HMF, and the HMF was successfully converted to FDCA after reacting at 40℃ for 1 hour. High-performance liquid chromatography (HPLC) analysis showed that the yield of FDCA reached the expected level, demonstrating the high efficiency and stability of the catalyst. This method is simple to operate, can effectively reduce production costs, and provides a feasible technical route for the industrial production of FDCA.

[0096] Example 2

[0097] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0098] Add 20 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 ml of water, add 30 grams of Co(AcO)2·4H2O, and stir until fully dissolved to obtain a mixture; the remaining steps are the same as in Example 1.

[0099] Example 3

[0100] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0101] Add 20 g of the humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, add 30 g of CuCl2, and stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance mixing homogeneity. Add 10 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0102] Example 4

[0103] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0104] Add 20 g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 15 g of Co(AcO)₂·4H₂O and 15 g of CuCl₂. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0105] Example 5

[0106] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0107] Add 20 g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 10 g of Co(AcO)₂·4H₂O and 20 g of CuCl₂. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0108] Example 6

[0109] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0110] Add 20 g of the humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 5 g of Co(AcO)₂·4H₂O and 25 g of CuCl₂. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0111] Example 7

[0112] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0113] Add 20 g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 15 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 15 g of CuCl2. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0114] Example 8

[0115] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0116] Add 20 g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 10 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20 g of CuCl2. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0117] Example 9

[0118] The only difference from Example 1 is the method of catalyst preparation. Specifically, in this example:

[0119] Add 20 g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 mL of water, along with 5 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 25 g of CuCl2. Stir until fully dissolved to obtain a mixture. Sonicate the mixture for 30 minutes to enhance homogeneity. Add 7.5 g of sodium hydroxide (NaOH) to the mixture and continue stirring to ensure complete reaction; the remaining steps are the same as in Example 1.

[0120] Example 10

[0121] The only difference from Example 1 is the catalyst preparation method and the catalyst activation treatment method. Specifically, in this example:

[0122] (1) Add 20g of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100ml of water, add 10g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20g of CuCl2, and stir until fully dissolved to obtain a mixture; wherein, the humic substances are humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) using fructose as raw material, the carbon-oxygen ratio of the humic substances is 63.52:31.51, and the molecular weight is 835Da.

[0123] The above mixture was ultrasonically treated for 30 minutes to enhance mixing homogeneity. 7.5 g of sodium hydroxide (NaOH) was added to the mixture, and stirring was continued to ensure a complete reaction. After the reaction was complete, the mixture was filtered, and the solid was collected and dried in an oven at 105°C for 4 hours to obtain solid A. The dried solid was placed in a quartz boat and then placed in a tube furnace. Under nitrogen (N2) protection, the temperature was increased to 300°C at a rate of 10°C / min, and then further increased to 550°C at a rate of 5°C / min, and held at 550°C for 1 hour to obtain solid B.

[0124] (2) Activation treatment of the catalyst: Solid B was ground and sieved to obtain a uniform powder. The powder was slowly added to 200 mL of sodium hypochlorite solution (available chlorine content 7.5%) and mixed thoroughly with stirring to promote activation. The mixture was filtered, the solid was collected, and washed with deionized water until neutral. The washed solid was dried in an oven to obtain the catalyst for the preparation of 2,5-furandicarboxylic acid (FDCA).

[0125] The remaining steps are the same as in Example 1.

[0126] Example 11

[0127] The only difference between this embodiment and Example 10 is the activation method of the catalyst. Specifically, in this embodiment:

[0128] Catalyst activation: Solid B was ground and sieved to obtain a uniform powder. The powder was slowly added to 100 mL of sodium hypochlorite solution (available chlorine content 7.5%), and thoroughly mixed with stirring to promote activation. The mixture was filtered, the solid was collected, and washed with deionized water until neutral. The washed solid was dried in an oven to obtain the catalyst for the preparation of 2,5-furandicarboxylic acid (FDCA).

[0129] The remaining steps are the same as in Example 10.

[0130] Example 12

[0131] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment, the mixture is ultrasonically treated for 90 minutes, while in Example 11 it is ultrasonically treated for 30 minutes.

[0132] The remaining steps are the same as in Example 11.

[0133] Example 13

[0134] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment: 5 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) are added to 100 ml of water, along with 10 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20 g of CuCl2. The mixture is stirred until fully dissolved to obtain a mixed solution.

[0135] The remaining steps are the same as in Example 11.

[0136] Example 14

[0137] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment: 30 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) are added to 100 ml of water, along with 10 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20 g of CuCl2. The mixture is stirred until fully dissolved to obtain a mixed solution.

[0138] The remaining steps are the same as in Example 11.

[0139] Example 15

[0140] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment: 50 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) are added to 100 ml of water, along with 10 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20 g of CuCl2. The mixture is stirred until fully dissolved to obtain a mixed solution.

[0141] The remaining steps are the same as in Example 11.

[0142] Example 16

[0143] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment: 300 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) are added to 100 ml of water, along with 10 g of nickel sulfate hexahydrate (NiSO4·6H2O) and 20 g of CuCl2. The mixture is stirred until fully dissolved to obtain a mixed solution.

[0144] The remaining steps are the same as in Example 11.

[0145] Example 17

[0146] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment, the mixture is ultrasonically treated for 20 minutes, while in Example 11, it is ultrasonically treated for 30 minutes.

[0147] The remaining steps are the same as in Example 11.

[0148] Example 18

[0149] The only difference between this embodiment and Example 11 is the preparation method of the catalyst. Specifically, in this embodiment, the mixture is ultrasonically treated for 0 minutes, while in Example 11, it is ultrasonically treated for 30 minutes.

[0150] The remaining steps are the same as in Example 11.

[0151] Example 19

[0152] The only difference between this embodiment and Example 11 is that the available chlorine content of sodium hypochlorite is 10%, while the available chlorine content of sodium hypochlorite in Example 11 is 7.5%.

[0153] The remaining steps are the same as in Example 11.

[0154] Example 20

[0155] The only difference between this embodiment and Example 11 is that the available chlorine content of sodium hypochlorite is 6%, while the available chlorine content of sodium hypochlorite in Example 11 is 7.5%.

[0156] The remaining steps are the same as in Example 11.

[0157] Example 21

[0158] The only difference between this embodiment and Example 11 is that the available chlorine content of sodium hypochlorite is 4%, while the available chlorine content of sodium hypochlorite in Example 11 is 7.5%.

[0159] The remaining steps are the same as in Example 11.

[0160] Example 22

[0161] (1) Catalyst preparation:

[0162] Add 3 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 ml of water, add 30 grams of nickel sulfate hexahydrate (NiSO4·6H2O), and stir until fully dissolved to obtain a mixture. The humic substances are produced during the preparation of 5-hydroxymethylfurfural (HMF) from glucose and cellulose, and have a carbon-to-oxygen ratio of 61.37:33.25 and a molecular weight of 1030 Da.

[0163] The above mixture was subjected to ultrasonic treatment for 25 minutes to enhance the mixing uniformity.

[0164] Add 30 grams of sodium carbonate to the mixture and continue stirring to allow the reaction to proceed fully.

[0165] After the reaction was completed, the solid material was filtered, collected, and dried in an oven at 105°C for 4 hours to obtain solid A.

[0166] The dried solid was placed in a quartz boat and placed in a tube furnace. Under nitrogen (N2) protection, the temperature was increased to 350°C at a rate of 15°C / min, and then increased to 600°C at a rate of 7°C / min. The temperature was then held at 600°C for 1 hour to obtain solid B.

[0167] (2) Activation treatment of catalyst:

[0168] Solid B is ground and sieved to obtain a uniform powder with a particle size of 200-400 mesh.

[0169] Slowly add the above powder to 60 ml of sodium hypochlorite solution (available chlorine content 14%), mix thoroughly with stirring to promote activation.

[0170] The mixture was filtered, the solids were collected, and the mixture was washed with deionized water until neutral.

[0171] The washed solid was dried in an oven to obtain a catalyst for the preparation of 2,5-furandicarboxylic acid (FDCA).

[0172] (3) Synthesis of 2,5-furandicarboxylic acid (FDCA):

[0173] Take 12.5 ml of sodium hypochlorite solution (available chlorine content 14%) and place it in an Erlenmeyer flask.

[0174] Add 0.5 g of the catalyst prepared above and shake well to disperse the catalyst evenly.

[0175] Add 0.4 g of sodium hydroxide (NaOH), mix well, and adjust the alkalinity of the solution.

[0176] Finally, 0.63 g of 5-hydroxymethylfurfural (HMF) was added, and the mixture was reacted at 40 °C for 1 hour with stirring to ensure complete reaction, thus yielding 2,5-furandicarboxylic acid (FDCA).

[0177] Example 23

[0178] (1) Catalyst preparation:

[0179] Add 25 grams of humic substances produced during the preparation of 5-hydroxymethylfurfural (HMF) to 100 ml of water, add 30 grams of nickel sulfate hexahydrate (NiSO4·6H2O), and stir until fully dissolved to obtain a mixture. The humic substances are produced during the preparation of 5-hydroxymethylfurfural (HMF) from sucrose and starch, and have a carbon-to-oxygen ratio of 59.89:32.57 and a molecular weight of 916 Da.

[0180] The above mixture was subjected to ultrasonic treatment for 25 minutes to enhance the mixing uniformity.

[0181] Add 2.5 grams of potassium carbonate to the mixture and continue stirring to allow the reaction to proceed fully.

[0182] After the reaction was completed, the solid material was filtered, collected, and dried in an oven at 105°C for 4 hours to obtain solid A.

[0183] The dried solid was placed in a quartz boat and placed in a tube furnace. Under nitrogen (N2) protection, the temperature was increased to 300°C at a rate of 10°C / min, and then increased to 500°C at a rate of 6°C / min. The temperature was then held at 500°C for 1 hour to obtain solid B.

[0184] (2) Activation treatment of catalyst:

[0185] Solid B is ground and sieved to obtain a uniform powder with a particle size of 200-400 mesh.

[0186] Slowly add the above powder to 25 ml of sodium hypochlorite solution (available chlorine content 30%), mix thoroughly with stirring to promote activation.

[0187] The mixture was filtered, the solids were collected, and the mixture was washed with deionized water until neutral.

[0188] The washed solid was dried in an oven to obtain a catalyst for the preparation of 2,5-furandicarboxylic acid (FDCA).

[0189] (3) Synthesis of 2,5-furandicarboxylic acid (FDCA):

[0190] Take 12.5 ml of sodium hypochlorite solution (available chlorine content 30%) and place it in an Erlenmeyer flask.

[0191] Add 0.5 g of the catalyst prepared above and shake well to disperse the catalyst evenly.

[0192] Add 0.4 g of sodium hydroxide (NaOH), mix well, and adjust the alkalinity of the solution.

[0193] Finally, 0.63 g of 5-hydroxymethylfurfural (HMF) was added, and the mixture was reacted at 40 °C for 1 hour with stirring to ensure complete reaction, thus yielding 2,5-furandicarboxylic acid (FDCA).

[0194] Example 24

[0195] The only difference from Example 1 is that the humic material was replaced with humic material generated during the preparation of 5-hydroxymethylfurfural (HMF) from glucose and cellulose. The carbon-to-oxygen ratio of the humic material was 61.37:33.25, and the molecular weight was 1030 Da. The FDCA yield was 94.8%.

[0196] Example 25

[0197] The only difference from Example 1 is that the humic material was replaced with humic material generated during the preparation of 5-hydroxymethylfurfural (HMF) from sucrose and starch. The carbon-to-oxygen ratio of the humic material was 59.89:32.57, and the molecular weight was 916 Da. The FDCA yield was 94.0%.

[0198] Comparative Example 1

[0199] The only difference between this comparative example and Example 11 is that, in this comparative example, no humic substances generated during the preparation of the catalyst from 5-hydroxymethylfurfural (HMF) are added.

[0200] The yields of 2,5-furandicarboxylic acid (FDCA) in Examples 1 to 21 and Comparative Example 1 are shown in Table 1 below:

[0201] Table 1:

[0202]

[0203]

[0204] Comparing Comparative Example 1 with Example 11, the only difference being the absence of humic substances in Comparative Example 1, the FDCA yield was 85.6%, significantly lower than the 93.9% yield in Example 11. Firstly, the lack of humic substances led to uneven dispersion of metal ions on the catalyst surface. The macromolecular network structure and abundant oxygen-containing functional groups in humic substances can effectively capture and uniformly disperse metal ions, forming a dot network structure with high specific surface area and multiple active sites. Without humic substances, metal ions easily aggregate, forming large metal clusters, reducing the number and dispersion of active sites, thereby decreasing the overall activity and selectivity of the catalyst.

[0205] Secondly, the role of humic substances in catalyst supports is not limited to the dispersion of metal ions, but also includes enhancing the structural stability and durability of the catalyst. In Comparative Example 1, without the addition of humic substances, the mechanical strength and high-temperature resistance of the catalyst may be poor, leading to easy deactivation or breakage of the catalyst during the reaction, further affecting the yield and stability of FDCA.

[0206] Furthermore, catalysts lacking humic substances exhibit weaker hydrophilicity and dispersibility. The oxygen-containing functional groups (such as carboxyl and hydroxyl groups) introduced by humic substances enhance the hydrophilicity of the catalyst, resulting in more uniform dispersion in the aqueous reaction system and increasing the contact opportunities between the catalyst and HMF and the oxidant. Without humic substances, the catalyst may aggregate in the reaction system, leading to reduced catalytic efficiency, incomplete reaction, and thus limited FDCA yield.

[0207] In contrast, the addition of 20g of humic material in Example 11 significantly increased the FDCA yield to 93.9%. Humic material, through its complex polymer network structure and abundant oxygen-containing functional groups, can effectively capture and uniformly disperse Ni. 2 Transition metal ions such as Cu2+ and Cu2+ form highly dispersed metal oxide nanoparticles. This uniformly dispersed dot network structure greatly increases the specific surface area and the number of active sites of the catalyst, improving the overall activity and catalytic efficiency of the catalyst, thereby significantly increasing the yield of FDCA.

[0208] The presence of humic substances enhances the structural stability and durability of the catalyst. During high-temperature carbonization and surface oxidation treatments, the cross-linked bonds and aromatic ring structures in the humic substances provide a robust framework, preventing the migration and aggregation of metal oxide particles and maintaining the catalyst's high specific surface area and the stability of its active sites. This structural advantage ensures the catalyst's high efficiency and long lifespan during repeated use, reducing catalyst deactivation rate and replacement frequency.

[0209] The oxygen-containing functional groups introduced by humic substances significantly enhance the hydrophilicity and dispersibility of the catalyst. In the aqueous reaction system, the catalyst can be uniformly dispersed, increasing the contact opportunities between the catalyst and HMF and the oxidant, thus promoting the efficient oxidation reaction. The uniformly dispersed catalyst reduces the problem of local high concentrations in the reaction, avoiding local over-oxidation or incomplete reaction, and improving the yield and product quality of FDCA.

[0210] Humic substances, as carriers for non-precious metal catalysts, significantly reduce the cost of catalyst preparation. Compared with traditional precious metal catalysts, non-precious metals such as Ni and Cu are abundant and inexpensive. The effective utilization of humic substances not only achieves high-value utilization of waste but also improves the economics and sustainability of catalysts.

[0211] Comparing Examples 1, 2, and 3, in Example 1, 20 g of humic material reacted with 30 g of NiSO4·6H2O, followed by surface oxidation treatment in a sodium hypochlorite solution with 7.5% available chlorine content and ultrasonic treatment for 30 minutes, ultimately achieving a FDCA yield of 95.2%. This result demonstrates that nickel, as the active catalyst component, exhibits high catalytic activity and effectiveness on the humic material support, efficiently promoting the oxidation reaction of HMF and generating high yields of FDCA.

[0212] In contrast, in Example 2, 20 g of humic material reacted with 30 g of Co(AcO)₂·4H₂O, followed by surface oxidation treatment in a sodium hypochlorite solution with 7.5% available chlorine content and ultrasonication for 30 minutes, further increasing the FDCA yield to 97.4%. This data indicates that cobalt, as another transition metal, exhibits slightly better catalytic performance than nickel on the humic material support. Cobalt ions may provide more active sites or higher catalytic activity during the catalytic process, thereby improving the efficiency of HMF to FDCA conversion.

[0213] However, in Example 3, 20 g of humic material was reacted with 30 g of CuCl2 and subjected to surface oxidation treatment under the same conditions, but the final yield of FDCA was only 20.8%, far lower than that in Examples 1 and 2. This significant difference indicates that copper, as a catalyst active component, performs poorly in this method and cannot effectively promote the conversion of HMF to FDCA when used alone.

[0214] It is evident that the key role of humic substances in catalyst preparation lies in their ability to uniformly disperse and fix highly active metal ions, thereby enhancing the overall activity and efficiency of the catalyst. At the same time, selecting appropriate active metal components is crucial for achieving efficient HMF oxidation reactions. Among them, nickel and cobalt are more ideal choices in this method due to their superior catalytic performance.

[0215] Comparing Examples 2, 4 to 6, in Example 2, 20 g of humic material and 30 g of Co(AcO)2·4H2O were added, while NiSO4·6H2O and CuCl2 were not added, and the yield of FDCA reached 97.4%. This result indicates that cobalt, as the active component of the catalyst, exhibits excellent catalytic activity on the humic material support and can efficiently promote the conversion of HMF to FDCA.

[0216] However, in Example 4, 15 g of CuCl2 was added, and the FDCA yield was 92.5%; in Example 5, 20 g of CuCl2 was added, and the FDCA yield increased to 93.0%; while in Example 6, when the amount of CuCl2 was further increased to 25 g, the FDCA yield decreased significantly to 83.7%.

[0217] First, copper, as a transition metal, is relatively cheaper than nickel and cobalt. Therefore, introducing copper into the catalyst preparation helps to reduce the overall cost of the catalyst, thereby reducing the amount of expensive metals used while maintaining a high FDCA yield, thus achieving a balance between economy and catalytic efficiency.

[0218] In Examples 4 and 5, appropriate amounts of copper doping (15 g and 20 g, respectively) did not significantly reduce the yield of FDCA, which was 92.5% and 93.0%, respectively. This indicates that within a certain range, the introduction of copper can effectively supplement nickel and cobalt, maintaining the high efficiency of the catalyst. Furthermore, as the amount of copper added increases, the FDCA yield first increases and then decreases, indicating that the addition of copper is beneficial to improving catalytic activity. The addition of copper is conducive to the formation of oxygen vacancies in the catalyst, and oxygen vacancies are an important medium for the catalyst to play a catalytic role. Therefore, increasing the amount of copper added is beneficial to improving the catalytic activity of the catalyst.

[0219] However, excessive copper doping (such as 25 g of CuCl2 in Example 6) led to a significant decrease in the FDCA yield to 83.7%. This phenomenon stems from the following problems caused by the excessive presence of copper in the catalyst. First, excess copper forms inactive metal complexes or metal oxides with cobalt, reducing the effective active sites of cobalt and lowering the overall activity of the catalyst. Second, excess copper occupies the active sites on the humic support, hindering the uniform dispersion of cobalt and nickel, resulting in a reduction of active sites on the catalyst surface.

[0220] Similarly, comparing Examples 1 and 7 through 9, in Example 1, 20 g of humic material and 30 g of NiSO4·6H2O were added, while Co(AcO)2·4H2O and CuCl2 were not added, and the yield of FDCA reached 95.2%. This result indicates that nickel, as the active component of the catalyst, exhibits excellent catalytic activity on the humic material support and can efficiently promote the conversion of HMF to FDCA.

[0221] Furthermore, as shown in Examples 7, 8, and 9, the FDCA yield initially increased and then decreased with increasing copper content, indicating that the addition of copper is beneficial for improving catalytic activity. The addition of copper promotes the formation of oxygen vacancies in the catalyst, which are crucial mediators for catalytic action. Therefore, increasing the amount of copper added is beneficial for improving the catalyst's catalytic activity. However, excessive copper addition reduces the percentage of nickel, significantly decreasing catalytic activity.

[0222] Comparing Examples 8 and 10, in Example 8, the amount of sodium hypochlorite added was 100 ml, and the FDCA yield was 93.2%; in Example 10, the amount of sodium hypochlorite added was increased to 200 ml, and the FDCA yield increased to 94.7%. It is evident that increasing the amount of oxidant within an appropriate range can effectively improve the catalytic performance of the catalyst and the yield of FDCA.

[0223] Comparing the data from Examples 8, 13, 14, 15, and 16, it is evident that the amount of humic material added has a significant impact on catalyst performance and FDCA yield. When the amount of humic material added is moderate, the catalyst can effectively capture and disperse metal ions, forming a highly efficient network of active sites, significantly improving the FDCA yield. However, both excessively low and excessively high amounts of humic material added will lead to a decrease in catalyst performance. Too little humic material cannot sufficiently capture and disperse metal ions, resulting in an uneven number and distribution of active sites on the catalyst surface, reducing the overall activity and efficiency of the catalyst; furthermore, low amounts of humic material cannot effectively fix metal ions, leading to the formation of metal clusters, further reducing catalytic performance. Although increasing the amount of humic material can provide more support, the relatively fixed amount of metal salt leads to a decrease in the proportion of metal ions on the humic material support. Excessive humic material forms too many complexes with metal ions, hindering effective contact between metal ions, resulting in reduced catalyst activity.

[0224] Compared with Examples 11, 12, 17, and 18, with other conditions kept constant, the FDCA yield showed a trend of first increasing and then decreasing when the ultrasonic treatment time was extended from 0 minutes to 90 minutes. If the ultrasonic treatment time was too short or no ultrasonic treatment was performed, the humic macromolecular network could not be fully spread, resulting in a lower ability to capture metal active sites and thus a decrease in catalyst activity.

[0225] However, prolonged ultrasonic treatment can lead to excessive destruction of the macromolecular network structure of humic substances, reducing their effective ability to capture and fix metal ions. This causes metal ions to re-aggregate, forming larger metal clusters and reducing the number and dispersion of catalytic active sites. Therefore, reasonable control of ultrasonic time is beneficial for the full spread of the macromolecular network of humic substances, which enhances the ability to capture metal active sites and improves the catalytic activity of the catalyst.

[0226] Comparing Examples 11, 19, 20, and 21, the available chlorine content of sodium hypochlorite in Example 11 was 7.5%, and its FDCA yield was 93.9%. When the available chlorine content of sodium hypochlorite increased to 10% (Example 19), the FDCA yield slightly increased to 94.2%. This indicates that, within a certain range, increasing the available chlorine content of sodium hypochlorite helps to improve the oxidation efficiency of the reaction, thereby increasing the yield of FDCA. As an oxidant, the higher the available chlorine content of sodium hypochlorite, the stronger the activity of the oxidation reaction, thus promoting the efficiency of HMF conversion to FDCA.

[0227] However, when the available chlorine content of sodium hypochlorite decreased to 6% (Example 20), the FDCA yield dropped to 90.2%, and when it was further reduced to 4% (Example 21), the FDCA yield further decreased to 85.9%. This indicates that when the available chlorine content of sodium hypochlorite is below a certain level, the oxidation capacity of the reaction is limited, and oxygen vacancies and lattice oxygen on the catalyst surface cannot be effectively reformed, thus affecting the catalytic activity of the catalyst.

[0228] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for preparing a catalyst for 2,5-furandicarboxylic acid, characterized in that: include: (1) The humic substances generated during the preparation of 5-hydroxymethylfurfural are mixed with non-precious metal salts to form a dot network structure adsorbed with non-precious metal ions. (2) The catalyst for preparing 2,5-furandicarboxylic acid was then obtained through carbonization and surface oxidation treatment.

2. The method for preparing a catalyst for 2,5-furandicarboxylic acid according to claim 1, characterized in that: The weight ratio of the humic substance to the non-precious metal salt is 1:0.1-10, preferably 1:1-1.

5.

3. A method for preparing a catalyst for 2,5-furandicarboxylic acid according to claim 1 or 2, characterized in that: The non-precious metal salt is selected from one or more of cobalt, manganese, copper, and nickel salts; Preferably, the non-precious metal salt includes one or two of cobalt salt, nickel salt, and copper salt; Preferably, the non-precious metal salt includes one or both of nickel sulfate hexahydrate and cobalt acetate tetrahydrate; Preferably, the non-precious metal salt includes cobalt acetate tetrahydrate and copper salt; Preferably, the cobalt salt is 5-30 parts by weight and the copper salt is 0-25 parts by weight; Preferably, the cobalt salt is 10-30 parts by weight and the copper salt is 0-20 parts by weight.

4. A method for preparing a catalyst for 2,5-furandicarboxylic acid according to any one of claims 1-3, characterized in that: In step (1), the humic substances produced during the preparation of 5-hydroxymethylfurfural are mixed with water and non-precious metal salts to form a uniform mixture, and then subjected to ultrasonic treatment. Preferably, the ultrasonic treatment time is 20-90 min, more preferably 20-30 min.

5. The method for preparing a catalyst for 2,5-furandicarboxylic acid according to claim 4, characterized in that: In step (1), after ultrasonic treatment, an alkali agent is added, and the weight ratio of the humic substance to the alkali agent is 1:0.1-10. Preferably, the alkaline agent is selected from one or more of metal hydroxides or carbonates; Preferably, the alkaline agent is selected from one or more of sodium hydroxide, potassium hydroxide, barium hydroxide, sodium carbonate, and potassium carbonate.

6. A method for preparing a catalyst for preparing 2,5-furandicarboxylic acid according to any one of claims 1-5, characterized in that: In step (2), a sodium hypochlorite solution with an effective chlorine content of 4-30% is used for surface oxidation treatment; Preferably, a sodium hypochlorite solution with an effective chlorine content of 6-14% is used for surface oxidation treatment; Preferably, a sodium hypochlorite solution with an effective chlorine content of 7.5% is used for surface oxidation treatment; Preferably, the mass ratio of the humic substance to the sodium hypochlorite solution is 1:1-20.

7. The method for preparing a catalyst for 2,5-furandicarboxylic acid according to claim 6, characterized in that: In step (2), the carbonized product is first ground and sieved to obtain carbonized powder, and the carbonized powder is slowly added to sodium hypochlorite solution for surface oxidation treatment. Preferably, carbonized powder with a particle size of 200-400 mesh is obtained by sieving.

8. A method for preparing a catalyst for preparing 2,5-furandicarboxylic acid according to any one of claims 1-7, characterized in that: In step (2), carbonization includes: carbonization by gradient heating under an inert atmosphere.

9. A method for preparing a catalyst for 2,5-furandicarboxylic acid according to any one of claims 1-8, characterized in that: The humus is the humus produced during the preparation of 5-hydroxymethylfurfural using one or more of cellulose, glucose, fructose, starch, and sucrose as raw materials.

10. A method for preparing 2,5-furandicarboxylic acid, characterized in that: Includes the following steps: (1) Take sodium hypochlorite solution and disperse the catalyst prepared by any of the preparation methods described in claims 1-9 to obtain a dispersion; (2) Add an alkaline agent to the obtained dispersion, and then add 5-hydroxymethylfurfural to react and prepare 2,5-furandicarboxylic acid.