A chromium-silicon sputtering target, its preparation method and application

By constructing a continuously distributed grain boundary network structure and introducing functional elements in the chromium-silicon target, the problem of uneven distribution of free silicon phase was solved, and the high density of the target and the stability of the thin film were improved.

CN122189577BActive Publication Date: 2026-11-10GRIKIN ADVANCED MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202610440104.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-04-03
Publication Date
2026-11-10
Estimated Expiration
2046-04-03

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively control the distribution of free silicon phase in silicon-chromium-rich silicon targets, leading to target brittleness, arcing, and particulate contamination, which affect thin-film resistance and TCR stability.

Method used

The microstructure of the chromium-silicon target is constructed so that the free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and/or grain boundary bifurcations of the chromium silicide main phase. Functional elements Ti, Zr, Hf, and Y are introduced to capture impurities and form stable dispersed oxide particles. The chromium-silicon target is then prepared by vapor deposition, cold isostatic pressing, and hot isostatic pressing processes.

Benefits of technology

It effectively suppresses the random migration and aggregation of free silicon phase, reduces the risk of target embrittlement, reduces the number of particles during thin film deposition, and improves sputtering stability and thin film electrical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122189577B_ABST
    Figure CN122189577B_ABST
Patent Text Reader

Abstract

This invention provides a chromium-silicon sputtering target, its preparation method, and its applications, relating to the field of alloy sputtering target technology. The chromium-silicon sputtering target has a chromium silicide phase as its main phase framework, containing a free silicon phase. The free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. The grain boundary network structure includes at least the following characteristics (a) to (c): a) the free silicon phase covers 40-85% of the grain boundaries of the chromium silicide main phase; b) the maximum cluster size of the free silicon phase is ≤100 μm; c) the particle size D90 of the free silicon phase is ≤10 μm. This invention constructs a microstructure for the chromium-silicon sputtering target, which can avoid the random migration, diffusion, and aggregation of the free silicon phase, and its enrichment in the target blank pores or low diffusion energy regions. It suppresses the formation of coarse clusters, reduces the maximum cluster size of the free silicon phase and the risk of target brittleness, avoids arc light and particle sources during deposition, and improves sputtering stability and thin film electrical controllability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon-chromium alloy target technology, and in particular to a chromium-silicon target, its preparation method, and its application. Background Technology

[0002] Chromium-silicon alloy thin films, due to their high resistivity and good thermal stability, are widely used as resistive materials in high-precision thin-film resistors, analog / RF front-end resistor networks, and sensor readout circuits; these films are typically prepared by deposition using chromium-silicon alloy targets. The performance requirements for chromium-silicon alloy targets mainly include: (i) large-size targets (such as…) 200~ (i) The target material must have high density, low porosity and low inclusions (450mm); (ii) High consistency of structure and composition to avoid arcing, grain shedding and partial discharge during sputtering; (iii) The microstructure of the target material must be able to support the controllability of the thin film resistivity and temperature coefficient (TCR).

[0003] To improve target performance, numerous studies have been conducted on existing technologies. For example, CN113897585B employs a process of "powder preparation - surface treatment - plasma spraying - laser cladding - machining" to fabricate large-size rotating targets, which improves macroscopic density and strength and reduces oxygen content. However, due to the complex influence of the spraying and cladding layer microstructure characteristics and the Si migration and aggregation behavior in silicon-rich systems, it is difficult to achieve reproducible constraints on the microstructure variables of the free silicon phase. CN105331939A uses a process of powder mixing followed by cold isostatic pressing, encapsulation degassing and sealing, and HIP (hot isostatic pressing), which provides a wider range of Si content, but focuses on densification and general uniformity, lacking clear quantitative indicators for the grain boundary morphology, coverage, and cluster upper limit of the free silicon phase in silicon-rich systems. CN111058004A uses a process of "one-time mold loading - vibration compaction - degassing - HIP - machining," which can obtain high density and strength. While low-oxygen targets are being developed, the focus remains on efficiency and densification, lacking targeted closed-loop solutions for controllable indicators such as the network formation mechanism and scale distribution of the free silicon phase. JP2023064278A introduces C into the CrSi main phase to form a hard SiC second phase to suppress cracking and improve mechanical reliability, but this mechanism does not directly address issues such as random segregation of the free silicon phase, noise, and discharge window fluctuations in silicon-rich systems. Furthermore, a higher C / SiC ratio may lead to side effects such as changes in film composition and narrowing of the process window. CN113770360B and CN111996507A improve the densification and forming quality of the target material through multi-segment heat preservation / segmented pressurization strategies in vacuum hot pressing sintering, vacuum three-segment heat preservation sintering curves, and ball milling powder mixing, respectively. These approaches still belong to the route of achieving high density and uniform microstructure by optimizing the sintering curve.

[0004] In general, while the existing technologies can improve the density, strength and preparation efficiency of chromium-silicon targets to some extent, they lack effective control over the distribution of free silicon phase in silicon-rich chromium-silicon systems. However, in silicon-rich chromium-silicon systems, free silicon phases often migrate and aggregate randomly, and accumulate in the pores or low diffusion energy regions of the target blank to form coarse clusters. These coarse Si phases and their coupling with oxide inclusions can lead to target brittleness, and the occurrence of arc light and particle sources during deposition, resulting in particle contamination. The number of these particles will reduce the quality of the film (e.g., Selwyn GS, Weiss CA, Sequeda F, et al. Particle contamination formation in magnetron sputtering processes[J]. Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films, 1997, 15(4): 2023-2028. DOI: 10.1116 / 1.580674.), resulting in poor film sheet resistance and TCR stability.

[0005] Therefore, how to reduce the number of particles during thin film deposition to improve the sheet resistance and TCR stability has become an urgent problem to be solved. Summary of the Invention

[0006] To address the aforementioned technical problems, this invention provides a chromium-silicon target, its preparation method, and its application. The specific solution is as follows: In a first aspect, the present invention provides a chromium-silicon sputtering target, wherein the chromium-silicon sputtering target has a chromium silicide phase as the main phase framework and contains a free silicon phase, wherein the free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary bifurcations of the chromium silicide main phase, and the grain boundary network structure includes at least the following features a to c: a. The free silicon phase has a grain boundary coverage of 40-85% in the chromium silicide main phase; b. The maximum cluster size of the free silicon phase is ≤100 μm; c. The particle size of the free silicon phase, D90, is ≤10 μm.

[0007] This invention constructs a microstructure for a chromium-silicon target material. Using the chromium silicide phase as the main phase framework, the free silicon (Si) phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. This effectively avoids the phenomenon that the free silicon phase often undergoes random migration, diffusion, and aggregation, and accumulates in the pores or low diffusion energy regions of the target blank. This effectively suppresses the formation of coarse clusters caused by the diffusion of the free silicon phase, reduces the maximum cluster size of the free silicon phase, and thus effectively reduces the risk of target material brittleness. It also avoids the occurrence of arc light and particle sources during the deposition process, effectively reduces the number of particles during thin film deposition, and improves sputtering stability and thin film electrical stability.

[0008] Furthermore, the free silicon phase accounts for 8 to 30 vol% of the volume of the chromium-silicon target material. This volume fraction corresponds to a chromium to silicon mass ratio of 1:1 to 3 and the silicon content in the chromium-silicon core-shell structure. This volume percentage can be statistically analyzed using cross-sectional scanning electron microscopy (SEM) and surface energy dispersive X-ray spectroscopy (EDS).

[0009] Furthermore, the mass ratio of chromium to silicon in the chromium-silicon target is 1:1 to 3. This mass ratio is primarily based on the dual requirements of thin film physical property control and sputtering kinetics adaptation. From a materials science perspective, chromium and silicon can form various intermetallic compounds such as CrSi2, CrSi, and Cr3Si. This composition range covers a multiphase coexistence region, from chromium-rich solid solutions to silicon-rich silicides. By adjusting the chromium-silicon ratio, the resistivity and temperature coefficient of resistance of the deposited thin film can be effectively controlled to achieve precision resistor applications. Simultaneously, within this ratio range, the thin film readily forms amorphous or nanocrystalline microstructures, significantly suppressing grain boundary diffusion and surface migration, thereby improving the long-term stability and anti-electromigration capability of the thin film. From a sputtering process perspective, the sputtering yields of chromium and silicon differ, and the target composition must balance the sputtering rates of both to ensure uniform and controllable thin film composition. A mass ratio of 1:1 to 3 precisely maintains the atomic fraction of chromium at 50-75 at.%, achieving good correspondence between the thin film composition and the target composition under common sputtering conditions, avoiding compositional shifts caused by selective sputtering.

[0010] Furthermore, the chromium-silicon target material also contains a functional element M with a mass fraction of 50-500 ppm, wherein the functional element M is selected from one or more of Ti, Zr, Hf, and Y, and is dispersed in the form of oxygen-containing compound particles at the grain boundaries and / or grain boundary bifurcations of the chromium silicide main phase.

[0011] Ti, Zr, Hf, Y, and other Group IVB and IIIB transition metals were chosen as functional elements for absorbing impurities primarily due to their unique outer layers. dThe strong affinity properties resulting from their electron orbital configurations. These elements possess extremely high oxygen and carbon potentials, enabling irreversible selective reactions with free O and C in the matrix to generate thermodynamically stable compounds with extremely high negative enthalpy of formation, such as oxides or carbides. This transforms harmful interstitial solid-solution atoms into dispersed inert second-phase particles. This purification process not only significantly reduces lattice distortion and impurity brittleness in the matrix but also, thanks to the high melting point and low diffusion coefficient of these carbon oxides, achieves long-term pinning of impurity atoms. Furthermore, the specific regulatory capabilities of Ti, Zr, Hf, and Y on grain boundary oxidation behavior further enhance the material purification and interface stabilization effects.

[0012] The mass fraction of functional element M in the chromium-silicon target is controlled between 50 and 500 ppm, effectively avoiding the negative effects caused by excessive residual active elements. When the mass fraction of functional element M exceeds 500 ppm, unreacted free Ti, Zr, Hf, and Y tend to segregate at grain boundaries or form coarse intermetallic compounds with matrix elements, which weakens the grain boundary bonding strength, induces stress concentration, and reduces the plasticity and fatigue resistance of the alloy. At the same time, excessive addition may change the intrinsic compositional balance of the matrix. Therefore, 500 ppm is a threshold that balances deep purification efficiency and crystal structure, giving full play to the strong affinity and impurity removal function of trace elements while strictly avoiding secondary performance degradation caused by over-alloying.

[0013] Preferably, the oxygen-containing compound particles are MO and / or M-Si-O particles, and their equivalent particle size is ≤0.5 μm.

[0014] In the preparation of chromium-silicon sputtering targets, impurities such as O and C are inevitably present. These impurities exist in unfavorable forms such as continuous oxide films or coarse inclusions, weakening grain boundary bonding, inducing discharge instability, and increasing noise. To control the morphology of O and C impurities, functional elements are introduced into the chromium-silicon sputtering target of this invention. By using trace amounts of functional elements to capture and purify impurities such as O and C, MO and / or M-Si-O oxygen-containing compound particles are formed and enriched in a dispersed and fine morphology at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. This transforms impurity fluctuations into a stable and dispersed grain boundary structure, improving sputtering stability and thin film electrical stability.

[0015] Furthermore, the surface roughness Ra of the chromium-silicon target is ≤0.4 μm, and the relative density is ≥99%.

[0016] A second aspect of the present invention provides a method for preparing the above-mentioned chromium-silicon target, comprising the following steps: (1) Using silicon powder as the core, a chromium shell is formed on the surface of the silicon core by vapor deposition to obtain Si@Cr core-shell precursor powder; (2) The Si@Cr core-shell precursor powder is subjected to cold isostatic pressing, encapsulation vacuum degassing and sealing, hot isostatic pressing (HIP) and machining in sequence.

[0017] To improve the density and other properties of silicon-chromium targets, conventional preparation methods rely on direct mixing of Cr powder / CrSi powder / CrSi2 powder + Si powder. This method, lacking a core-shell structure, allows the free silicon phase to randomly diffuse, migrate, and aggregate, accumulating in the pores or low-diffusion-energy regions of the target blank to form coarse clusters. This invention reveals that by adjusting the formation path of the free silicon phase during the preparation of chromium-silicon targets to a closed-loop control system of core-shell confinement, quantitative release, grain boundary wetting, and slow cooling and shaping, the coarse clustering of the free silicon phase can be effectively avoided, reducing the number of particles during film deposition. Specifically: Core-shell confinement: Using large-particle-size Si powder as the core, chromium is deposited on the surface of the silicon core using vapor deposition to form a chromium shell. The chromium shell (Cr shell) confines Si within the shell, greatly reducing its random diffusion reaction and large-area outflow. Quantitative release: During subsequent hot isostatic pressing (solid-phase densification stage), the Cr shell preferentially undergoes interfacial silanization reaction to form a silanized chromium outer skin, thereby providing a confinement effect for the melting and outward infiltration of Si in the core during the transient liquid phase stage of hot isostatic pressing. Grain boundary wetting: The release location, release rate and maximum cluster size of the free silicon phase can be engineered to constrain its diffusion reaction to occur only within the Cr shell. It cannot accumulate in the target blank pores or low diffusion energy regions to form coarse clusters. Moreover, it preferentially spreads along the chromium silicide grain boundaries and fills the powder gaps, growing into a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary forks of the chromium silicide main phase. This reduces the risk of brittle fracture and discharge instability caused by segregation and pore coupling in the silicon-rich system, and significantly improves the microstructure and batch stability of large-size target materials. Slow cooling and shaping: refers to the chromium silicide and free silicon phase in the target blank being cooled with temperature after hot isostatic pressing and shaped at room temperature.

[0018] Furthermore, the chromium shell has a surface coverage of 70-95% on the silicon core, with an equivalent thickness of 10-300 nm. Achieving a chromium shell surface coverage of 70-95% on the silicon core is a key threshold for ensuring compositional uniformity and controllable microstructure during powder metallurgy. First, the high surface coverage of the chromium shell forms a physical barrier for the silicon nucleus, effectively preventing direct large-area contact between silicon and chromium during the sintering densification stage. This significantly suppresses local overheating, compositional overburning, and non-equilibrium precipitation of brittle phases caused by the intense exothermic reaction of Cr and Si, thus avoiding a decrease in target density and the initiation of microcracks. Second, the chromium shell imparts uniform local compositional characteristics to each composite powder particle, allowing chromium to be distributed in a three-dimensional continuous network within the target matrix. This fundamentally eliminates the macroscopic segregation caused by the density difference and particle size variation of chromium and silicon in traditional mechanically mixed powders, ensuring high uniformity and batch stability of the sputtering surface composition. Furthermore, a low surface coverage of less than 70% is prone to abnormal grain growth or excessive reaction with the chromium liquid phase during sintering of exposed silicon nuclei. Complete encapsulation with a surface coverage of more than 95% poses challenges to process economy and particle size control. A surface coverage of 70–95% has been verified as a range that balances reaction suppression and preparation feasibility. By controlling the equivalent thickness within the above range, we can ensure that the chromium shell has sufficient physical continuity to achieve effective coating under high coverage, while also avoiding the shell layer being too thick, which would cause the mass percentage of chromium to silicon in the target material to deviate from the target range of 1:1 to 3, or cause the coating layer to peel off due to stress accumulation in the shell layer.

[0019] Further, step (1) includes: using a carrier gas to deliver a gaseous chromium source into a silicon powder-containing deposition zone, and performing vapor deposition at a temperature of 100~200 °C for 10~120 min. By using these specific deposition parameters, chromium can be deposited on the surface of the silicon core, allowing the surface coverage and thickness of the chromium shell to be controlled within the aforementioned range.

[0020] Preferably, the chromium source includes CrCl3 and / or CrBr3.

[0021] Preferably, the particle size of the silicon powder is 20~100 μm.

[0022] Preferably, the vapor deposition is performed in a reducing atmosphere.

[0023] Preferably, the carrier gas is Ar, and the reducing gas used in the reducing atmosphere is H2. 2。

[0024] Preferably, the step of preparing the gaseous chromium source includes: vaporizing the chromium source at 600~850°C.

[0025] Furthermore, after the vapor deposition is completed, a carrier gas is used to purge and keep warm in a reducing atmosphere for a period of time to reduce residual volatile impurities (such as C, H, etc.); preferably, purging is carried out at 100°C for 2 hours.

[0026] Furthermore, before the Si@Cr core-shell precursor powder is subjected to cold isostatic pressing, it is further comprising a step of mixing it with CrSi2 pre-alloy powder containing functional element M, so that the mass ratio of chromium to silicon in the mixed system is 1:1~3 and the mass fraction of functional element M is 50~500 ppm.

[0027] To address the unavoidable and difficult-to-complete elimination of O, C, and metallic impurities, this invention innovatively incorporates impurity behavior into the target structure design. It introduces 50–500 ppm of functional element M to preferentially capture oxygen and some carbon-related active sites sensitive to discharge and noise. This transforms unfavorable morphologies such as random solid solution or continuous oxide films at grain boundaries into stable, dispersed MO and M-Si-O particles, which are then directionally enriched at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. This achieves a dual effect of grain boundary purification and grain boundary pinning. It suppresses the formation of continuous insulating films and coarse impurities, reduces arc light and particle sources, and improves sputtering performance. Simultaneously, the synergistic pinning effect effectively inhibits the re-coarsening and agglomeration of the free silicon phase in the liquid phase, making the grain boundary Si network easier to expand and replicate, thus increasing film uniformity and device stability.

[0028] Preferably, the mass fraction of functional element M in the CrSi2 pre-alloyed powder is ≥500 ppm.

[0029] Preferably, the particle size D90 of the CrSi2 pre-alloyed powder is 20~100 μm.

[0030] Furthermore, the hot isostatic pressing is performed in two stages. The parameters for the first stage of hot isostatic pressing include: temperature of 1050~1250 ℃, pressure of 100~200 MPa, and holding time of 1~4 h. The parameters for the second stage of hot isostatic pressing include: temperature of 1420~1470 ℃, pressure of 100~200 MPa, and holding time of 5~20 min.

[0031] Two-stage HIP achieves both high density and grain boundary wetting and shaping, reducing the risk of large-size cracking and improving radial consistency. This invention employs two-stage HIP to achieve solid-state densification of the chromium silicide main phase framework and the free silicon phase. A short-term crossing of the Si melting point forms grain boundary wetting of the free silicon phase, followed by cooling to form a closed-loop process. While ensuring density and microstructure uniformity, the capillary wetting behavior of the short-term transient liquid phase allows the free silicon phase to preferentially spread along the chromium silicide grain boundaries and fill powder gaps. This reduces the risk of brittle fracture and discharge instability caused by segregation and porosity coupling in silicon-rich systems, reduces the number of particles in the thin film deposition process, and significantly improves the microstructure and batch stability of large-size targets.

[0032] Preferably, after hot isostatic pressing, the material is cooled and shaped at a rate of 1~10 °C / min. Specifically, the temperature is reduced to below 900 °C at a rate of 1~10 °C / min, followed by furnace cooling. Furthermore, the vacuum degree during the vacuum degassing of the enclosure is ≤10. -2 Pa, the degassing temperature is 350~600℃, and the degassing time is 2~10 h.

[0033] Furthermore, the machining process includes a decoupling and annealing step, wherein the annealing step includes annealing at 400~700°C for 1~4 h in a vacuum or inert atmosphere to release residual stress.

[0034] A third aspect of the present invention provides the application of the above-described chromium-silicon target or the chromium-silicon target prepared by the above-described preparation method in the preparation of chromium-silicon alloy thin films.

[0035] The chromium-silicon target material, its preparation method, and its application provided by this invention have at least the following beneficial effects: This invention constructs a microstructure for the chromium-silicon target material, which uses the chromium silicide phase as the main phase framework as a carrier, so that the free silicon (Si) phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary forks of the chromium silicide main phase. This can effectively avoid the phenomenon that the free silicon phase often undergoes random migration and diffusion, agglomeration, and enrichment in the target blank pores or low diffusion energy regions. This can effectively suppress the formation of coarse clusters caused by the diffusion of the free silicon phase, reduce the maximum cluster size of the free silicon phase, and thus effectively reduce the risk of target material brittleness, avoid the occurrence of arc light and particle sources during the deposition process, reduce the number of particles during thin film deposition, and improve sputtering stability and thin film electrical stability. Attached Figure Description

[0036] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0037] Figure 1 This is a flowchart illustrating the structure and preparation process of the chromium-silicon target material of the present invention.

[0038] Figure 2 This is a SEM image showing the distribution of free Si phase along grain boundaries in the chromium-silicon target of Example 1.

[0039] Figure 3 This is an SEM image showing the distribution of free Si phase along grain boundaries in the chromium-silicon target of Example 2.

[0040] Figure 4This is a SEM image of the distribution of free Si phase along grain boundaries in the chromium-silicon target material of Example 3. Detailed Implementation

[0041] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0042] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field, or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.

[0043] In this invention, the detection methods for each performance parameter are as follows: Grain boundary coverage of free silicon phase: SEM and EDS were used for detection. The standard procedure is as follows: The sample was precision polished and argon ion polished to remove the surface deformation layer. If necessary, a light chemical etching was used to enhance the grain boundary contrast. In backscattered electron mode, the chromium matrix grain boundaries were identified based on atomic number contrast, and high-resolution secondary electron morphology images and silicon elemental EDS surface distribution maps were acquired simultaneously. The volume percentage of silicon was calculated by image spatial overlay and data extraction from the grain boundary region. The measurement required the random selection of no less than 10 independent fields of view, covering a total grain boundary length of no less than 500 μm. A pure chromium reference sample was used to correct the background noise. The final results were presented in the form of mean ± standard deviation, realizing a quantitative evaluation of the degree of silicon segregation along the grain boundaries. The detection method is referenced from: Zhou Yu. Materials Analysis Methods [M]. 4th Edition. Beijing: Machinery Industry Press, 2020. Maximum cluster size and particle size: measured using a laser particle size analyzer, referring to GB / T 19077-2024; Volume fraction of free silicon: statistically determined by a combination of cross-sectional scanning electron microscopy (SEM) and surface energy dispersive X-ray spectroscopy (EDS); detection method reference: Zhou Yu. Materials Analysis Methods [M]. 4th ed. Beijing: Machinery Industry Press, 2020; The equivalent thickness of the Cr shell was measured by a weight gain of 0.5-10%, and calibrated by combining cross-sectional SEM statistical shell thickness distribution with EDS statistical coverage and Cr shell thickness; the detection method reference is: Zhou Yu. Materials Analysis Methods [M]. 4th ed. Beijing: Machinery Industry Press, 2020; Cr shell surface coverage: Calibration was performed by combining cross-sectional scanning electron microscopy (SEM) statistical shell thickness distribution with surface energy dispersive X-ray spectroscopy (EDS) statistical coverage; Detection method reference: Zhou Yu. Materials Analysis Methods [M]. 4th ed. Beijing: Machinery Industry Press, 2020; Surface roughness: Measured with a roughness tester, refer to GB / T 6062-2009; Relative density: Archimedes displacement method, refer to GB / T 3850-2015.

[0044] Example 1 This embodiment provides a method for preparing a chromium-silicon target, including the following steps: (1) Preparation of Si@Cr core-shell precursor powder: A volatile Cr source (CrCl3) was placed in the upstream supply zone and heated to 780℃ to provide a Cr-containing gas phase (flow rate of 80 mL / min); large-particle-size Si powder (particle size of Si powder is 20 μm) was selected as the core, and 10 kg of Si powder (purity ≥4N) was placed in the downstream deposition zone of the tube furnace. Ar carrier gas (flow rate of 80 mL / min) and a small amount of H2 reducing gas (flow rate of 20 mL / min) were introduced into the upstream supply zone to carry the Cr gas phase into the downstream deposition zone. The temperature of the downstream deposition zone was controlled at 150℃ for vapor phase deposition for 60 min, so that chromium was deposited on the surface of the silicon core to form a chromium shell. After deposition, the core was purged and kept at 100℃ for 2 h in Ar (containing a small amount of H2) to reduce residual volatile impurities (such as C, H, etc.). The obtained Si@Cr core-shell precursor powder was subjected to weight gain measurement, and the Cr shell thickness was statistically analyzed by cross-sectional SEM and the coverage was statistically analyzed by EDS. It was found that the equivalent thickness of the Cr shell was 200 nm, and its surface coverage on the silicon core was 90%, ensuring that the mass ratio (mass ratio Cr:Si=1:2) met the requirements.

[0045] (2) Mixed phase seed: Using Y-containing CrSi2 pre-alloyed powder (D90=50 μm, the mass fraction of Y in the pre-alloyed powder is 2100 ppm) as the phase seed, the CrSi2 pre-alloyed powder is mixed with the Si@Cr core-shell precursor powder so that the Cr:Si=1:2 and the mass fraction of Y is 300 ppm in the mixed system. The mixture is ball-milled under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0046] (3) Cold Isostatic Pressing (CIP), Encasing Degassing and Sealing: The mixed powder is loaded into a rubber mold and cold isostatically pressed under the parameters of 300 MPa for 20 min to obtain a blank. The blank is then encased in a metal casing; vacuum degassing is performed (vacuum degree ≤ 10). -2 Pa, degassing temperature 450 ℃, degassing time 6 h, followed by sealing.

[0047] (4) Two-stage HIP: The encapsulated blank is subjected to two-stage HIP. The first stage is solid-state densification at 1150 °C and locking the main phase skeleton and grain boundary channels. The pressure is 150 MPa and the temperature is held for 2 h. The second stage is to briefly cross the melting point of Si at 1450 °C to form a transient Si-rich liquid phase and spread along the grain boundary under capillary wetting drive. The pressure is 150 MPa and the temperature is held for 10 min. Then, it is slowly cooled in a controlled manner at 3 °C / min to below 900 °C and then furnace cooled.

[0048] (5) Removal of the cladding, annealing, and machining: After removing the cladding, the sample is held at 550 °C for 2 h in a vacuum or inert atmosphere to release residual stress; subsequently, it is machined to obtain the specified dimensions. The target material is a 200 mm × 8 mm thick disc, and the target surface is finely ground and polished to a surface roughness Ra≤0.4 μm.

[0049] The structure of the chromium-silicon target material prepared by the above method is as follows: Figure 1 As shown, the chromium-silicon target material has a chromium silicide phase as the main phase framework and contains a free silicon phase. The free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. The mass ratio of chromium to silicon in the chromium-silicon target material is 1:2. The chromium-silicon target material also contains 300 ppm of Y (yttrium) by mass, which is dispersed in the form of YO and / or Y-Si-O oxygen-containing compound particles at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase; the equivalent particle size of the oxygen-containing compound particles is ≤0.5 μm.

[0050] Furthermore, testing revealed that the relative density of the chromium-silicon target was 99.7%, which is ≥99% (measured by Archimedes' water displacement method); the volume percentage of the free silicon phase in the chromium-silicon target was 10 vol%; the grain boundary coverage of the free silicon phase in the chromium silicide main phase was 60%; the maximum cluster size of the free silicon phase was 80 μm, which is ≤100 μm; and the particle size D90 of the free silicon phase was 8 μm, which is ≤10 μm. Figure 2 This is a SEM image showing the distribution of the free Si phase (darker areas) along the grain boundaries. The free Si phase is mainly distributed at the grain boundaries, with no obvious coarse, blocky agglomerations observed. This result indicates that the free Si phase can form a uniform and continuous grain boundary network structure along the grain boundaries of the chromium silicide main phase. The particle count during thin film deposition was 0.08 particles / cm². 2 .

[0051] Example 2 This embodiment provides a method for preparing a chromium-silicon target, the flowchart of which is shown below. Figure 1 As shown, it includes the following steps: (1) Preparation of Si@Cr core-shell precursor powder: A volatile Cr source (CrBr3) was placed in the upstream supply zone and heated to 720℃ to provide a Cr-containing gas phase (flow rate of 80 mL / min); large-particle-size Si powder (particle size of Si powder is 30 μm) was selected as the core, and 10 kg of Si powder (purity ≥4N) was placed in the downstream deposition zone of the tube furnace. Ar carrier gas (flow rate of 80 mL / min) and a small amount of H2 reducing gas (flow rate of 20 mL / min) were introduced into the upstream supply zone to carry the Cr gas phase into the downstream deposition zone. The temperature of the downstream deposition zone was controlled at 180 ℃ for vapor phase deposition for 90 min, so that chromium was deposited on the surface of the silicon core to form a chromium shell. After deposition, the core was purged and kept at 100 ℃ for 2 h in Ar (containing a small amount of H2) to reduce residual volatile impurities (such as C, H, etc.). The obtained Si@Cr core-shell precursor powder was subjected to weight gain measurement, and the Cr shell thickness was statistically analyzed by cross-sectional SEM and the coverage was statistically analyzed by EDS. It was found that the equivalent thickness of the Cr shell was 150 nm, and its surface coverage on the silicon core was 90%, ensuring that the mass ratio (mass ratio Cr:Si = 1:1.4) met the requirements.

[0052] (2) Mixed phase seed: Using Zr-containing CrSi2 pre-alloyed powder (D90=50 μm, the mass fraction of Zr in the pre-alloyed powder is 1400 ppm) as the phase seed, the CrSi2 pre-alloyed powder is mixed with the Si@Cr core-shell precursor powder so that the Cr:Si ratio is 1:1.4 and the mass fraction of Zr is 200 ppm in the mixed system. The mixture is ball-milled under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0053] (3) Cold isostatic pressing, degassing and sealing: The mixed powder is loaded into a rubber mold and cold isostatically pressed under the parameters of 250 MPa and 15 min to obtain a blank. The blank is then loaded into a metal sleeve; vacuum degassing (vacuum degree ≤ 10) is performed. -2 Pa, degassing temperature is 500 ℃, degassing time is 4 h, and then sealing is performed.

[0054] (4) Two-stage HIP: The encapsulated blank is subjected to two-stage HIP. The first stage of HIP is carried out at 1120 ℃, 150 MPa and 2 h to complete solid-phase densification and skeleton locking. The second stage of HIP is carried out at 1435 ℃, 150 MPa and 8 min to form transient Si-rich liquid phase and spread along the grain boundary capillary wetting. Then it is slowly cooled to below 900 ℃ at 2 ℃ / min and then furnace cooled.

[0055] (5) Removal of the cladding, annealing, and machining: After removing the cladding, the sample is held at 600 ℃ for 2 h in a vacuum or inert atmosphere to release residual stress; subsequently, it is machined to obtain the specified dimensions. The target material is a 300 mm × 10 mm thick disc, and the target surface is finely ground and polished to a surface roughness Ra≤0.4 μm.

[0056] The structure of the chromium-silicon target material prepared by the above method is as follows: Figure 1 As shown, the chromium-silicon target material has a chromium silicide phase as the main phase framework and contains a free silicon phase. The free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. The mass ratio of chromium to silicon in the chromium-silicon target material is 1:1.4. The chromium-silicon target material also contains 200 ppm of Zr (zirconium) by mass, and it is dispersed in the form of Zr-O and / or Zr-Si-O oxygen-containing compound particles at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase; the equivalent particle size of the oxygen-containing compound particles is ≤0.5 μm.

[0057] Furthermore, testing revealed that the relative density of the chromium-silicon target was 99.5%, which is ≥99% (measured by Archimedes' water displacement method); the volume percentage of the free silicon phase in the chromium-silicon target was 8 vol%; the grain boundary coverage of the free silicon phase in the chromium silicide main phase was 50%; the maximum cluster size of the free silicon phase was 75 μm, which is ≤100 μm; and the particle size D90 of the free silicon phase was 7 μm, which is ≤10 μm. Figure 3 This is a SEM image showing the distribution of the free Si phase (darker areas) along the grain boundaries. The free Si phase is mainly distributed at the grain boundaries, with no obvious coarse, blocky agglomerations observed. This result indicates that the free Si phase can form a uniform and continuous grain boundary network structure along the grain boundaries of the chromium silicide main phase. The particle count during thin film deposition was 0.09 particles / cm². 2 .

[0058] Example 3 This embodiment provides a method for preparing a chromium-silicon target, the flowchart of which is shown below. Figure 1 As shown, it includes the following steps: (1) Preparation of Si@Cr core-shell precursor powder: A volatile Cr source (CrCl3 or CrBr3) was placed in the upstream supply zone and heated to 750 °C to provide a Cr-containing gas phase (flow rate of 80 mL / min); large-particle-size Si powder (particle size of Si powder is 90 μm) was selected as the core, and 10 kg of Si powder (purity ≥4N) was placed in the downstream deposition zone of the tube furnace. Ar carrier gas (flow rate of 80 mL / min) was introduced into the upstream supply zone, and a small amount of H2 reducing gas (flow rate of 20 mL / min) was introduced to carry the Cr gas phase into the downstream deposition zone. The temperature of the downstream deposition zone was controlled at 150 °C for vapor phase deposition for 60 min, so that chromium was deposited on the surface of the silicon core to form a chromium shell. After deposition, the core was purged and kept at 100 °C for 2 h in Ar (containing a small amount of H2) to reduce residual volatile impurities (such as C, H, etc.). The obtained Si@Cr core-shell precursor powder was subjected to weight gain measurement, and the Cr shell thickness was statistically analyzed by cross-sectional SEM and the coverage was statistically analyzed by EDS. It was found that the equivalent thickness of the Cr shell was 180 nm, and its surface coverage on the silicon core was 80%, ensuring that the mass ratio (mass ratio Cr:Si = 1:1.8) met the requirements.

[0059] (2) Mixed phase seed: Using Hf-containing CrSi2 pre-alloyed powder (D90=60 μm, the mass fraction of Zr in the pre-alloyed powder is 1050 ppm) as the phase seed, the CrSi2 pre-alloyed powder is mixed with the Si@Cr core-shell precursor powder so that the Cr:Si ratio is 1:1.8 and the mass fraction of Hf is 150 ppm in the mixed system. The mixture is ball-milled under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0060] (3) Cold isostatic pressing, degassing and sealing: The mixed powder is loaded into a rubber mold and cold isostatically pressed under the parameters of 300 MPa for 30 min to obtain a blank. Then the blank is loaded into a metal sleeve; vacuum degassing (vacuum degree ≤ 10) is performed. -2 Pa, degassing temperature is 500 ℃, degassing time is 6 h, and then sealing is performed.

[0061] (4) Two-stage HIP: The encapsulated blank after sealing is subjected to two-stage HIP. The first stage of HIP is carried out at 1100 ℃, 100 MPa and held for 2 h to complete solid-phase densification and skeleton locking. The second stage of HIP is carried out at 1450 ℃, 150 MPa and held for 10 min to form transient Si-rich liquid phase and spread along the grain boundary capillary wetting. Then it is slowly cooled to below 900 ℃ at 4 ℃ / min and then furnace cooled.

[0062] (5) Removal of the cladding, annealing, and machining: After removing the cladding, the sample is held at 500 °C for 2 h in a vacuum or inert atmosphere to release residual stress; subsequently, it is machined to obtain the specified dimensions. The target material is a 300 mm × 10 mm thick disc, and the target surface is finely ground and polished to a surface roughness Ra≤0.4 μm.

[0063] The structure of the chromium-silicon target material prepared by the above method is as follows: Figure 1 As shown, the chromium-silicon target material has a chromium silicide phase as the main phase framework and contains a free silicon phase. The free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary junctions of the chromium silicide main phase. The mass ratio of chromium to silicon in the chromium-silicon target material is 1:1.8. The chromium-silicon target material also contains 150 ppm of Hf (hafnium) by mass, and it is dispersed in the form of oxygen-containing compound particles (Hf-O and / or Hf-Si-O) at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase; the equivalent particle size of the oxygen-containing compound particles is ≤0.5 μm.

[0064] Furthermore, testing revealed that the relative density of the chromium-silicon target was 99.8%, which is ≥99% (measured by Archimedes' water displacement method); the free silicon phase accounted for 15 vol% of the volume of the chromium-silicon target; the free silicon phase had a grain boundary coverage of 50% in the chromium silicide main phase; the maximum cluster size of the free silicon phase was 90 μm, which is ≤100 μm; and the particle size D90 of the free silicon phase was 8 μm, which is ≤10 μm. Figure 4 This is a SEM image showing the distribution of the free Si phase (darker areas) along the grain boundaries. The free Si phase is mainly distributed at the grain boundaries, with no obvious coarse, blocky agglomerations observed. This result indicates that the free Si phase can form a uniform and continuous grain boundary network structure along the grain boundaries of the chromium silicide main phase. The particle count during thin film deposition was 0.07 particles / cm². 2 .

[0065] Comparative Example 1 This comparative example uses a conventional method to prepare a chromium-silicon target, which includes the following steps: (1) Raw material mixing: Si powder (the same Si powder as in Example 1) is mixed with CrSi2 pre-alloyed powder (which does not contain Y element compared with CrSi2 pre-alloyed powder in Example 1) so that the mass ratio of Cr to Si in the mixed system is 1:2. The mixture is ball-milled under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0066] (2) Cold isostatic pressing, vacuum degassing and sealing: Performed under the same conditions as step (3) of Example 1.

[0067] (3) Single-stage HIP: Densification is carried out using conventional single-stage HIP with the following parameters: temperature 1150 ℃, pressure 150MPa, time 2 h, followed by furnace cooling.

[0068] (4) De-coating, annealing and machining: After de-coating, proceed under the same conditions as step (5) of Example 1.

[0069] Although the chromium-silicon target prepared in Comparative Example 1 achieved a high relative density (99%), it exhibited the following typical differences in microstructure control: Free silicon phases tend to migrate and aggregate randomly. Due to the lack of core-shell confinement and quantitative release mechanisms, free silicon in silicon-rich systems tends to migrate and aggregate in pores or low-diffusion-energy regions, failing to stably form a continuous network structure along the chromium silicide grain boundaries; cluster size and particle size distribution are out of control, with free Si phases forming coarse clusters, the largest cluster size exceeding 100 μm and reaching 150 μm, and the particle size D90 cannot be stably controlled within ≤10 μm; grain boundary coverage fluctuates significantly and cannot fall within the reproducible range of 40–85%; impurity morphology is unfavorable. Without the addition of functional element M, residual O / C and other impurities are more likely to exist near grain boundaries / pores in unfavorable forms such as continuous oxide films or coarse inclusions, weakening grain boundary bonding and increasing the risk of arcing, grain shedding, and partial discharge during sputtering, thus making it difficult to stabilize the film resistivity and TCR. The number of particulate contaminants during film deposition was 0.7 particles / cm. 2 .

[0070] Comparative Example 2 The difference between this comparative example and Example 1 is that: instead of preparing Si@Cr core-shell precursor powder, Si powder is directly mixed with Y-containing CrSi2 pre-alloyed powder; the remaining steps (CIP, cladding degassing and sealing, two-stage HIP, controlled slow cooling, decladding, annealing and machining) are the same as in Example 1. The preparation method steps are as follows: (1) Raw material mixing: The same Si powder as in Example 1 and the same Y-containing CrSi2 pre-alloyed powder as in Example 1 are mixed according to the set ratio so that Cr:Si = 1:2 in the mixed system and the mass fraction of Y is 300 ppm; the mixture is ball-milled under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0071] (2) Cold isostatic pressing, degassing and sealing: Performed under the same conditions as step (3) in Example 1.

[0072] (3) Two-stage HIP: Performed under the same conditions as step (4) of Example 1.

[0073] (4) Remove the casing, anneal and machine: Perform the same conditions as step (5) in Example 1.

[0074] Organization and testing results: The chromium-silicon target material prepared in this comparative example still contains 300 ppm of Y by mass, and after heat treatment, YO and / or Y-Si-O oxygen-containing compound particles can be observed to be dispersed at grain boundaries and / or grain boundary junctions, with the equivalent particle size of the oxygen-containing compound particles being ≤0.5 μm. The relative density of the target material can still reach ≥99% (determined by Archimedes' displacement method).

[0075] However, due to the lack of core-shell confinement and quantitative release mechanisms, the free silicon phase undergoes random migration and aggregation in the silicon-rich system, failing to stably form a grain boundary network structure continuously distributed along the chromium silicide main phase grain boundaries. Compared to Example 1, the grain boundary coverage (30%) in this comparative example is significantly reduced, the maximum cluster size of the free silicon phase exceeds 100 μm (up to 150 μm), and the particle size D90 is difficult to stably control at ≤10 μm (15 μm), failing to meet the characteristics a~c of the grain boundary network structure. The number of particulate contaminants during thin film deposition is 0.6 particles / cm. 2 .

[0076] Comparative Example 3 The difference between this comparative example and Example 1 is that the CrSi2 pre-alloyed powder used for the mixed phase seed does not contain Y (no functional element M is introduced); the remaining steps (Si@Cr core-shell precursor powder preparation, CIP, cladding degassing and sealing, two-stage HIP, controlled slow cooling, decladding, annealing and machining) are the same as in Example 1. The preparation method steps are as follows: (1) Preparation of Si@Cr core-shell precursor powder: Si@Cr core-shell precursor powder was prepared using the same raw materials and conditions as in step (1) of Example 1.

[0077] (2) Mixed phase seed: Y-free CrSi2 pre-alloyed powder (particle size consistent with Example 1, D90=50 μm) is used as the phase seed and mixed with the Si@Cr core-shell precursor powder to make Cr:Si=1:2 in the mixed system; ball milling under an inert atmosphere to achieve uniform dispersion and obtain mixed powder.

[0078] (3) Cold isostatic pressing, degassing and sealing: Performed under the same conditions as step (3) in Example 1.

[0079] (4) Two-stage HIP: Performed under the same conditions as step (4) in Example 1.

[0080] (5) Remove the casing, anneal and machine: Perform the same conditions as step (5) in Example 1.

[0081] Organization and testing results: The relative density of the chromium-silicon target material prepared in this comparative example can still reach ≥99% (determined by Archimedes' water displacement method); the free silicon phase can still form a continuous grain boundary network structure, and the volume percentage (10 vol%), grain boundary coverage (60%), maximum cluster size (≤100 μm), and particle size D90 (≤10 μm) of the free silicon phase are close to those of Example 1.

[0082] However, due to the absence of functional element M(Y), residual O / C and other impurities are more likely to exist in unfavorable forms such as continuous oxide films or coarse inclusions near grain boundaries and / or pores. Cross-sectional SEM / EDS reveals oxide-enriched bands at grain boundaries, and oxide inclusions are more prone to coarsening. Their equivalent particle size cannot consistently meet the requirement of ≤0.5 μm for dispersed fineness (resulting in coarse oxide particles / agglomerates >0.5 μm), thus weakening grain boundary bonding and increasing the risk of arcing, particle shedding, and partial discharge during sputtering, leading to unstable film resistivity and TCR. Particle contamination during film deposition is 0.3 particles / cm. 2 .

[0083] Based on the results of the above embodiments and comparative examples, it can be seen that the chromium-silicon target materials prepared by the method of the present invention all satisfy characteristics a~c, and the number of particles can be stably controlled to less than 0.1 particles / cm during thin film deposition. 2 This improves the resistivity and TCR stability of thin films; however, the number of particles in the chromium-silicon target prepared by the comparative method is all less than 0.1 particles / cm². 2 The above-mentioned number of particles is significantly higher than in the example, making it impossible to achieve thin-film resistance and TCR stability.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A chromium-silicon sputtering target, characterized in that, The chromium-silicon target material has a chromium silicide phase as the main phase framework and contains a free silicon phase. The free silicon phase forms a continuously distributed grain boundary network structure along the grain boundaries and / or grain boundary bifurcations of the chromium silicide main phase. The grain boundary network structure includes at least the following features a to c: a. The free silicon phase has a grain boundary coverage of 40-85% in the chromium silicide main phase; b. The maximum cluster size of the free silicon phase is ≤100 μm; c. The particle size of the free silicon phase, D90, is ≤10 μm.

2. The chromium-silicon sputtering target according to claim 1, characterized in that, The free silicon phase accounts for 8-30 vol% of the volume of the chromium-silicon target.

3. The chromium-silicon sputtering target according to claim 1, characterized in that, The mass ratio of chromium to silicon in the chromium-silicon target is 1:1~3.

4. The chromium-silicon sputtering target according to claim 2, characterized in that, The mass ratio of chromium to silicon in the chromium-silicon target is 1:1~3.

5. The chromium-silicon sputtering target according to any one of claims 1 to 4, characterized in that, The chromium-silicon target material also contains a functional element M with a mass fraction of 50-500 ppm. The functional element M is selected from one or more of Ti, Zr, Hf, and Y, and it is dispersed in the form of oxygen-containing compound particles at the grain boundaries and / or grain boundary junctions of the chromium silicide main phase.

6. The chromium-silicon sputtering target according to claim 5, characterized in that, The oxygen-containing compound particles are MO and / or M-Si-O particles, and their equivalent particle size is ≤0.5 μm.

7. The method for preparing the chromium-silicon target material according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Using silicon powder as the core, a chromium shell is formed on the surface of the silicon core by vapor deposition to obtain Si@Cr core-shell precursor powder; (2) The Si@Cr core-shell precursor powder is subjected to cold isostatic pressing, encapsulation vacuum degassing and sealing, hot isostatic pressing and machining in sequence.

8. The method for preparing the chromium-silicon target according to claim 7, characterized in that, The chromium shell has a surface coverage of 70-95% on the silicon core, and its equivalent thickness is 10-300 nm.

9. The method for preparing the chromium-silicon target according to claim 7, characterized in that, Step (1) includes: using a carrier gas to deliver a gaseous chromium source into a deposition zone containing silicon powder, and depositing the gas phase at a temperature of 100~200 ℃ for 10~120 min.

10. The method for preparing the chromium-silicon target according to claim 9, characterized in that, The chromium source includes CrCl3 and / or CrBr3.

11. The method for preparing the chromium-silicon target according to claim 9, characterized in that, The particle size of the silicon powder is 20~100 μm.

12. The method for preparing the chromium-silicon target according to claim 9, characterized in that, The vapor deposition was performed in a reducing atmosphere.

13. The method for preparing the chromium-silicon target according to any one of claims 7 to 12, characterized in that, Before the Si@Cr core-shell precursor powder is subjected to cold isostatic pressing, it is further comprising a step of mixing it with CrSi2 pre-alloy powder containing functional element M, so that the mass ratio of chromium to silicon in the mixed system is 1:1~3 and the mass fraction of functional element M is 50~500 ppm.

14. The method for preparing the chromium-silicon target according to claim 13, characterized in that, The mass fraction of functional element M in the CrSi2 pre-alloyed powder is ≥500 ppm.

15. The method for preparing the chromium-silicon target according to claim 13, characterized in that, The particle size D90 of the CrSi2 pre-alloyed powder is 20~100 μm.

16. The method for preparing the chromium-silicon target according to any one of claims 7 to 12, characterized in that, The hot isostatic pressing is performed in two stages. The parameters for the first stage of hot isostatic pressing include: temperature of 1050~1250 ℃, pressure of 100~200 MPa, and holding time of 1~4 h. The parameters for the second stage of hot isostatic pressing include: temperature of 1420~1470 ℃, pressure of 100~200 MPa, and holding time of 5~20 min.

17. The method for preparing the chromium-silicon target according to claim 16, characterized in that, After hot isostatic pressing, the material is cooled and shaped at a cooling rate of 1~10 °C / min.

18. The use of the chromium-silicon target material according to any one of claims 1 to 6 or the chromium-silicon target material prepared by the preparation method according to any one of claims 7 to 17 in the preparation of chromium-silicon alloy thin films.

Citation Information

Patent Citations

  • Silicon-alloy-containing target material and preparation method thereof

    CN105331939A

  • Chromium-silicon alloy sputtering target and preparation method thereof

    CN111058004A

  • Preparation method of chrome-silicon sputtering target material

    CN111996507A

  • A chromium-silicon alloy sputtering target and its preparation method

    CN113770360B

  • A silicon-chromium rotating sputtering target and its preparation method

    CN113897585B