TiAl alloy target material, preparation method thereof and application thereof

By combining TiAl alloy preforms with powder through sintering, the problems of density and impurity control in large-size TiAl alloy targets were solved, resulting in targets with high density, low porosity, and low inclusions, which improved sputtering stability and film consistency.

CN122687139BActive Publication Date: 2026-11-10GRIKIN ADVANCED MATERIALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611187139.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-10
Estimated Expiration
2046-08-06

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously achieve high density, low porosity, low inclusions, and uniform microstructure in large-size TiAl alloy sputtering targets, resulting in a high risk of abnormal discharge and particle defects during sputtering.

Method used

A method of co-sintering at least two TiAl alloy preforms with TiAl alloy powder is adopted. Through the plastic flow and diffusion sintering of TiAl alloy powder, a metallurgical diffusion bond is formed to form a connecting matrix, which reduces the risk of introducing oxygen, carbon and foreign metal impurities, and improves density and microstructure uniformity.

Benefits of technology

This study achieved high density (≥99%), low oxygen and low carbon content (≤1000 ppm and 100 ppm) in large-size TiAl alloy targets, reducing the risk of discharge anomalies and particle defects, and improving sputtering stability and film consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122687139B_ABST
    Figure CN122687139B_ABST
Patent Text Reader

Abstract

The application provides a TiAl alloy target material and a preparation method and application thereof, and relates to the technical field of TiAl alloy target materials. The TiAl alloy target material is a target body formed by co-sintering at least two TiAl alloy preforms and TiAl alloy powder, the TiAl alloy preforms are formed by cutting TiAl alloy ingots, and the TiAl alloy target material comprises the following characteristics of a and b: a, relative density is greater than or equal to 99%; b, oxygen content is less than or equal to 1000 ppm, and carbon content is less than or equal to 100 ppm. The TiAl alloy target material takes the TiAl alloy preform as a low-inclusion dense skeleton, and takes the TiAl alloy powder as a gap-filling and diffusion bridging phase, so that the powder-related inclusion risk is reduced. The TiAl alloy target material meets the requirements of high density, low porosity, low inclusion and consistent organization composition, solves the problem that large-size target materials and low inclusion cannot be simultaneously considered, and improves sputtering stability and film consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of TiAl alloy target technology, and in particular to a TiAl alloy target, its preparation method and application. Background Technology

[0002] TiAl alloys have potential applications in electronic devices and functional thin films. By adjusting the Al content in the alloy, the work function properties of nitride thin films can be controlled. At the same time, TiAl alloys also have engineering value in terms of thermal stability, environmental resistance, and interfacial interdiffusion suppression. Therefore, they are considered as one of the candidate sputtering target systems for applications such as metal gates, diffusion barrier layers, and wear-resistant and corrosion-resistant coatings.

[0003] However, the industrial application of sputtering targets places more stringent requirements on the quality of the target blank. Especially under large-size conditions (e.g., planar targets with a diameter of 300 mm or more, or even larger sizes), the target material usually needs to simultaneously meet the requirements of high density, low porosity, low inclusions and low impurities (e.g., oxygen, carbon, and foreign metal impurities), as well as consistency in microstructure and composition, in order to avoid problems such as particle sources, arcing or micro-arcs, and partial discharge during sputtering, which can lead to process instability and thin film defects. From a physical mechanism perspective, factors such as internal pores or micropores in the target material, non-metallic inclusions, insulating phases or oxides on the surface or in the bulk, and gas retention can all induce arcing and particle defects; insufficient densification or the presence of micropores in powder metallurgy targets can also lead to gas release and micro-arc phenomena.

[0004] There are two main approaches to the preparation of TiAl alloy targets. One is the smelting and casting (or smelting, ingot making, and subsequent densification) route. This route usually has the advantage of introducing relatively few impurities. However, when the target size is significantly increased, the TiAl intermetallic compound system is brittle and experiences high thermal stress during solidification and cooling, which easily leads to problems such as shrinkage cavities, elemental segregation, cracking, and edge chipping. It is difficult to stably obtain large-sized target billets with a diameter of 300 mm or more, and the yield is low.

[0005] The second route is powder metallurgy, which includes pressure-assisted sintering processes such as cold isostatic pressing, encapsulation and degassing, packaging, hot isostatic pressing, and vacuum hot pressing. This route is suitable for preparing large-size TiAl alloy targets and can achieve the advantage of high density. Hot isostatic pressing (HIP) usually requires high temperature and isostatic densification within an airtight enclosure or mold to reduce porosity and improve reliability. However, in active metal systems such as Ti and Al, the powder has a large specific surface area, many interfaces, and a long process chain. Processes such as powder mixing or ball milling, loading, degassing, sintering, and tooling contact can easily introduce oxygen, carbon, and foreign metal impurities. Furthermore, the densification inside large-size target blanks may be asynchronous, and problems such as residual porosity, uneven microstructure, and insufficient interface reliability will further amplify the risks of arc light and particles during sputtering.

[0006] For example, existing technologies have routes for densifying TiAl targets through pre-degassing and HIP (such as CN113981388A, CN112725658B, etc.), which can obtain targets with relatively high density. However, such solutions still face the challenge of simultaneously achieving large size and low impurity: if relying entirely on powder metallurgy, the amount of powder used is large, and the pressure on impurity control and batch consistency increases; if relying entirely on integral melting to prepare large-size ingots, it is difficult to guarantee defect control and yield during the size scaling process.

[0007] In view of this, the present invention is hereby proposed. Summary of the Invention

[0008] This invention provides a TiAl alloy target material, its preparation method, and its application, achieving manufacturability of large-size target blanks, low impurity and high density, effectively reducing the oxygen and carbon content in TiAl alloy targets and the risk of target cracking, and solving the problem of difficulty in achieving both large size and low impurity.

[0009] In a first aspect, the present invention provides a TiAl alloy target, wherein the TiAl alloy target is a target formed by sintering at least two TiAl alloy preforms and TiAl alloy powder together, wherein the TiAl alloy preforms are formed by cutting TiAl alloy ingots, and the TiAl alloy target includes the following features a and b: a. The relative density of the TiAl alloy target is ≥99%; b. The oxygen content of the TiAl alloy target is ≤1000 ppm and the carbon content is ≤100 ppm.

[0010] The TiAl alloy target of the present invention is a target formed by sintering at least two TiAl alloy preforms and TiAl alloy powder together. During the sintering process, the TiAl alloy powder undergoes plastic flow and diffusion sintering and closes the pores, forming a metallurgical diffusion bond between the TiAl alloy preform, the TiAl alloy powder matrix and the TiAl alloy preform, thus forming a connecting matrix and realizing diffusion bridging.

[0011] TiAl alloy preforms are formed by cutting TiAl alloy ingots. Their specific surface area is lower than that of TiAl alloy powder, resulting in a relatively lower risk of introducing oxygen, carbon, and foreign metal impurities. Using TiAl alloy preforms as one of the sintering raw materials not only reduces the amount of TiAl alloy powder used, thus lowering the risk of oxygen, carbon, and impurity introduction from the source (oxygen and carbon contents can be controlled below 1000 ppm and 100 ppm, respectively), but also achieves a relative density of over 99% for the TiAl alloy target. This meets the requirements of high density, low porosity, low impurity introduction, and consistent microstructure and composition, solving the problem of simultaneously achieving large-size targets and low impurity introduction. This helps reduce the risk of abnormal discharge and particle defects, thereby improving sputtering stability and film consistency.

[0012] Preferably, the oxygen content is ≤500 ppm and the carbon content is ≤50 ppm.

[0013] Furthermore, the particle size D90 of the TiAl alloy powder is within 100 μm; the atomic ratio of Ti to Al in the TiAl alloy preform and the TiAl alloy powder are independently (20:80) to (80:20).

[0014] Preferably, the atomic ratio of Ti to Al is (40:60) to (60:40).

[0015] Preferably, the TiAl alloy powder has a purity ≥4N and a particle size of 10–100 μm.

[0016] Furthermore, the TiAl alloy preform is disc-shaped with a diameter of 10–120 mm and a thickness of 2–20 mm.

[0017] If the diameter or thickness of the TiAl alloy preform is too small, the number of preforms required to prepare a target blank of the same size will increase. The cutting surface of the TiAl alloy preform, the interface between it and the TiAl alloy powder, and the proportion of the TiAl alloy powder filling area will increase, which will increase the risk of introducing impurities such as oxygen. At the same time, too many interfaces are not conducive to the full closure of pores and the homogenization of the microstructure during sintering, and will reduce the density.

[0018] If the diameter or thickness of the TiAl alloy preform is too large, it is more prone to defects such as shrinkage cavities, segregation, cracks, or edge chipping during ingot preparation, cutting, and filling. At the same time, an excessively large TiAl alloy preform will reduce the continuity of the TiAl alloy powder interstitial area, resulting in insufficient pressure transmission and interfacial diffusion during sintering. This can easily lead to the formation of unbonded areas, residual pores, or weak interfaces, thereby reducing the density and microstructure uniformity of the target material and affecting the yield.

[0019] Therefore, controlling the diameter of the TiAl alloy preform to 10–120 mm and the thickness to 2–20 mm can reduce the risk of impurity introduction and ensure high density, which helps to improve the microstructure uniformity of the TiAl alloy target, reduce porosity and cracking risk, and increase the yield of large-size target preparation.

[0020] Preferably, the diameter of the TiAl alloy preform is 20–80 mm and the thickness is 3–10 mm.

[0021] Furthermore, the TiAl alloy target material also includes at least one of the following characteristics: c. Diameter 300–600 mm, thickness 5–25 mm; d. Surface roughness Ra≤0.4 μm; e. Flatness ≤ 0.05 mm.

[0022] A second aspect of the present invention provides a method for preparing the above-mentioned TiAl alloy target, comprising the following steps: (1) Cut the TiAl alloy ingot into TiAl alloy preforms; (2) At least two of the TiAl alloy preforms are loaded into a sleeve, and TiAl alloy powder is filled between adjacent TiAl alloy preforms and between the TiAl alloy preforms and the sleeve to obtain a loading system; (3) The charging system is degassed and then sintered to obtain a target blank; (4) Post-process the target blank.

[0023] This invention first prepares small-sized TiAl alloy ingots, cuts them into multiple TiAl alloy preforms, and then fills the gaps between the preforms with TiAl alloy powder before integral sintering. Using TiAl alloy preforms as a low-impurity, dense framework and TiAl alloy powder as interstitial filler and diffusion bridging phase significantly reduces the amount of TiAl alloy powder used. This avoids the problems of shrinkage cavities, segregation, cracking, and low yield that are easily generated in the large-sized TiAl ingot melting process, and also reduces the risk of introducing impurities such as oxygen and carbon in the all-powder sintering process. It improves the internal microstructure uniformity and interface reliability of large-sized target blanks, thereby achieving low-impurity, high-density, and high-yield preparation of large-sized TiAl alloy targets. This helps reduce the risk of edge chipping, cracking, and abnormal discharge, and improves the operational stability of high-power sputtering. The specific principle is as follows: During the sintering process, TiAl alloy powder undergoes plastic flow and diffusion sintering under high temperature and high pressure conditions, forming metallurgical diffusion bonding and closing pores between TiAl alloy preforms, TiAl alloy powder matrix and TiAl alloy preforms, forming a connecting matrix located between adjacent TiAl alloy preforms and / or around individual TiAl alloy preforms.

[0024] This connecting substrate enables diffusion bridging between each TiAl alloy preform and the TiAl alloy powder, achieving metallurgical bonding between each TiAl alloy preform and the TiAl alloy powder, as well as between adjacent TiAl alloy preforms, forming an integral target blank. This effectively improves the stability and density of the microstructure, reduces the risk of introducing oxygen, carbon, and foreign metal impurities, and increases porosity, thereby improving the yield of the target material. The prepared TiAl alloy target material simultaneously meets the requirements of high density, low porosity, low inclusions, and consistent microstructure composition, solving the problem of simultaneously achieving large-size target material and low impurity. It effectively reduces the risk of discharge anomalies and particle defects, and improves sputtering stability and film consistency.

[0025] Preferably, in step (2), after the TiAl alloy powder is filled, it can be subjected to vibration compaction, pre-compaction or cold isostatic pressing to improve the filling uniformity and initial density.

[0026] Furthermore, the total volume of the TiAl alloy preform accounts for 35% to 90% of the volume of the cladding. Preferably, it is 50% to 80%.

[0027] Accordingly, the volume fraction of the TiAl alloy powder in the casing is 10% to 65%; preferably 20% to 50%.

[0028] In the preparation of the TiAl alloy target of the present invention, the TiAl alloy preform is used as the main volume unit, and the TiAl alloy powder mainly undertakes the functions of filling gaps and diffusion bridging. By controlling the volume fraction of the TiAl alloy preform in the cladding volume within the above-mentioned range, the amount of TiAl alloy powder used can be significantly reduced, thereby reducing the risk of foreign impurities introduced by oxygen, carbon and tooling wear from the source, enhancing the overall integrity of large-size targets, and improving the sputtering stability and film consistency of the target.

[0029] Preferably, the number of TiAl alloy preforms is 10 to 120.

[0030] Furthermore, the width of the gap is 0.2 to 10 mm.

[0031] Preferably, the width of the gap is 0.5 to 5 mm.

[0032] Controlling the width of the gap within the aforementioned range facilitates the full filling of TiAl alloy powder between adjacent TiAl alloy preforms and between the TiAl alloy preform and the cladding, forming a diffusion region during subsequent sintering. If the gap is too small, the TiAl alloy powder will not easily enter the gap uniformly, easily resulting in local unfilled areas or residual pores, leading to insufficient interfacial bonding. If the gap is too large, the amount of TiAl alloy powder used will increase, increasing the specific surface area of ​​the powder and raising the risk of inclusions of impurities such as oxygen and carbon. At the same time, large volume fraction powder areas are prone to uneven densification and microstructure differences during sintering.

[0033] Therefore, controlling the gap width to 0.2–10 mm can take into account the requirements of powder filling uniformity, sufficient interfacial diffusion and bonding and low impurity introduction, thereby helping to improve the density and microstructure uniformity of the target material, reduce porosity and inclusion risk, and improve the yield.

[0034] Furthermore, the TiAl alloy preform is arranged within the casing in at least one of the following ways: single-layer flat laying, multi-layer stacking, or staggered arrangement of adjacent layers.

[0035] Preferably, the adjacent layers are arranged in a staggered manner so that the projected positions of the adjacent TiAl alloy preforms do not completely overlap, in order to avoid the formation of a continuous weak interface that runs through the thickness direction. During sintering, this helps to improve the metallurgical diffusion bonding effect between the TiAl alloy preform, the TiAl alloy powder matrix and the TiAl alloy preform, reduce unbonded pores and through cracks, increase the density of the target material, reduce porosity and reduce the risk of impurity introduction.

[0036] Furthermore, the diameter of the TiAl alloy ingot is 20–120 mm.

[0037] Preferably, the diameter of the TiAl alloy ingot is 30–80 mm.

[0038] Preferably, the sintering is carried out by hot isostatic pressing, and the parameters of the hot isostatic pressing include: temperature of 900-1300 °C, pressure of 80-180 MPa, and time of 2-6 h.

[0039] More preferably, the temperature of the hot isostatic pressing is 1000–1200 °C and the pressure is 100–150 MPa.

[0040] Preferably, the sintering is performed using vacuum hot pressing, and the parameters of the vacuum hot pressing include: vacuum degree ≤ 10. -2 Pa, temperature 900–1200 ℃, pressure 20–50 MPa, time 2–6 h.

[0041] Preferably, the temperature of the vacuum hot pressing is 1000-1100 °C and the pressure is 25-35 MPa.

[0042] In the above technical solutions, controlling the parameters of hot isostatic pressing or vacuum hot pressing within the aforementioned range allows TiAl alloy powder to undergo particle rearrangement, local deformation, and diffusion bonding under high temperature and pressure. This promotes interfacial bonding and pore closure between the TiAl alloy preform and the TiAl alloy powder, thereby improving the density and microstructure uniformity of the target blank. If the sintering temperature, pressure, or holding time is too low, powder sintering and interfacial diffusion bonding will be insufficient, easily leaving unbonded areas and pores. If the sintering temperature, pressure, or holding time is too high, it may lead to grain coarsening, local component segregation, cladding or target blank deformation, and thermal stress defects, affecting the target material yield and microstructure uniformity. Simultaneously, controlling the vacuum level during vacuum hot pressing helps reduce the formation of pores or oxide inclusions by residual and adsorbed gases during sintering.

[0043] Furthermore, the degassing parameters include: a temperature of 300–600 °C and a vacuum degree ≤10. -2 Pa, heat preservation time is 1 to 4 hours.

[0044] Preferably, the degassing temperature is 400–550 °C and the vacuum degree is ≤5 × 10⁻⁶. -3 Pa, heat preservation time is 2-3 hours.

[0045] By controlling the degassing parameters within the above-mentioned range, this invention can effectively reduce the risk of residual pores formed by adsorbed gases on the powder surface during subsequent pressure sintering, thereby reducing the porosity and carbon and oxygen content of the TiAl alloy target and improving the sputtering performance of the TiAl alloy target.

[0046] Furthermore, after degassing is completed, the process also includes a step of encapsulating the package; the encapsulation step can be used to reduce the risk of residual pores formed by the gas adsorbed on the powder surface during subsequent pressure sintering.

[0047] Preferably, the encapsulation is performed under vacuum sealing or in a high-purity inert atmosphere.

[0048] Furthermore, after sealing, helium leak testing is performed, and the leakage rate is ≤1×10⁻⁶. -8 Pa·m 3 / s.

[0049] Furthermore, the post-processing includes machining and / or annealing steps.

[0050] Furthermore, the machining steps include: first removing the casing, then performing turning, end face grinding, and polishing on the target blank after casing removal to obtain a planar target material of the target size; if necessary, annealing can be performed to release residual stress, and the annealing parameters include: temperature of 850~950 ℃, vacuum degree ≤1×10 -3 Pa, heat preservation time is 1-2 hours.

[0051] Furthermore, before step (2), a surface treatment step is included to remove the oxide layer on the surface of the TiAl alloy preform, wherein the thickness of the oxide layer removed is preferably 0.1 to 1.0 mm.

[0052] Furthermore, the preparation method of the TiAl alloy ingot includes: weighing high-purity titanium raw materials and high-purity aluminum raw materials according to the atomic ratio of Ti and Al, and then melting them into TiAl alloy ingots.

[0053] Furthermore, the purity of the high-purity titanium raw material and the high-purity aluminum raw material is above 4N.

[0054] Furthermore, the melting process is one or more of vacuum induction melting, vacuum consumable arc melting, or water-cooled copper crucible melting, and is remelted 2 to 5 times to improve the uniformity of composition.

[0055] Furthermore, the smelting step includes: evacuating the furnace cavity to a vacuum level of ≤1×10⁻⁶. -2 The process begins with the introduction of high-purity Ar (≥99.999%) as a protective atmosphere. The melting temperature is 1500–1750 °C, or until the high-purity titanium and aluminum raw materials are completely melted and form a uniform molten pool. The single melting time is 3–30 min. By controlling these melting parameters, it is possible to ensure sufficient alloying and homogenization of Ti and Al raw materials while reducing the introduction of gaseous impurities such as oxygen and nitrogen. This also reduces the risk of Al volatilization, compositional deviation, and ingot defects caused by excessively high temperatures or long melting times.

[0056] The TiAl alloy target prepared by this invention can also be connected to a copper backing plate by brazing or diffusion welding according to the application requirements.

[0057] A third aspect of the present invention provides the use of the above-described TiAl alloy target or the TiAl alloy target prepared by the above-described preparation method in the preparation of TiAl thin films and / or TiAlN thin films.

[0058] The beneficial effects of the TiAl alloy target, its preparation method, and its application provided by this invention are as follows: The TiAl alloy target of this invention is a target formed by sintering at least two TiAl alloy preforms and TiAl alloy powder together. During the sintering process, the TiAl alloy powder undergoes plastic flow and diffusion sintering, closing the pores. Metallurgical diffusion bonding is formed between the TiAl alloy preform, the TiAl alloy powder matrix, and the TiAl alloy preform, constituting a connecting matrix and achieving diffusion bridging. This not only significantly reduces the amount of powder used, but also achieves a relative density of over 99%, with oxygen and carbon content controlled below 1000 ppm and 100 ppm, respectively. This meets the requirements of high density, low porosity, low inclusions, and consistent microstructure, solving the problem of simultaneously achieving large-size targets and low inclusions. It also reduces the risk of abnormal discharge and particle defects, and improves sputtering stability and film consistency. Attached Figure Description

[0059] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0060] Figure 1 This is a process flow diagram of the preparation process of TiAl alloy target material provided by the present invention.

[0061] Figure 2 This is a diagram of the loading structure for preparing TiAl alloy targets according to the present invention. Detailed Implementation

[0062] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0063] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field, or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.

[0064] The key terms used in this invention are explained as follows: (1) Large size preferred refers to diameter reaching Planar targets of 300 mm and above; (2) The relative compactness is preferably determined by the Archimedes method; (3) Surface roughness is preferably measured using a surface roughness meter, and the measurement object is the surface of TiAl target material; (4) Flatness is preferably measured using a coordinate measuring machine to measure the surface flatness of the TiAl target material; (5) The carbon content is preferably determined using a LECO carbon-sulfur analyzer, and the preferred testing method is combustion-infrared absorption method; (6) The oxygen content is preferably determined by a LECO oxygen, nitrogen and hydrogen analyzer, and the preferred test method is the inert gas melting method.

[0065] Example 1 A method for preparing a TiAl alloy target, the process flow diagram of which is shown below. Figure 1 As shown, it includes the following steps: (1) Smelting and preparing small-sized titanium-aluminum alloy ingots: High-purity titanium raw materials with a purity ≥4N and high-purity aluminum raw materials are selected and the materials are batched according to the atomic ratio of Ti:Al of 50:50; vacuum consumable arc melting is adopted, and the furnace cavity is evacuated to 5×10 before melting. -3 Pa was then introduced, followed by the introduction of high-purity Ar with a purity of 99.999% as a protective atmosphere. The melting current was 600 A, the melting voltage was 30 V, the melting temperature was 1650 ℃, and the single melting time was 10 min. After the alloy ingot cooled, it was turned over and remelted repeatedly, for a total of 3 remeltings, to obtain a small-sized TiAl alloy ingot with uniform composition. The small-sized TiAl alloy ingot was cylindrical with a diameter of 60 mm and a length of 80 mm. The test showed that there were no obvious shrinkage cavities or macroscopic cracks inside the small-sized TiAl alloy ingot, and the oxygen content was 260 ppm.

[0066] (2) Cutting and preparing TiAl alloy preforms: The above-mentioned small-sized TiAl alloy ingots were wire-cut into disc-shaped TiAl alloy preforms with a diameter of 50 mm and a thickness of 8 mm. The two ends and side surfaces of the TiAl alloy preforms were mechanically ground to remove the oxide layer on the surface. The thickness of the oxide layer removed was about 0.3 mm. The preforms were then dried at 80 °C for 2 h in an Ar atmosphere. A total of 61 disc-shaped TiAl alloy preforms were obtained.

[0067] (3) Preparation of titanium-aluminum alloy powder: Select TiAl alloy powder with the same composition as TiAl alloy preform, with an atomic ratio of Ti:Al of 50:50, purity ≥4N, D10 of 20 μm, D50 of 35 μm, and D90 of 60 μm; the oxygen content in TiAl alloy powder is 780 ppm, and it is transported in a high-purity Ar (purity of 99.999%) glove box for later use.

[0068] (4) Coordinated loading and structural arrangement: A stainless steel cladding with an inner diameter of 460 mm and a height of 16 mm was selected as the sintering container; a layer of TiAl alloy powder was laid at the bottom of the cladding; 61 TiAl alloy preforms were arranged in two staggered layers and loaded into the stainless steel cladding, so that the projected positions of adjacent TiAl alloy preforms did not completely overlap; TiAl alloy powder was then filled between adjacent TiAl alloy preforms, between TiAl alloy preforms and the side walls of the stainless steel cladding, and in the remaining spaces above and below. The total volume of the TiAl alloy preforms accounted for 36% of the cladding volume, and the TiAl alloy powder accounted for 64% of the cladding volume; after loading, the cladding was vibrated to ensure that the TiAl alloy powder fully filled all gaps, thus obtaining the loading system. The structural diagram of the loading is shown below. Figure 2 As shown.

[0069] (5) Degassing and encapsulation: The loading system is placed in a vacuum degassing furnace and heated to 500 ℃ at a rate of 5 ℃ / min, under a vacuum of 4×10 -3 The casing was held at Pa for 2.5 h; after degassing, it was welded and sealed in a high-purity Ar atmosphere with a purity ≥99.999%, and a helium leak test was performed, with a leakage rate ≤1×10⁻⁶. -8 Pa·m 3 / s.

[0070] (6) Overall diffusion sintering densification: The sealed stainless steel sheath is placed in a HIP (hot isostatic pressing) device, heated to 1100 ℃ and simultaneously pressurized to 135 MPa, and held at 1100 ℃ and 135 MPa for 3 h, and then cooled to room temperature with the furnace; during this process, TiAl alloy powder undergoes plastic flow and diffusion sintering, and metallurgical bonding is achieved between TiAl alloy preform and TiAl alloy powder, as well as between adjacent TiAl alloy preforms, to form a connecting matrix and form an integral TiAl target blank.

[0071] (7) Uncoating and Machining: The stainless steel cladding is mechanically removed to obtain a dense TiAl target blank; subsequently, it is machined, face-ground, and surface-polished to obtain a target blank with dimensions of [missing information]. A 450 mm × 12 mm TiAl alloy target, which is a large-size TiAl alloy target.

[0072] Testing revealed that the TiAl alloy target had a flatness of 0.028 mm, a surface roughness Ra of 0.25 μm, a relative density of 99.5%, an oxygen content of 780 ppm, a carbon content of 95 ppm, and a metallic impurity content of 0.0065 wt.%, meeting the 4N purity requirements. Microstructure analysis showed that the sintered TiAl alloy preforms were continuously and densely bonded to the surrounding substrate, with no obvious unbonded pores or through cracks.

[0073] Example 2 A method for preparing a large-size TiAl alloy target is basically the same as that in Example 1, except that the HIP in step (6) is replaced by vacuum hot pressing sintering, and the parameters of vacuum hot pressing sintering are: vacuum degree ≤ 5 × 10 -3 Pa, temperature 1050 ℃, pressure 30 MPa, heat and pressure holding time 4 h.

[0074] The TiAl alloy target material prepared in this embodiment has the following dimensions: A 450 mm × 12 mm TiAl alloy target, which is a large-size TiAl alloy target.

[0075] Testing revealed that the TiAl alloy target had a flatness of 0.035 mm, a surface roughness Ra of 0.28 μm, a relative density of 99.2%, an oxygen content of 760 ppm, a carbon content of 72 ppm, and a metallic impurity content of 0.0072 wt.%, meeting the 4N purity requirements. Microstructure showed that the TiAl alloy preforms were continuously and densely bonded to the surrounding substrate, with no obvious unbonded pores or through cracks.

[0076] Example 3 A method for preparing a large-size TiAl alloy target is basically the same as that in Example 1, except that the total volume of the TiAl alloy preform accounts for 50% of the cladding volume, and 85 TiAl alloy preforms are required.

[0077] The TiAl alloy target material prepared in this embodiment has the following dimensions: A 450 mm × 12 mm TiAl alloy target, which is a large-size TiAl alloy target.

[0078] Testing revealed that the TiAl alloy target had a flatness of 0.026 mm, a surface roughness Ra of 0.24 μm, a relative density of 99.6%, an oxygen content of 590 ppm, a carbon content of 51 ppm, and a metallic impurity content of 0.0060 wt.%, meeting the 4N purity requirements. Microstructure showed that the TiAl alloy preforms were continuously and densely bonded to the surrounding substrate, with no obvious unbonded pores or through cracks.

[0079] Example 4 A method for preparing a large-size TiAl alloy target is basically the same as that in Example 1, except that the atomic ratio of Ti:Al in step (1) is 55:45.

[0080] The TiAl alloy target material prepared in this embodiment has the following dimensions: A 450 mm × 12 mm TiAl alloy target, which is a large-size TiAl alloy target.

[0081] Testing revealed that the TiAl alloy target had a flatness of 0.030 mm, a surface roughness Ra of 0.26 μm, a relative density of 99.4%, an oxygen content of 710 ppm, a carbon content of 63 ppm, and a metallic impurity content of 0.0068 wt.%, meeting the 4N purity requirements. Microstructure showed that the TiAl alloy preforms were continuously and densely bonded to the surrounding substrate, with no obvious unbonded pores or through cracks.

[0082] Comparative Example 1 A method for preparing a TiAl alloy target is basically the same as that in Example 3, except that the TiAl alloy preform is replaced with TiAl alloy powder of equal volume.

[0083] The comparative example yielded a size of [size missing]. TiAl alloy target material of 450 mm × 12 mm.

[0084] The TiAl alloy target was tested and found to have a flatness of 0.041 mm, a surface roughness Ra of 0.31 μm, a relative density of 99.1%, an oxygen content of 1320 ppm, a carbon content of 126 ppm, and a metallic impurity content of 0.0095 wt.%.

[0085] Compared with Example 3, this comparative example uses TiAl alloy powder as raw material. Although a certain densification effect can be obtained, due to the large specific surface area of ​​the powder, oxygen, carbon and inclusions are more easily introduced during powder preparation, transportation, filling and sintering, resulting in an increase in the oxygen content and carbon content of the target material, which is not conducive to obtaining low-impurity TiAl alloy target material.

[0086] Comparative Example 2 A method for preparing a TiAl alloy target is basically the same as that in Example 3, except that TiAl alloy powder is not added, that is, in step (4), the TiAl alloy preform is simply put into a stainless steel sleeve.

[0087] The comparative example yielded a size of [size missing]. A 450 mm × 12 mm TiAl alloy target, which is a large-size TiAl alloy target.

[0088] Testing revealed that the TiAl alloy target had a flatness of 0.052 mm, a surface roughness Ra of 0.34 μm, a relative density of 93.8%, an oxygen content of 460 ppm, a carbon content of 48 ppm, and a metallic impurity content of 0.0062 wt.%. Compared to Example 3, this comparative example did not use TiAl alloy powder to fill the gaps between adjacent preforms and between the preforms and the cladding. This resulted in a lack of effective interstitial phases and diffusion bridging phases during sintering, making it difficult to achieve sufficient metallurgical bonding between multiple TiAl alloy preforms. Consequently, the relative density of the target decreased, and the porosity increased.

[0089] Comparative Example 3 A method for preparing a TiAl alloy target is basically the same as that in Example 3, except that the total volume of the TiAl alloy preform accounts for 30% of the encapsulation volume, and the TiAl alloy powder accounts for 70% of the encapsulation volume.

[0090] The comparative example yielded a size of [size missing]. TiAl alloy target material of 450 mm × 12 mm.

[0091] The TiAl alloy target was tested and found to have a flatness of 0.039 mm, a surface roughness Ra of 0.30 μm, a relative density of 99.2%, an oxygen content of 1150 ppm, a carbon content of 112 ppm, and a metallic impurity content of 0.0088 wt.%.

[0092] Compared with Example 3, the volume fraction of TiAl alloy preform in this comparative example is less than 35%, and the amount of TiAl alloy powder is significantly increased. This weakens the role of TiAl alloy preform as a low-impurity dense framework and increases the risk of oxygen, carbon and inclusions introduced by TiAl alloy powder, resulting in increased oxygen and carbon content of the target material.

[0093] Comparative Example 4 A method for preparing a TiAl alloy target is basically the same as that in Example 3, except that the total volume of the TiAl alloy preform accounts for 95% of the encapsulation volume, and the TiAl alloy powder accounts for 5% of the encapsulation volume.

[0094] The comparative example yielded a size of [size missing]. TiAl alloy target material of 450 mm × 12 mm.

[0095] The TiAl alloy target was tested and found to have a flatness of 0.058 mm, a surface roughness Ra of 0.36 μm, a relative density of 97.3%, an oxygen content of 520 ppm, a carbon content of 54 ppm, and a metallic impurity content of 0.0064 wt.%.

[0096] Compared with Example 3, the volume fraction of TiAl alloy preforms in this comparative example is higher than 90%, and the amount of TiAl alloy powder is too small, making it difficult to fully fill the gaps between TiAl alloy preforms and between the preforms and the cladding. This results in insufficient diffusion area and inadequate interfacial metallurgical bonding, thereby reducing the relative density and microstructure uniformity of the target material and increasing the risk of porosity and weak interface formation.

[0097] Based on the results of Example 3 and Comparative Examples 1-4, it can be seen that although using full powder sintering alone in Comparative Example 1 is beneficial for large-size forming, it is easy to introduce high levels of oxygen, carbon, and inclusions due to excessive TiAl alloy powder usage. In Comparative Example 2, using TiAl alloy preform sintering alone, there is a lack of effective interstitial filling and diffusion, which easily leads to unbonded interfaces and residual pores.

[0098] When the volume fraction of the TiAl alloy preform in Comparative Example 3 is less than 30%, the risk of impurity introduction related to the TiAl alloy powder increases; when the volume fraction of the TiAl alloy preform in Comparative Example 4 is greater than 90%, the TiAl alloy powder has insufficient interstitial filling and interfacial bridging.

[0099] Therefore, by controlling the total volume of the TiAl alloy preform within the range of 35% to 90% of the cladding volume, and by combining TiAl alloy powder interstitial filling and overall diffusion sintering, a TiAl alloy target material that simultaneously achieves low oxygen and low carbon content, high density, uniform microstructure, and high yield can be obtained.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A TiAl alloy target material, characterized in that, The method for preparing the TiAl alloy target includes the following steps: (1) Cut TiAl alloy ingots into TiAl alloy preforms; (2) At least two of the TiAl alloy preforms are loaded into a sleeve, and TiAl alloy powder is filled between adjacent TiAl alloy preforms and between the TiAl alloy preforms and the sleeve to obtain a loading system; (3) The charging system is degassed and then sintered to obtain a target blank; (4) Perform post-processing on the target blank; The TiAl alloy target material includes the following characteristics a and b: a. Relative density ≥ 99%; b. Oxygen content ≤ 1000 ppm and carbon content ≤ 100 ppm; The particle size D90 of the TiAl alloy powder is within 100 μm; the atomic ratio of Ti to Al in the TiAl alloy preform and the TiAl alloy powder are independently (20:80) to (80:20). The total volume of the TiAl alloy preform accounts for 35% to 90% of the volume of the cladding.

2. The TiAl alloy target material according to claim 1, characterized in that, The TiAl alloy preform is disc-shaped with a diameter of 10–120 mm and a thickness of 2–20 mm.

3. The TiAl alloy target material according to claim 1 or 2, characterized in that, The TiAl alloy target material also includes at least one of the following characteristics: c. The TiAl alloy target is a disc-shaped planar target with a diameter of 300-600 mm and a thickness of 5-25 mm; d. Surface roughness Ra≤0.4 μm; e. Flatness ≤ 0.05 mm.

4. The TiAl alloy target material according to claim 3, characterized in that, The width of the gap is 0.2–10 mm; And / or, the diameter of the TiAl alloy ingot is 20 to 120 mm.

5. The TiAl alloy target material according to claim 3 or 4, characterized in that, The sintering is carried out by hot isostatic pressing, and the parameters of hot isostatic pressing include: temperature of 900-1300 ℃, pressure of 80-180 MPa, and time of 2-6 h. Alternatively, the sintering may be performed using vacuum hot pressing, wherein the parameters of the vacuum hot pressing include: vacuum degree ≤ 10. -2 Pa, temperature 900–1200 ℃, pressure 20–50 MPa, time 2–6 h.

6. The TiAl alloy target material according to claim 3 or 4, characterized in that, The degassing parameters include: temperature of 300–600 °C and vacuum degree ≤10. -2 Pa, heat preservation time is 1-4 h; the post-treatment includes machining and / or annealing steps; And / or, after the degassing is completed, the process further includes a step of sealing the package.

7. The TiAl alloy target material according to claim 3 or 4, characterized in that, Before step (2), the TiAl alloy preform is further subjected to a surface treatment step to remove the oxide layer on the surface.

8. The use of the TiAl alloy target according to any one of claims 1 to 7 in the preparation of TiAl thin films and / or TiAlN thin films.

Citation Information

Patent Citations

  • A method for preparing a titanium-aluminum alloy target

    CN112725658B

  • Preparation method of high-density TiAl and TiAlMe target material

    CN113981388A

  • Preparation method of molybdenum titanium alloy material with high density, large size and high homogeneity

    CN103740979A

  • Titanium-aluminum (Ti-Al) alloy sputtering target

    TW201612347A