A method for preparing a graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant and its application.
By constructing a polyphenol functional transition layer on the surface of magnesium-based Prussian white and loading ultrafine Prussian blue nanoparticles, a hierarchical hybrid flame retardant and smoke suppressant is formed, which solves the problems of flammability and toxic smoke release of soft PVC and achieves the synergistic effect of flame retardancy, smoke suppression and toxicity reduction.
Patent Information
- Application Number
- CN202610878299.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-06-17
AI Technical Summary
Existing flexible PVC materials are flammable and release toxic fumes. Traditional flame retardants suffer from resource scarcity, performance degradation, and poor interfacial compatibility, making it difficult to achieve the synergistic integration of multiple flame retardant mechanisms.
By constructing a polyphenol functional transition layer on the surface of sheet-like magnesium-based Prussian white and loading ultrafine Prussian blue analog nanoparticles in situ, a hierarchical magnesium-based Prussian white hybrid flame retardant and smoke suppressant is formed, achieving the synergistic effects of physical barrier, catalytic char formation and catalytic oxidation.
Only 3 to 7 parts of the additive can significantly improve the flame retardant, smoke suppression and toxicity reduction properties of flexible PVC, overcome the agglomeration of nanoparticles, and achieve a synergistic effect of multiple green and safe flame retardant mechanisms.
Smart Images

Figure CN122404802B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame-retardant polymer composite material technology, specifically relating to a method for preparing a graded magnesium-based Prussian white hybrid flame-retardant and smoke-suppressing agent and its application. Background Technology
[0002] Flexible polyvinyl chloride (PVC) boasts excellent processability, good electrical insulation, and low cost, making it widely used in wires and cables, building decoration, and automotive interiors. However, its flexibility relies on a large amount of flammable plasticizers, resulting in highly flammable materials that release large amounts of toxic black smoke and corrosive gases, posing significant fire safety and environmental hazards. Developing novel flame retardants that combine high-efficiency flame retardancy, smoke suppression, and toxicity reduction is an urgent need for the industry.
[0003] Currently, flame retardants for flexible PVC mainly include halogen-antimony synergistic systems, metal hydroxides, and phosphorus-based flame retardants. Halogen-antimony systems offer good flame retardancy, but the raw materials are increasingly constrained by resource scarcity. Metal hydroxides are environmentally friendly, but require a filling rate of over 50 phr to meet flame retardancy requirements, severely degrading the material's mechanical properties and processability. Phosphorus-based flame retardants suffer from insufficient heat resistance, easy migration and precipitation, and poor compatibility with the PVC matrix. Traditional strategies relying on multiple filler formulations often result in compromised performance due to poor interfacial compatibility and dispersion difficulties between different fillers. Therefore, achieving synergistic integration of multiple flame retardant mechanisms at the microstructural level of individual filler particles has become an important development direction in the field of flame-retardant polymer materials.
[0004] Prussian blue analogues (PBAs) are a class of compounds derived from ferricyanide ions ([Fe(CN)6]). 3- Composed of Mg and transition metal ions, PBA nanoparticles can be in situ converted into highly active transition metal oxides during pyrolysis or combustion, exhibiting highly efficient catalytic oxidation capabilities for carbon monoxide and aromatic volatile organic compounds, thus making them a highly promising catalytically active component. However, due to their high surface energy, single PBA nanoparticles are prone to uncontrolled aggregation in the polymer matrix, leading to a sharp reduction in the effective catalytic surface area and hindering the full realization of their nanosize effect and catalytic activity. Magnesium-based Prussian white (Mg-PW) is composed of Mg... 2+ With ferrocyanide ([Fe(CN)6]) 4- It is formed by coordination precipitation, presents a regular sheet-like morphology, has excellent thermal stability, and possesses ideal physical barrier substrate characteristics. However, it has few surface active functional groups and insufficient catalytic oxidation active sites, resulting in limited catalytic elimination ability for toxic gases such as CO.
[0005] An ideal single-component flame retardant and smoke suppressant should integrate a sheet-like physical barrier substrate, catalytically active ultrafine nanoparticles, and an interface layer with both anchoring and compatibility within a single particle. The key technical problem this invention aims to solve is how to construct a hybrid structure with strong interfacial bonding and controllable PBA particle size on the Mg-PW surface using green and mild methods, organically coupling the physical barrier function of the sheet-like substrate with the catalytic char formation and catalytic oxidation functions of the ultrafine PBA nanoparticles, thereby obtaining a single-component hybrid flame retardant and smoke suppressant with multiple flame retardant mechanisms and excellent nanoparticle dispersibility. Summary of the Invention
[0006] To address the aforementioned problems, this invention provides a method for preparing a hierarchical magnesium-based Prussian white hybrid flame retardant and smoke suppressant, as well as its application, to overcome the shortcomings of existing flame retardants such as single function, easy agglomeration of nanoparticles, and reliance on organic solvents or high temperature and pressure in the preparation process, thereby achieving synergistic effects of flame retardancy, smoke suppression, and toxicity reduction.
[0007] The preparation method of the graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant of the present invention includes the following steps:
[0008] Step 1: Disperse the sheet-like magnesium-based Prussian white substrate in a buffer solution containing polyphenols, and form a functional transition layer on its surface through polyphenol self-polymerization to obtain modified magnesium-based Prussian white.
[0009] Step 2: Add the transition metal salt solution to the dispersion of the modified magnesium-based Prussian white and mix to allow the transition metal ions to complex and anchor onto the functional transition layer; then add the ferricyanide salt solution dropwise and co-precipitate in situ at room temperature and atmospheric pressure to load ultrafine Prussian blue analog nanoparticles onto the surface of the functional transition layer, thus obtaining a magnesium-based Prussian white hybrid with a hierarchical composite structure.
[0010] further:
[0011] In step 1, the sheet-like magnesium-based Prussian white substrate is prepared by co-precipitation.
[0012] Specifically, magnesium salts and ferrocyanide salts are added to deionized water, and glycerol and potassium acetate are used as morphology modifiers. The mixture is allowed to stand at 20-25°C for 18-24 hours to obtain sheet-like magnesium-based Prussian white substrate.
[0013] The magnesium salt is one of magnesium acetate, magnesium chloride, or magnesium sulfate, preferably magnesium acetate; the molar ratio of magnesium salt to ferrocyanide is 1:1 to 1.5:1, preferably 1:1; the volume ratio of glycerol to water is 1:1 to 1.5:1, preferably 1:1. The amount of potassium acetate added is 1 to 3 mol / L, based on the total volume of deionized water and glycerol.
[0014] In step 1, the polyphenolic substance is at least one of dopamine hydrochloride, tannic acid, or gallic acid. The mass ratio of the sheet-like magnesium-based Prussian white substrate to the polyphenolic substance is 5:1 to 10:1. The buffer solution is a Tris-HCl buffer solution with pH=8.0.
[0015] In step 1, the self-polymerization reaction is carried out at a temperature of 20–25 °C for 6–36 h. The thickness of the transition functional layer is 10–30 nm. This transition functional layer is rich in phenolic hydroxyl groups and possesses dual complexing and anchoring capabilities for transition metal ions. In subsequent steps, it can effectively control the size of the ultrafine Prussian blue analog nanoparticles and inhibit their aggregation.
[0016] In step 2, the transition metal ion in the transition metal salt is Cu. 2+ Co 2+ Ni 2+ or Fe 2+ One or more of the following are present. The molar ratio of the transition metal ion to the ferricyanide salt is 1:1 to 2:1. The transition metal salt includes one or more of transition metal chlorides, nitrates, and sulfates. The ferricyanide salt is potassium ferricyanide or sodium ferricyanide. The order of addition of the transition metal salt solution and the ferricyanide solution is not interchangeable.
[0017] In step 2, the transition metal salt solution is first added to the dispersion of modified magnesium-based Prussian white, and the mixture is stirred and adsorbed for 15–30 min to allow the metal ions to complex and anchor at the active sites of the functional transition layer. Then, a ferricyanide salt solution is slowly added dropwise. By adjusting the dropping rate (2–7 mL / min), reactant concentration (0.01–0.03 mol / L, where reactant refers to ferricyanide salt), and subsequent stirring time (6–18 h), the particle size of PBAs nanoparticles can be controlled to be 20–150 nm. Controlling the particle size within this range results in a larger contact surface area due to the nano-effect, leading to enhanced catalytic efficiency in subsequent flame retardancy. The loading of PBAs nanoparticles is 10–20 wt%.
[0018] In step 2, during the process of metal ions complexing and anchoring to the active sites of the functional transition layer, sodium citrate can be added to the system. Sodium citrate can form soluble weak coordination complexes with metal ions, slowly releasing free metal ions and preventing rapid aggregation and precipitation. The multi-carboxyl structure optimizes the liquid-phase dispersion environment, facilitating stable coordination of metal ions with the amino and phenolic hydroxyl groups of PDA, thus achieving uniform anchoring of the metal component.
[0019] The preparation method described above is completed entirely in an aqueous system, without the use of any volatile organic solvents, and without the need for heating or pressurization steps.
[0020] The hierarchical structured magnesium-based Prussian white hybrid flame retardant and smoke suppressant of this invention has a three-level composite structure of "sheet-like magnesium-based Prussian white - polyphenol functional transition layer - ultrafine Prussian blue analog nanoparticles". The ultrafine Prussian blue analog nanoparticles are generated by in-situ complexation anchoring-coprecipitation method, with a particle size of 20~150 nm, and are uniformly loaded on the surface of sheet-like substrate.
[0021] This invention relates to the application of a graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant in the preparation of flame retardant and smoke suppressant soft polyvinyl chloride composite materials.
[0022] The raw materials of the flame-retardant and smoke-suppressing soft polyvinyl chloride composite material include, by weight:
[0023] 100 parts PVC resin, 0.5-1 part glyceryl monostearate, 1-3 parts calcium-zinc stabilizer, 30-50 parts dioctyl phthalate plasticizer, and 3-7 parts magnesium-based Prussian white hybrid flame retardant and smoke suppressant.
[0024] Processing technology: Weigh the above components according to the formula, add them to a high-speed mixer and premix at room temperature for 5 min at 800 rpm. Transfer the premix to a two-roll mill (roller temperature 160±5 ℃, roll gap 1 mm) for melt mixing for 8 min until the material is uniformly plasticized. After mixing, cut the sheet and place it in a flat vulcanizing mold, hot press at 160 ℃ and 10 MPa for 5 min, then cold press to set.
[0025] Compared with the prior art, the beneficial effects of the present invention are reflected in:
[0026] (1) By utilizing the dual complexation and anchoring effect of the polyphenol functional transition layer, the ultrafine Prussian blue analog nanoparticles were loaded in situ, uniformly and firmly on the surface of the sheet-like magnesium-based Prussian white, effectively overcoming the problem of nanoparticle aggregation.
[0027] (2) A hierarchical synergistic structure of "physical barrier-catalytic char formation-catalytic oxidation" was constructed: the sheet-like Mg-PW provides a physical barrier and promotes char formation, while the outer ultrafine PBA catalyzes the oxidation of toxic gases and reduces smoke. The two work synergistically to give the polymer composite material excellent flame retardant, smoke suppression and detoxification properties.
[0028] (3) The entire preparation process is carried out in the aqueous phase without the need for volatile organic solvents. The reaction is completed at room temperature and normal pressure, making the process green, safe and controllable.
[0029] (4) Only 3 to 7 parts by weight are needed to simultaneously improve the flame retardant, smoke suppression and toxicity reduction effects in soft PVC. Attached Figure Description
[0030] Figure 1Figure a is a schematic diagram of the synthesis of the hierarchical magnesium-based Prussian white hybrid flame retardant and smoke suppressant of the present invention; Figure b is a comparison of the X-ray diffraction (XRD) patterns of magnesium-based Prussian white (Mg-PW), polydopamine-coated magnesium-based Prussian white (Mg-PW@PDA), hierarchical magnesium-based Prussian white (Mg-PW@PDA@CuFe-PBA) with grown copper-iron Prussian blue nanoparticles, and copper-iron Prussian blue (CuFe-PBA) involved in Examples 1, 2, and 3; Figure c is a comparison of the heat release rate (HRR) curves of polyvinyl chloride and its composites prepared in Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2, and Application Example 1; Figure d is a comparison of the total smoke release curves of polyvinyl chloride and its composites prepared in Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2, and Application Example 1; Figure e is a comparison of the total smoke release of polyvinyl chloride and its composites prepared in Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2, and Application Example 1. A comparison curve of carbon monoxide release rates of the prepared polyvinyl chloride and its composite materials.
[0031] Figure 2a shows a scanning electron microscope (SEM) image of magnesium-based Prussian white (Mg-PW) prepared in Example 1; Figure b shows a SEM image of polydopamine-coated magnesium-based Prussian white (Mg-PW@PDA) prepared in Example 2; Figure c shows a SEM image of a hierarchical hybrid flame retardant and smoke suppressant (Mg-PW@PDA@CuFe-PBA) prepared in Example 3.
[0032] Figure 3 shows a comparison of the Fourier transform infrared (FTIR) spectra of Mg-PW prepared in Example 1, Mg-PW@PDA prepared in Example 2, Mg-PW@PDA@CuFe-PBA prepared in Example 3, and CuFe-PBA prepared alone.
[0033] Figure 4 shows a comparison of the X-ray diffraction (XRD) patterns of Mg-PW prepared in Example 1, Mg-PW@PDA prepared in Example 2, Mg-PW@PDA@CuFe-PBA prepared in Example 3, and CuFe-PBA prepared alone.
[0034] Figure 5a shows the heat release rate (HRR) curves of the polyvinyl chloride composite materials prepared in Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2, and Application Example 1 in cone calorimetry testing; Figure b shows the total heat release (THR) of polyvinyl chloride and its composite materials; Figure c shows the smoke release rate (SPR) of polyvinyl chloride and its composite materials; and Figure d shows the total smoke release (TSP) curve of polyvinyl chloride and its composite materials. These figures demonstrate the excellent flame retardant and smoke suppression effects of the flame retardant and smoke suppressant on the flexible polyvinyl chloride material.
[0035] Figure 6 shows the comparison curves of carbon monoxide release rate (Figure a), carbon dioxide release rate (Figure b), and smoke density test (Figure c) of the materials prepared by Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2, and Application Example 1, demonstrating the excellent smoke and toxicity suppression effect of the flame retardant and smoke suppressant on the flexible polyvinyl chloride material.
[0036] Figure 7 shows the thermogravimetric analysis (TG) curves of polyvinyl chloride and its composites prepared in Comparative Example 1, Comparative Application Example 1, Comparative Application Example 2 and Application Example 1 under nitrogen atmosphere and heating rate of 20 °C / min, reflecting the effect of adding different flame retardants and smoke suppressants on the thermal degradation and char formation behavior of PVC composites.
[0037] Figure 8 The results are presented in TG-FTIR thermogravimetric infrared spectroscopy. Figure a shows a comparison of the absorbance of total volatiles in PVC and PVC / Mg-PW@PDA@CuFe-PBA; Figure b shows a comparison of the absorbance of hydrocarbons in PVC and PVC / Mg-PW@PDA@CuFe-PBA; Figure c shows a comparison of the absorbance of HCl in PVC and PVC / Mg-PW@PDA@CuFe-PBA; and Figure d shows a comparison of the absorbance of HCN release from PVC / Mg-PW and PVC / Mg-PW@PDA@CuFe-PBA. Detailed Implementation
[0038] To better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments and accompanying drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0039] Example 1: Preparation of sheet-like magnesium-based Prussian white substrate (Mg-PW)
[0040] At room temperature, 10.73 g of magnesium acetate (0.05 mol) and 19.63 g of potassium acetate (0.2 mol) were weighed and dissolved in 100 mL of deionized water. 100 mL of glycerol was added, and the solution was stirred until dissolved; this solution is denoted as solution A. 21.12 g of potassium ferrocyanide (K4[Fe(CN)6]·3H2O) (0.05 mol) was weighed and dissolved in 100 mL of deionized water. 100 mL of glycerol was added, and the solution was stirred until dissolved; this solution is denoted as solution B. Under stirring at 25 ℃ and 800 rpm, solution A was rapidly poured into solution B. After stirring for 1–2 min, the mixture was allowed to stand at room temperature and pressure for 24 h. The mixture was then vacuum filtered, thoroughly washed, and vacuum dried at 80 ℃ for 24 h to obtain a white powdery magnesium-based Prussian white substrate, denoted as Mg-PW.
[0041] Example 2: Preparation of sheet-like magnesium-based Prussian white (Mg-PW@PDA) coated with a polyphenol functional transition layer
[0042] 10.0 g of the Mg-PW powder obtained in Example 1 was dispersed in 400 mL of Tris-HCl buffer (pH 8.0), stirred, and sonicated for 10 min to obtain a uniform milky white dispersion. 1.0 g of dopamine hydrochloride (Mg-PW to dopamine hydrochloride mass ratio 10:1) was added at 25 °C, and the mixture was stirred at 400 rpm for 6 h. After the reaction was complete, the mixture was vacuum filtered, washed, and vacuum dried at 80 °C for 12 h to obtain a brownish-gray powder, which is the polydopamine (PDA) functional transition layer-coated sheet-like magnesium-based Prussian white, denoted as Mg-PW@PDA.
[0043] Example 3: Preparation of a hybrid flame retardant and smoke suppressant (Mg-PW@PDA@CuFe-PBA) loaded with copper-iron Prussian blue analogues
[0044] The use of copper-iron Prussian blue (CuFe-PBA) as the outer active nanoparticles is described in detail.
[0045] Step 1: Metal ion pre-complexation
[0046] Take 10.0 g of Mg-PW@PDA powder obtained in Example 2, disperse it in 200 mL of deionized water, stir and sonicate for 20 min to obtain a uniform dispersion C. Then weigh 1.02 g of CuCl2·2H2O (0.006 mol) and 2.21 g of sodium citrate dihydrate (0.0075 mol, sodium citrate to copper salt molar ratio 1.25:1) and dissolve them in 50 mL of deionized water, denoted as solution D. Slowly add solution D to dispersion C, stir at 400 rpm for 30 min, so that Cu... 2+ The phenolic hydroxyl and amino active sites on the surface of the PDA layer are fully coordinated and anchored.
[0047] Step 2: In-situ coprecipitation reaction
[0048] Weigh 1.31 g of K3[Fe(CN)6] (0.004 mol, copper salt to potassium ferricyanide molar ratio 1.5:1) and dissolve it in 50 mL of deionized water, denoted as solution E. Add solution E dropwise to dispersion C (after adding solution D in step 1) at a constant rate of 3 mL / min while stirring at 400 rpm. After the addition is complete, continue stirring at 25 °C for 12 h to allow for sufficient nucleation and maturation of CuFe-PBA nanoparticles.
[0049] Step 3: Post-processing
[0050] After the reaction was completed, the mixture was vacuum filtered, and the filter cake was washed with deionized water until the filtrate was colorless and neutral. The mixture was then vacuum dried at 80 °C for 12 h to obtain a magnesium-based Prussian white hybrid flame retardant and smoke suppressant with a hierarchical composite structure, denoted as Mg-PW@PDA@CuFe-PBA.
[0051] Preparation of CuFe-PBA:
[0052] Weigh 1.02 g of CuCl2·2H2O (0.006 mol) and 2.21 g of sodium citrate dihydrate (0.0075 mol, molar ratio of sodium citrate to copper salt 1.25:1) and dissolve them in 250 mL of deionized water. Stir and sonicate for 20 min until fully dissolved, and record this as solution A. Then weigh 1.31 g of K3[Fe(CN)6] (0.004 mol, molar ratio of copper salt to potassium ferricyanide 1.5:1) and dissolve it in 50 mL of deionized water until fully dissolved, and record this as solution B. Add solution B dropwise to solution A at a constant rate of 3 mL / min while stirring at 400 rpm. After the addition is complete, continue stirring at 25 °C for 12 h. After the reaction is complete, wash, centrifuge, dry, and collect the powder. The yield, calculated based on the mass of potassium ferricyanide, is approximately 87%.
[0053] Product characterization:
[0054] SEM observation (Figure 2) showed that the Mg-PW prepared in Example 1 was a regular square sheet with a lateral size of 3~5μm; the Mg-PW@PDA@CuFe-PBA prepared in Example 3 retained the sheet-like substrate structure, and its surface was uniformly and densely covered by a large number of CuFe-PBA nanoparticles.
[0055] FTIR analysis ( Figure 3 Compared to Mg-PW@PDA, Mg-PW@PDA@CuFe-PBA exhibits better performance at 2060 cm⁻¹. -1The enhanced absorption peak of C≡N stretching vibration at the point indicates that CuFe-PBA was successfully loaded onto the surface of the functional transition layer.
[0056] XRD analysis ( Figure 4 The product exhibited characteristic CuFe-PBA diffraction peaks at 2θ = 17.7°, 24.8°, 35.8°, and 40.1°, with sharp peak shapes, indicating good crystallinity.
[0057] Example 4: Preparation of a hybrid flame retardant and smoke suppressant (Mg-PW@PDA@CoFe-PBA) loaded with a cobalt-iron Prussian blue analogue
[0058] In Example 3, step 1, the 1.02 g CuCl2·2H2O (0.006 mol) in solution D was replaced with 1.42 g CoCl2·6H2O (0.006 mol), while all other steps remained the same. The conditions and operations in subsequent steps 2 and 3 were exactly the same as in Example 3, yielding Mg-PW@PDA@CoFe-PBA.
[0059] Example 5: Preparation of a hybrid flame retardant and smoke suppressant (Mg-PW@PDA@NiFe-PBA) loaded with a nickel-iron Prussian blue analogue
[0060] In Example 3, step 1, 1.02 g CuCl2·2H2O (0.006 mol) in solution D was replaced with 1.43 g NiCl2·6H2O (0.006 mol), while all other steps remained the same. The conditions and operations for subsequent steps 2 and 3 were exactly the same as in Example 3, yielding Mg-PW@PDA@NiFe-PBA.
[0061] Example 6: Preparation of a hybrid flame retardant and smoke suppressant (Mg-PW@PDA@FeFe-PBA) loaded with iron-iron Prussian blue analogues
[0062] In Example 3, step 1, the 1.02 g CuCl2·2H2O (0.006 mol) in solution D was replaced with 1.67 g FeSO4·7H2O (0.006 mol) (the solution must be freshly prepared and a trace amount of ascorbic acid should be added to prevent oxidation; operation should be carried out in the dark). All other steps remained the same. The conditions and operations of subsequent steps 2 and 3 were exactly the same as in Example 3, yielding a dark blue powder product, denoted as Mg-PW@PDA@FeFe-PBA.
[0063] Application Examples and Comparative Application Examples: Preparation and Performance Testing of Flame-Retardant and Smoke-Suppressing Flexible PVC Composite Materials
[0064] To systematically evaluate the application effect of the hybrid flame retardant and smoke suppressant of the present invention, a series of polyvinyl chloride composite material samples were prepared according to a unified soft PVC basic formula and processing technology.
[0065] Basic formulation (by weight): 100 parts PVC resin (SG-5 type, degree of polymerization 1000), 2 parts calcium-zinc stabilizer, 0.5 parts glyceryl monostearate, and 40 parts dioctyl phthalate (DOP, industrial grade) plasticizer. Then, 5 parts by weight of different fillers are added to each of these components.
[0066] Processing technology: Weigh the above components according to the formula and add them to a high-speed mixer for premixing at 800 rpm at room temperature for 5 min. Transfer the premix to a two-roll mill (roller temperature 160±5 ℃, roll gap 1 mm) for melt mixing for 8 min until the material is uniformly plasticized. After mixing, cut the sheet and place it in a flat vulcanizing mold. Hot press at 160 ℃ and 10 MPa for 5 min, followed by cold pressing for 3 min to set the shape. Cut the strips to obtain standard test strips with thicknesses of 1 mm and 3 mm.
[0067] Comparative Example 1 (blank control, pure PVC): prepared according to the basic formula without any flame retardant fillers.
[0068] Comparative Application Example 1 (PVC / Mg-PW): 5 parts of Mg-PW synthesized in Example 1 were added to the basic formulation.
[0069] Comparative Application Example 2 (PVC / Mg-PW@PDA): 5 parts of Mg-PW@PDA synthesized in Example 2 were added to the basic formulation.
[0070] Application Example 1 (PVC / Mg-PW@PDA@CuFe-PBA): Add 5 parts of the hybrid flame retardant and smoke suppressant synthesized in Example 3 to the basic formulation.
[0071] Application Example 2 (PVC / Mg-PW@PDA@CoFe-PBA): Add 5 parts of the hybrid flame retardant and smoke suppressant synthesized in Example 4 to the basic formulation.
[0072] Application Example 3 (PVC / Mg-PW@PDA@NiFe-PBA): Add 5 parts of the hybrid flame retardant and smoke suppressant synthesized in Example 5 to the basic formulation.
[0073] Application Example 4 (PVC / Mg-PW@PDA@FeFe-PBA): Add 5 parts of the hybrid flame retardant and smoke suppressant synthesized in Example 6 to the basic formulation.
[0074] The test method for flame retardant and smoke suppression performance is as follows:
[0075] The limiting oxygen index (LOI) test was conducted in accordance with the GB / T 2406.2-2023 standard, and the sample size was 100 mm × 80 mm × 3 mm.
[0076] Cone calorimetry (CONE) testing was conducted according to ISO 5660-1:2015 standard, with a radiation intensity of 35 kW / m². 2 The sample size was 100 mm × 100 mm × 3 mm, and data such as heat release rate (HRR) and total heat release (THR) were recorded.
[0077] Smoke density (DS) testing was conducted according to GB / T 8323.2-2008 standard, using flameless radiation mode, with a radiation intensity of 25 kW / m². 2 The sample size was 75 mm × 75 mm × 1 mm, and the maximum smoke density (Ds,max) was recorded.
[0078] The flame retardant and smoke suppression performance data of the flexible PVC composite materials in each embodiment and comparative example were obtained by testing the performance of each sample using the above standard methods. The results are summarized in Table 1.
[0079]
[0080] Note: LOI represents the limiting oxygen index value. Cone calorimetry results: peak heat release rate (PHRR), total smoke release (TSP), and peak carbon monoxide release rate (PCOP).
[0081] As shown in Table 1, compared with Application Example 1, Comparative Example 1 (pure PVC) has an LOI of only 23.7% and a PHRR as high as 298.1 kW / m². 2 This indicates that the material is highly flammable and exhibits a rapid heat release. While the addition of unmodified Mg-PW (comparative Application Example 1) showed some improvement, the effect was limited. However, after using the Mg-PW@PDA@CuFe-PBA hybrid flame retardant and smoke suppressant from Example 1 of this invention, only 5 parts were added, and the LOI of the material increased from 23.7% to 28.2%, an increase of 19.0%; the peak heat release rate (PHRR) increased from 298.1 kW / m³. 2 Significantly reduced to 186.6 kW / m 2 The decrease was as high as 37.4%; total smoke emissions (TSP) decreased from 20.9 m³ / s. 2 Descended to 9.9 m 2Simultaneously, the peak carbon monoxide release (PCOP) decreased from 0.0160 g / s to 0.0127 g / s. This fully demonstrates that the hierarchical hybrid flame retardant and smoke suppressant of the present invention achieves simultaneous and efficient improvement in flame retardant, smoke suppressant, and toxicity reduction performance through the synergistic effect of physical barrier and catalytic oxidation. In application examples 2-4, different PBA components also exhibited comprehensive and excellent overall performance, confirming the universality of the technical solution of the present invention.
[0082] In addition, the present invention also conducted tests using a TG-FTIR coupled system, under the following specific conditions: Thermogravimetric (TG) conditions: nitrogen atmosphere, heating rate 20 °C / min, temperature range 30–800 °C, sample mass 5–10 mg, carrier gas flow rate 50 mL / min; Fourier transform infrared (FTIR) spectroscopy conditions: scanning range 4000–400 cm⁻¹ -1 The scanning interval is 10 s, and the temperature of the transmission line and gas pool is maintained at 200 ℃ to prevent gas condensation.
[0083] All samples used a uniform PVC base formulation (100 parts PVC + 5 parts corresponding filler), and the test results are shown below. Pure PVC resin and its additives do not contain cyano (-CN) structures; therefore, the integrated area of its HCN characteristic peak is merely background signal, with no substantial HCN formation. The only source of HCN in this system is the cyano coordination framework of the Prussian blue flame retardant itself, a common industry issue for this type of functional material. For comparison, the HCN of PVC / Mg-PW was compared with that of PVC / Mg-PW@PDA@CuFe-PBA to explain the catalytic and absorption effects of the graded hybrid flame retardant on HCN, thereby reducing the release of toxic gases.
[0084] The results of the gas release behavior analysis based on TG-FTIR are as follows:
[0085] (1) Total pyrolysis volatile gas release is significantly reduced
[0086] The TG-FTIR total volatile concentration comparison chart shows ( Figure 8 (Figure a) Pure PVC exhibits a strong volatile matter release peak at 250–350℃, corresponding to the deHCl removal reaction; a second release peak appears at 400–550℃, corresponding to the cracking and carbonization of conjugated polyenes. After adding Mg-PW@PDA@CuFe-PBA, the total volatile matter release significantly decreased, demonstrating that the tertiary composite structure of this application effectively inhibits the pyrolysis process of PVC and promotes the conversion of more carbon elements into the condensed phase carbon layer, rather than volatilizing into the gas phase.
[0087] (2) The release of corrosive hydrogen chloride (HCl) is significantly reduced.
[0088] like Figure 8 As shown in Figure c, the HCl volatile concentrations measured by TG-FTIR show a significant reduction in HCl release after the addition of Mg-PW@PDA@CuFe-PBA. HCl is the main corrosive gas released during PVC combustion, causing serious damage to equipment and the environment. Furthermore, it catalyzes the Mg-PW-based flame retardant of this application, significantly reducing the total HCl release. This is because the metal oxides produced by the pyrolysis of Mg-PW can react with HCl, consuming it at the source and simultaneously inhibiting the chain decomposition of PVC, achieving a synergistic effect of acid absorption and flame retardancy.
[0089] (3) The release of highly toxic hydrogen cyanide (HCN) was effectively controlled.
[0090] The characteristic absorption peak of HCN is located at 722 cm⁻¹. -1 , Figure 8 The middle d-figure shows the TG-FTIR test results:
[0091] The sample with added unmodified pure Mg-PW showed a characteristic HCN peak, but the overall release was very low. However, this indicates a high risk of HCN release after the high-temperature cyano skeleton of the unmodified Mg-based Prussian white fractures. The sample with added the graded flame retardant (Mg-PW@PDA@CuFe-PBA) of this application showed a decrease in the intensity of the HCN characteristic peak, indicating a reduction in the total release. This result fully demonstrates that the three-level graded structure of this application effectively mitigates the safety hazard of HCN release from cyanide-containing flame retardants.
[0092] (4) Hydrocarbon release decreased synchronously.
[0093] Hydrocarbons are a significant factor contributing to asphyxiation and the spread of fire in fires, but the total release of hydrocarbons is significantly lower compared to pure PVC. Figure 8 (Figure b in the middle)
[0094] Elucidation of the mechanisms of toxicity reduction and smoke suppression:
[0095] This application's hierarchical hybrid flame retardant can simultaneously inhibit the release of multiple toxic and corrosive gases. It is based on a synergistic mechanism of "physical barrier adsorption - chemical neutralization - catalytic conversion," with each mechanism working together to cover the entire chain of gas generation, release, and diffusion.
[0096] (1) The physical barrier effect of the dense carbon layer (all-gas suppression)
[0097] During combustion, the Mg-PW sheet substrate provides a rigid framework, the polyphenol layer pyrolyzes to form an organic carbon film, and the metal oxides generated from the decomposition of CuFe-PBA nanoparticles fill the pores of the carbon layer. Together, these three elements form a continuous, dense, and crack-free composite carbon layer. This carbon layer not only isolates oxygen and heat, inhibiting the pyrolysis of PVC, but also acts as a physical barrier, adsorbing and encapsulating undecomposed cyanide compounds, HCl, hydrocarbons, etc., within the condensed phase, preventing their release into the gas phase and allowing reaction time for subsequent chemical neutralization and catalytic conversion.
[0098] (2) Chemical fixation and neutralization of metal ions (specific inhibition of HCN and HCl)
[0099] HCN fixation: At high temperatures, the cyano skeletons of Mg-PW and CuFe-PBA break down, releasing free CN. - Mg in the system 2+ Fe 2+ / Fe 3+ Cu 2+ Plasma can be used with CN - A coordination reaction occurs, generating highly thermally stable metal cyanides. These metal cyanides are difficult to decompose again at fire temperatures, thus permanently fixing the cyano groups in the condensed phase carbon layer, preventing HCN formation at the source. HCl neutralization: The metal oxides produced by the pyrolysis of Mg-PW can react with the HCl released from PVC, eliminating the corrosiveness of HCl and inhibiting its catalytic effect on PVC decomposition.
[0100] (3) Catalytic conversion of transition metal oxides (general inhibition of CO, HCN and hydrocarbons)
[0101] The CuO and Fe3O4 bimetallic oxides generated by the pyrolysis of CuFe-PBA nanoparticles exhibit excellent catalytic oxidation activity: they catalyze the oxidation of CO to CO2, the oxidation of trace amounts of HCN to non-toxic products, and the cross-linking of hydrocarbons into carbon, reducing their volatilization and release.
[0102] In summary, the pyrolysis gas release behavior of the flame retardant in this application has been fully verified using the TG-FTIR standard test method. The test results show that:
[0103] Unmodified pure Mg-PW poses a certain risk of HCN release. This application reduces the total HCN release by constructing a three-level graded composite structure, effectively solving the common safety hazards of cyanide-containing flame retardants.
[0104] This application also significantly reduces the release of various toxic and corrosive gases such as HCl, CO, and hydrocarbons, thus comprehensively improving the fire safety of the material.
[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant, characterized in that... Includes the following steps: Step 1: Disperse the sheet-like magnesium-based Prussian white substrate in a buffer solution containing polyphenols, and form a functional transition layer on its surface through polyphenol self-polymerization to obtain modified magnesium-based Prussian white. Step 2: Add the transition metal salt solution to the dispersion of the modified magnesium-based Prussian white and mix to allow the transition metal ions to complex and anchor onto the functional transition layer; then add the ferricyanide salt solution dropwise and co-precipitate in situ at room temperature and atmospheric pressure to load ultrafine Prussian blue analog nanoparticles onto the surface of the functional transition layer to obtain a magnesium-based Prussian white hybrid with a hierarchical composite structure. In step 1, the sheet-like magnesium-based Prussian white substrate is prepared by a co-precipitation method, specifically including the following steps: Magnesium salt and ferrocyanide salt were added to deionized water, and glycerol and potassium acetate were used as morphology modifiers. The mixture was allowed to stand at 20-25°C for 18-24 h to obtain sheet-like magnesium-based Prussian white substrate. In step 1, the polyphenolic substance is at least one of dopamine hydrochloride, tannic acid, or gallic acid; In step 2, the transition metal ion in the transition metal salt is Cu. 2+ Co 2+ Ni 2+ or Fe 2+ One or more of the following, wherein the types of transition metal salts include one or more of transition metal chlorides, nitrates, and sulfates.
2. The preparation method according to claim 1, characterized in that: The volume ratio of glycerol to water is 1:1 to 1.5:1; the amount of potassium acetate added is 1 to 3 mol / L, based on the total volume of deionized water and glycerol.
3. The preparation method according to claim 1, characterized in that: In step 1, the mass ratio of the sheet-like magnesium-based Prussian white substrate to the polyphenolic substance is 5:1 to 10:
1.
4. The preparation method according to claim 1, characterized in that: In step 1, the reaction temperature of the self-polymerization reaction is 20~25℃, and the reaction time is 6~36 h.
5. The preparation method according to claim 1, characterized in that: In step 2, the particle size of the Prussian blue analog nanoparticles is 20~150 nm.
6. The preparation method according to claim 1, characterized in that: In step 2, the loading amount of the Prussian blue analog nanoparticles is 10~20 wt%.
7. A graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant, prepared by the method according to any one of claims 1-6.
8. The application of the hierarchical magnesium-based Prussian white hybrid flame retardant and smoke suppressant according to claim 7 in the preparation of flame retardant and smoke suppressant soft polyvinyl chloride composite materials, characterized in that: The amount of the graded magnesium-based Prussian white hybrid flame retardant and smoke suppressant added is 3 to 7 parts by weight, based on 100 parts of PVC resin.