A method for preparing sodium hexafluorophosphate

By conducting homogeneous synthesis and two-stage gradient cooling crystallization in a supercritical anhydrous hydrogen fluoride medium, combined with silane catalysts and an Oslo crystallizer, the problems of low efficiency, low yield, and high energy consumption in the synthesis of sodium hexafluorophosphate were solved, achieving efficient and low-energy preparation of sodium hexafluorophosphate.

CN122853353BActive Publication Date: 2026-11-10HUBEI HONGYUAN PHARMA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611347674.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-10
Estimated Expiration
2046-09-02

AI Technical Summary

Technical Problem

Existing processes for synthesizing sodium hexafluorophosphate suffer from low efficiency in batch reactions, low crystallization yield, and high energy consumption. Furthermore, the limited solubility in supercritical carbon dioxide systems increases the complexity of the system.

Method used

Supercritical anhydrous hydrogen fluoride was used as the reaction medium, combined with silane catalysts for homogeneous synthesis. Continuous and efficient synthesis of sodium hexafluorophosphate was achieved through two-stage gradient cooling crystallization and reaction stabilization treatment. Controllable nucleation and crystal growth were carried out using the solubility curve of sodium hexafluorophosphate in anhydrous hydrogen fluoride. The Oslo crystallizer was used for staged growth, and the waste heat of the supercritical reaction liquid was recovered.

Benefits of technology

The continuous and efficient synthesis of sodium hexafluorophosphate was achieved, with a crystallization yield increased by more than 50%, energy consumption reduced by more than 20%, product purity and particle size distribution uniformity improved, and the total yield of mother liquor recycling reached 99%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This application relates to the field of fluorochemical material preparation technology, and in particular to a method for preparing sodium hexafluorophosphate. The preparation method includes: mixing phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride; adding a silane catalyst under supercritical anhydrous hydrogen fluoride conditions to carry out a homogeneous synthesis reaction, obtaining a primary reaction solution; transferring the primary reaction solution to a stirred tank for phase stabilization treatment, obtaining a stable reaction solution; pre-cooling the stable reaction solution and then subjecting it to two-stage gradient cooling crystallization with simultaneous pressure reduction to obtain a crystallization slurry containing sodium hexafluorophosphate crystals; performing solid-liquid separation, washing, and drying of the crystallization slurry to obtain the sodium hexafluorophosphate product, with the mother liquor recycled. The preparation method of this application solves the problems of low reaction efficiency, low crystallization yield, and high energy consumption associated with traditional batch reactor processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of fluorochemical materials preparation technology, and in particular to a method for preparing sodium hexafluorophosphate. Background Technology

[0002] Sodium hexafluorophosphate (NaPF6) is the core electrolyte salt in sodium-ion battery electrolytes. Its purity, crystal form, and particle size distribution directly affect the battery's cycle performance, rate performance, and safety.

[0003] In existing technologies, the industrial synthesis process of sodium hexafluorophosphate mainly employs a batch reactor, using anhydrous hydrogen fluoride as a solvent, to carry out a heterogeneous reaction between phosphorus pentafluoride and sodium fluoride. This route suffers from problems such as difficulty in achieving continuous production, low crystallization yield, and high energy consumption.

[0004] In addition, there are existing technologies that use supercritical carbon dioxide as a reaction solvent or crystallization medium to synthesize hexafluorophosphate. However, the solubility of sodium hexafluorophosphate in the supercritical carbon dioxide system is limited, and the additional CO2 required increases the complexity of the system.

[0005] Therefore, it is necessary to develop a continuous preparation process for sodium hexafluorophosphate that takes into account synthesis efficiency, crystallization yield, energy consumption, and safety in order to overcome the above-mentioned technical bottlenecks. Summary of the Invention

[0006] This invention provides a method for preparing sodium hexafluorophosphate, which solves the technical problems of low efficiency, low crystallization yield, high energy consumption and uneven crystal form in the prior art.

[0007] This application provides a method for preparing sodium hexafluorophosphate, comprising the following steps: S1. Phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride are mixed, and a silane catalyst is added under supercritical anhydrous hydrogen fluoride conditions to carry out a homogeneous synthesis reaction to obtain a primary reaction solution containing sodium hexafluorophosphate; wherein the silane catalyst is trimethylfluorosilane and / or triethylfluorosilane. S2. The primary reaction solution is subjected to a reaction stabilization treatment to obtain a stable reaction solution; S3. After precooling the stable reaction liquid, a two-stage gradient cooling crystallization is performed, and a gradient depressurization is performed simultaneously to obtain a crystallization slurry containing sodium hexafluorophosphate crystals; wherein, the two-stage gradient cooling crystallization includes a first-stage cooling crystallization and a second-stage cooling crystallization; the temperature of the first-stage cooling crystallization is 50-52℃, and the pressure is reduced to 0.72-0.75MPa; the temperature of the second-stage cooling crystallization is 20-22℃, and the pressure is reduced to 0.11-0.20MPa. S4. Perform solid-liquid separation on the crystallized slurry, wash and dry the obtained sodium hexafluorophosphate crystals to obtain sodium hexafluorophosphate product, and recycle the obtained mother liquor to step S1.

[0008] Furthermore, in step S3, before the stable reaction solution undergoes two-stage gradient cooling crystallization, the stable reaction solution is pre-cooled to 60-65°C.

[0009] Further, in step S3, the stable reaction solution is pre-cooled to 60-65°C, including the following steps: The stable reaction liquid is heated by exchanging heat with phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride, so that the stable reaction liquid is cooled to 70-80°C, and phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride are preheated to 120-150°C. The stable reaction liquid is cooled by exchanging heat with cooling water, so that the stable reaction liquid is cooled to 60-65℃.

[0010] Further, in step S1, the molar ratio of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride is 1.05-1.1:1:22-24.

[0011] Further, in step S1, the reaction temperature of the homogeneous synthesis reaction is set to 190–220°C, and the reaction pressure is set to 7.0–9.0 MPa.

[0012] Furthermore, in step S1, the reaction time of the homogeneous synthesis reaction is set to 15–30 s.

[0013] Further, in step S1, the amount of the silane catalyst added is 0.1% to 0.5% of the total mass of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride.

[0014] Further, in step S2, the reaction stabilization treatment includes: stirring the primary reaction solution at a stirring speed of 150-300 r / min for a stirring time of 5-15 min.

[0015] Further, in step S4, the sodium hexafluorophosphate crystals are washed with anhydrous hydrogen fluoride 2 to 3 times; and / or In step S4, the drying temperature is 100-110℃, the drying time is 8-10h, and the vacuum degree is -0.09--0.1MPa.

[0016] In summary, this application includes at least one of the following beneficial technical effects: 1. Supercritical anhydrous hydrogen fluoride is used as the reaction medium to dissolve or highly disperse phosphorus pentafluoride and sodium fluoride in supercritical HF to form a homogeneous reaction system, which reduces the gas-liquid heterogeneous mass transfer resistance in traditional batch process; combined with the synergistic catalytic effect of silane catalysts, the reaction residence time is further shortened, realizing continuous and efficient synthesis.

[0017] 2. A two-stage gradient cooling process is set up to match the high slope region of the solubility curve of sodium hexafluorophosphate in anhydrous hydrogen fluoride, taking into account both high precipitation and controllable nucleation. The yield of one crystallization can reach 11.7% to 12.3%, which is about 50% to 60% higher than the traditional low temperature crystallization process. The total yield after mother liquor recycling can reach more than 99%.

[0018] 3. By recovering the waste heat of the supercritical reaction liquid in stages and setting a narrow cooling range, the heat exchange load is significantly reduced, and the energy consumption per unit product is reduced to 4.0-4.5 kWh / kg, which saves more than 20% energy compared with the traditional process and reduces production costs. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0020] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent three situations: A exists alone, A and B exist simultaneously, and B exists alone.

[0021] As described in the background section, the existing synthesis process of sodium hexafluorophosphate mainly uses a batch reactor for gas-liquid heterogeneous reaction, which has prominent problems such as low reaction efficiency, low crystallization yield and high energy consumption.

[0022] To address the aforementioned problems, this application provides a supercritical synthesis coupled with gradient crystallization process, the core of which is as follows: 1) By replacing the subcritical or atmospheric pressure HF solvent system with supercritical anhydrous hydrogen fluoride, and combining it with a pipeline reactor and silane catalysts, homogeneous synthesis can be achieved, which greatly improves the reaction efficiency. 2) Stabilize the reaction by using a time-delayed stirred tank to eliminate reaction pulses in the pipeline reactor, ensuring the full conversion of phosphorus pentafluoride and the uniformity and stability of the reaction liquid components; 3) According to numerous experiments, the solubility of sodium hexafluorophosphate in anhydrous hydrogen fluoride varies most drastically in the range of 40–60°C (slope of approximately 0.32 wt% / °C), while the solubility change tends to be gradual in the range below 20°C.

[0023] Based on this discovery, this application selects a nucleation stage of 50–52°C and a growth stage of 20–22°C to divide the crystallization process into a nucleation stage and a growth stage, respectively. This fully utilizes the precipitation potential of the high-slope region while avoiding energy waste and solvent flash evaporation risks caused by excessive cooling. If the crystallization temperature is further reduced to 0°C (as in Comparative Example 3), although the yield will increase slightly, it will lead to serious problems such as solvent flash evaporation, crystal fragmentation, decreased purity, and a surge in energy consumption.

[0024] This application ultimately selects the cooling range and pressure reduction path based on the solubility curve of sodium hexafluorophosphate in anhydrous hydrogen fluoride determined by the system, and adopts a two-stage gradient cooling crystallization coupled with an Oslo crystallizer to achieve controllable nucleation and crystal hierarchical growth. 4) The waste heat of the supercritical reaction liquid is recovered in stages, which greatly reduces the total energy consumption of the system.

[0025] Correspondingly, the core reaction equation involved in this application is as follows: ①PF5 + NaF → NaPF6 (Main reaction) Catalytic mechanism: ②(CH3)3SiF+HF⇌(CH3)3Si + +HF2 - (Activation F) - ) ③PF5+HF2 - +Na + →NaPF6+HF This application discloses a method for preparing sodium hexafluorophosphate, comprising the following steps: S1. Phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride are mixed, and a silane catalyst is added under supercritical anhydrous hydrogen fluoride conditions to carry out a homogeneous synthesis reaction to obtain a primary reaction solution containing sodium hexafluorophosphate.

[0026] Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride are mixed in a certain molar ratio and fed into a pipeline reactor. The temperature and pressure of the reaction system are raised to the supercritical anhydrous hydrogen fluoride state. A silane catalyst is added, and the homogeneous synthesis reaction is completed in the pipeline reactor to obtain a primary reaction solution containing sodium hexafluorophosphate.

[0027] Anhydrous hydrogen fluoride serves as both a solvent and a catalyst in the reaction, thus eliminating the need for additional solvents or reaction media after it reaches supercriticality. In the supercritical state, anhydrous hydrogen fluoride combines the high diffusivity of a gas with the high solubility of a liquid, allowing both phosphorus pentafluoride and sodium fluoride to dissolve or disperse highly within it, forming a homogeneous reaction system and reducing the mass transfer resistance between the gas and liquid phases in traditional batch processes.

[0028] In some embodiments, the reaction temperature can be any value or a range between any two of 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, and 220°C. The reaction pressure can be any value or a range between any two of 7.0 MPa, 7.5 MPa, 8.0 MPa, 8.5 MPa, and 9.0 MPa.

[0029] In a preferred embodiment, the reaction temperature is 205°C and the reaction pressure is 8.0 MPa.

[0030] In some embodiments, the molar ratio of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride is 1.05 to 1.1:1:22 to 24, for example 1.05:1:22, 1.08:1:23, 1.1:1:24.

[0031] Phosphorus pentafluoride is used in a slightly excess amount (5%–10%) relative to sodium fluoride to fully promote the reaction towards the formation of sodium hexafluorophosphate and ensure the conversion rate of sodium fluoride. If the amount of phosphorus pentafluoride is insufficient, unreacted sodium fluoride will remain in the product, affecting purity; if the amount of phosphorus pentafluoride is excessive, the excess phosphorus pentafluoride needs to be separated and recovered in subsequent processes, increasing operational complexity and cost.

[0032] In some embodiments, the amount of anhydrous hydrogen fluoride is selected as 22-24 mol, which ensures that the system has good fluidity and solubility in the supercritical state, and also keeps the sodium hexafluorophosphate concentration in the appropriate crystallization range in the subsequent crystallization process.

[0033] It should be noted that the silane catalyst introduced in this application is a key technical element for achieving second-level reactions. Taking trimethylfluorosilane as an example, its catalytic mechanism can be described as follows: The Si–F bond in trimethylfluorosilane undergoes an exchange reaction with the HF molecule in anhydrous hydrogen fluoride to generate a trimethylsilane cation (CH3)3Si. + and hydrogen difluoride anions HF2 - HF2 - It is a more active nucleophilic fluoride species that can efficiently attack the phosphorus center of phosphorus pentafluoride and promote the formation of PF bonds.

[0034] Meanwhile, silane groups and Na +Weak coordination can form between them, which to some extent reduces the lattice energy of sodium fluoride, thus facilitating the dissolution of NaF and its participation in the reaction. This catalytic effect significantly lowers the activation energy of the reaction, thereby improving the conversion efficiency of phosphorus pentafluoride.

[0035] In some embodiments, the silane catalyst is trimethylfluorosilane and / or triethylfluorosilane. Of course, a mixture of trimethylfluorosilane and triethylfluorosilane can also be used as a catalyst.

[0036] It is understandable that the silane catalysts mentioned above have low boiling points and can be fully volatilized and removed in the subsequent vacuum drying step of 100-110°C, without the need for additional catalyst separation and purification processes, thus ensuring the purity of the final product.

[0037] In some embodiments, the amount of silane catalyst added is 0.1% to 0.5% of the total mass of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride, for example 0.1%, 0.2%, 0.3%, 0.4% and 0.5%.

[0038] In a preferred embodiment, the catalyst addition amount is 0.3%.

[0039] In some embodiments, the pipeline reactor employs a micro-static mixing structure with a dead-zone-free design to ensure homogeneous mixing of the raw materials the instant they enter the pipeline reactor, eliminating dead zones and short-circuit flow, and avoiding localized uneven reactions. The reaction time of the raw materials in the pipeline reactor can be any value among 15s, 20s, 25s, and 30s, or a range between any two values.

[0040] S2. The primary reaction solution is subjected to a reaction stabilization treatment to obtain a stable reaction solution.

[0041] The primary reaction liquid flowing out of the pipeline reactor is sent to a stirred tank. The stirring speed and stirring time are controlled to stabilize the primary reaction liquid, make up for the reaction residence time, eliminate any reaction pulses that may exist in the pipeline reactor, and ensure that the conversion rate of phosphorus pentafluoride in the reaction liquid reaches more than 99.9%, so as to obtain a stable reaction liquid with uniform composition.

[0042] The stirred tank effectively homogenizes the component concentration and temperature distribution of the reaction solution through a buffer stirring time of 5-15 min and moderate stirring at 150-300 r / min, providing a uniform feed for subsequent gradient crystallization and avoiding explosive nucleation or uneven crystal quality caused by concentration fluctuations.

[0043] In some embodiments, the stirring speed can be any value or a range between any two of 150 r / min, 200 r / min, 220 r / min, 250 r / min, and 300 r / min. The stirring time can be any value or a range between any two of 5 min, 8 min, 10 min, 12 min, and 15 min.

[0044] S3. After precooling the stable reaction liquid, perform two-stage gradient cooling crystallization and simultaneously perform gradient pressure reduction to obtain a crystallization slurry containing sodium hexafluorophosphate crystals.

[0045] Specifically, S3 includes the following steps: S31. Pre-cool the stable reaction solution to 60-65℃.

[0046] The high-temperature stable-phase reaction liquid flowing out of the stirred tank first enters a plate heat exchanger, where it undergoes countercurrent heat exchange with the synthesis raw materials before entering the tubular reactor, preheating the raw materials to 120–150°C while the stable-phase reaction liquid itself cools down to 70–80°C. Subsequently, the stable-phase reaction liquid is further cooled to 60–65°C by cooling water.

[0047] It is understandable that the above heat exchange operation can reduce the total energy consumption of the system. If waste heat recovery is not performed, and the high-temperature reaction liquid is directly cooled to 60-65°C by cooling water, not only will a large amount of high-grade heat energy be wasted, but the amount of cooling water and the area of ​​the heat exchanger will also need to be increased, resulting in a significant increase in both system energy consumption and equipment costs.

[0048] S32. The pre-cooled stable reaction solution is subjected to two-stage gradient cooling crystallization.

[0049] The crystals undergo a first-stage cooling process, with the temperature reduced to 50–52°C (nucleation stage) and the pressure simultaneously reduced to 0.72–0.75 MPa to achieve controllable nucleation. A second-stage cooling process then follows, reducing the temperature to 20–22°C (growth stage) and the pressure simultaneously reduced to 0.11–0.20 MPa to achieve stable crystal growth. The cooling range is controlled to approximately 40°C.

[0050] It should be noted that the gradient cooling range was determined based on the solubility curve of sodium hexafluorophosphate in anhydrous hydrogen fluoride, and the solubility in anhydrous hydrogen fluoride was determined through systematic experiments.

[0051] The specific determination method was as follows: In a sealed autoclave, the temperatures were controlled at 20℃, 30℃, 40℃, 50℃, 60℃, and 70℃ respectively. Excess sodium hexafluorophosphate was added to anhydrous hydrogen fluoride, and the mixture was stirred at a constant temperature for 24 hours until dissolution equilibrium was reached. Samples were then taken for analysis. The determination results are shown in Table 1.

[0052] Table 1. Solubility of sodium hexafluorophosphate in anhydrous hydrogen fluoride As shown in Table 1, the solubility increases significantly with increasing temperature in the range of 20–60℃. The solubility change is most dramatic in the range of 40–60℃, with a slope of approximately 0.32 wt% / ℃, which is a high-slope region.

[0053] Based on this discovery, 50–52℃ was selected as the nucleation stage, and 20–22℃ as the end point of the growth stage. The cooling range of approximately 40℃ covered the region with the most dramatic changes in the solubility curve, achieving a large precipitation amount with relatively small cooling costs, thus balancing crystallization yield and energy consumption.

[0054] It should be noted that the operating pressure must be synchronized with the saturated vapor pressure of anhydrous hydrogen fluoride at the corresponding temperature to ensure that the system remains in the liquid phase throughout the process and to avoid solvent flash evaporation. According to the physical property data of anhydrous hydrogen fluoride, its saturated vapor pressure is approximately 0.103 MPa at 20°C and approximately 1.045 MPa at 60°C.

[0055] In this process, the operating pressure is 0.72–0.75 MPa when the temperature is lowered to 50–52°C during the first-stage cooling crystallization and 0.11–0.20 MPa when the temperature is lowered to 20–22°C during the second-stage cooling crystallization. Both pressures are slightly higher than the saturated vapor pressure at the corresponding temperatures. If the operating pressure is lower than the saturated vapor pressure, anhydrous hydrogen fluoride will flash, generating bubbles that disturb the crystallization liquid surface, leading to problems such as explosive nucleation, crystal fragmentation, and uneven particle size.

[0056] In some embodiments, the two-stage gradient cooling crystallization is carried out in an Oslo crystallizer, which adopts a countercurrent fluidized bed structure and has an upward flow velocity of 0.05 to 0.15 m / s, for example 0.05 m / s, 0.08 m / s, 0.10 m / s, 0.12 m / s, or 0.15 m / s.

[0057] In a countercurrent fluidized bed, crystals are suspended according to particle size classification. Coarse crystals settle at the bottom and are collected, while fine crystals are suspended at the top. The rising mother liquor carries the fine crystals to the heat exchange zone for re-dissolution, nucleation, and growth. This avoids the problems of fine crystal entrainment and large crystal deposition that clog the tower, thus achieving the goal of controlling the crystal D90 to 50–150 μm and uniform particle size distribution.

[0058] Furthermore, the heat of crystallization released in the nucleation stage is removed by circulating water at 30–40°C, while the growth stage uses conventional cooling water at 7–12°C. This segmented heat exchange further reduces the overall energy consumption of the system.

[0059] S4. Perform solid-liquid separation on the crystallized slurry, wash and dry the obtained sodium hexafluorophosphate crystals to obtain sodium hexafluorophosphate product, and recycle the obtained mother liquor to step S1.

[0060] Sodium hexafluorophosphate crystals in the crystallization slurry are separated from the mother liquor by centrifugation and washed 2-3 times with anhydrous hydrogen fluoride to remove the mother liquor and trace impurities adhering to the crystal surface.

[0061] In some embodiments, the washed crystals are dried at a temperature of 100–110°C and a vacuum of -0.09–-0.1 MPa for 8–10 hours, for example, at 100°C for 10 hours, at 105°C for 8 hours, or at 110°C for 8 hours.

[0062] It is understandable that setting the drying temperature at 100-110℃ can ensure the full removal of anhydrous hydrogen fluoride adsorbed on the crystal surface, and also allow the trace amounts of silane catalyst residues to volatilize at this temperature, eliminating the need for a dedicated catalyst removal process.

[0063] The separated mother liquor (still containing dissolved sodium hexafluorophosphate) is returned to the raw material mixing tank via a mother liquor circulation pump. It is then mixed with newly added phosphorus pentafluoride and sodium fluoride and recycled to maximize the utilization of raw materials. The total yield of the mother liquor after recycling can reach over 99%.

[0064] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0065] Example 1: A method for preparing sodium hexafluorophosphate, comprising the following steps: S1. Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride are mixed in a molar ratio of 1.05:1:22 and fed into a pipeline reactor. The system temperature is raised to 190℃ and the pressure is raised to 7.0MPa to enter the supercritical anhydrous hydrogen fluoride homogeneous state. Trimethylfluorosilane catalyst (0.1% of the total mass of raw materials) is added and reacted in the pipeline reactor for 30s to carry out a homogeneous synthesis reaction to obtain the primary reaction solution.

[0066] S2. The primary reaction solution is fed into a stirred tank and stirred at 150 r / min for 5 min to obtain a stable phase reaction solution with uniform composition.

[0067] S3. The stable reaction liquid flowing out of the stirred tank is passed through a preheater and exchanged with the synthesis raw materials in a countercurrent manner to recover the waste heat and pre-cool it to 63°C. It is then fed into the Oslo crystallizer with a countercurrent fluidized bed structure, with an upward flow velocity of 0.10 m / s; The temperature was reduced to 51°C through primary cooling crystallization, and the pressure was simultaneously reduced to an absolute pressure of 0.73 MPa. The temperature was reduced to 22°C through a two-stage cooling crystallization process, while the pressure was simultaneously reduced to an absolute pressure of 0.15 MPa. The temperature drop was approximately 41°C.

[0068] S4. Centrifuge to separate sodium hexafluorophosphate crystals from the mother liquor, wash twice with anhydrous hydrogen fluoride, and dry at 100℃ and a vacuum of -0.09 MPa for 10 hours to obtain the sodium hexafluorophosphate product. The mother liquor is recycled back to the synthesis process.

[0069] Results of this embodiment: primary crystallization yield 11.7%, product purity 99.95%, energy consumption per unit product 4.0 kWh / kg, crystal D90 142 μm.

[0070] Example 2: A method for preparing sodium hexafluorophosphate, comprising the following steps: S1. Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride are mixed in a molar ratio of 1.08:1:23 and fed into a pipeline reactor. The system temperature is raised to 205℃ and the pressure is raised to 8.0MPa to enter the supercritical anhydrous hydrogen fluoride homogeneous state. Triethylfluorosilane catalyst (0.3% of the total mass of raw materials) is added and reacted in the pipeline reactor for 20s to carry out a homogeneous synthesis reaction, obtaining the primary reaction solution.

[0071] S2. The primary reaction solution is fed into a stirred tank, stirred at 220 r / min for 10 min, to obtain a stable phase reaction solution with uniform composition.

[0072] S3. The stable reaction liquid flowing out of the stirred tank is passed through a preheater and exchanged with the synthesis raw materials in a countercurrent manner to recover the waste heat and pre-cool it to 62°C. It is then fed into the Oslo crystallizer with a countercurrent fluidized bed structure, with an upward flow velocity of 0.08 m / s; The temperature was reduced to 50°C through primary cooling crystallization, and the pressure was simultaneously reduced to an absolute pressure of 0.74 MPa. The temperature was reduced to 20°C through a two-stage cooling crystallization process, and the pressure was simultaneously reduced to an absolute pressure of 0.13 MPa.

[0073] S4. Centrifuge to separate sodium hexafluorophosphate crystals from the mother liquor, wash three times with anhydrous hydrogen fluoride, and dry at 105℃ and a vacuum of -0.095MPa for 8 hours to obtain the sodium hexafluorophosphate product. The mother liquor is recycled back to the synthesis process.

[0074] Results of this embodiment: primary crystallization yield 12.2%, product purity 99.97%, energy consumption per unit product 4.2 kWh / kg, crystal D90 98 μm.

[0075] Example 3: A method for preparing sodium hexafluorophosphate, comprising the following steps: S1. Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride are mixed in a molar ratio of 1.1:1:24 and fed into a pipeline reactor. The system temperature is raised to 220°C and the pressure is raised to 9.0 MPa, entering a supercritical anhydrous hydrogen fluoride homogeneous state. A mixed catalyst of trimethylfluorosilane and triethylfluorosilane (mass ratio 1:1, total addition amount is 0.5% of the total mass of raw materials) is added. The reaction is carried out in the pipeline reactor for 15s to carry out a homogeneous synthesis reaction, obtaining the primary reaction solution.

[0076] S2. The primary reaction solution is fed into a stirred tank and stirred at 300 r / min for 15 min to obtain a stable phase reaction solution with uniform composition.

[0077] S3. The stable reaction liquid flowing out of the stirred tank is passed through a preheater and exchanged with the synthesis raw materials in a countercurrent manner to recover the waste heat and pre-cool it to 61°C. It is then fed into the Oslo crystallizer with a countercurrent fluidized bed structure, with an upward flow velocity of 0.12 m / s; The temperature was reduced to 52°C through primary cooling crystallization, and the pressure was simultaneously reduced to an absolute pressure of 0.75 MPa. The temperature was reduced to 20°C through a two-stage cooling crystallization process, and the pressure was simultaneously reduced to an absolute pressure of 0.18 MPa.

[0078] S4. Centrifuge to separate sodium hexafluorophosphate crystals from the mother liquor, wash three times with anhydrous hydrogen fluoride, and dry at 100℃ and a vacuum of -0.1MPa for 8 hours to obtain the sodium hexafluorophosphate product. The mother liquor is recycled back to the synthesis process.

[0079] Results of this embodiment: primary crystallization yield 12.3%, product purity 99.98%, energy consumption per unit product 4.5 kWh / kg, crystal D90 56 μm.

[0080] Comparative Example 1: The difference between Comparative Example 1 and Examples 1-3 is that: a traditional batch reactor was used for heterogeneous synthesis, no catalyst was added, and no pipeline reactor or Oslo crystallizer was used. The crystallization method was deep cooling single-stage crystallization.

[0081] The specific operation is as follows: Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride are mixed in a molar ratio of 1.07:1:60 in a batch reactor and reacted at 10℃ and 0.3-0.5MPa (autogenous pressure inside the closed reactor) for 2 hours. After the reaction is completed, the mixture is naturally cooled to -30℃ to crystallize. The product is then obtained by centrifugation, washing, and drying.

[0082] The specific steps are as follows: Phosphorus pentafluoride, sodium fluoride, and anhydrous hydrogen fluoride were mixed in a molar ratio of 1.07:1:60 in a batch reactor and reacted at 10°C and 0.3–0.5 MPa for 2 hours. After the reaction was completed, the mixture was allowed to cool naturally to -30°C to crystallize. The product was then obtained by centrifugation, washing, and drying.

[0083] Results: The yield of primary crystallization was 7.8%, the product purity was 99.80%, the energy consumption per unit product was 5.2 kWh / kg, the D90 was 210 μm, and the particle size distribution was uneven.

[0084] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that no silane catalyst is added in step S1, while the rest of the steps are exactly the same as in Example 2.

[0085] Results: The yield of one-time crystallization was 10.5%, the product purity was 99.62%, the energy consumption per unit product was 4.2 kWh / kg, and the D90 was 105 μm.

[0086] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that: in step S3, the two-stage gradient cooling crystallization is not used. Instead, the stable reaction liquid pre-cooled to 63°C is directly and rapidly cooled to 0°C in a single-stage crystallizer, and the operating pressure is reduced to 0.08 MPa. The remaining steps are exactly the same as in Example 2.

[0087] Results: The yield of primary crystallization was 14.8%, the product purity was 99.55%, the energy consumption per unit product was 5.8 kWh / kg, the D90 was 22 μm, the particle size distribution was extremely uneven, and the crystal morphology was irregular.

[0088] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that the Oslo crystallizer is not used in step S3, but a conventional stirred crystallizer is used for two-stage gradient cooling crystallization. The remaining steps are exactly the same as in Example 2.

[0089] Results: The yield of primary crystallization was 12.0%, the product purity was 99.80%, the energy consumption per unit product was 4.3 kWh / kg, the D90 was 235 μm, the particle size distribution was uneven, and there was obvious fine crystal entrainment.

[0090] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step S2 is omitted, and the primary reaction liquid flowing out of the pipeline reactor directly enters the gradient cooling crystallization process. The remaining steps are exactly the same as in Example 2.

[0091] Results: The yield of primary crystallization was 11.5%, the product purity was 99.70%, the energy consumption per unit product was 4.2 kWh / kg, and the D90 was 115 μm. However, the particle size fluctuated greatly between batches (D90 standard deviation ±35 μm).

[0092] Performance testing and data analysis The overall performance data of each embodiment and comparative example are summarized in Table 2.

[0093] Table 2 Performance Comparison of Examples and Comparative Examples A comparison of Comparative Example 1 with Examples 1-3 shows that the traditional batch process, employing low-temperature heterogeneous reaction and deep cooling single-stage crystallization, achieves a single-stage crystallization yield of only 7.8%, far lower than the 11.7%-12.3% of the embodiments of this invention. The fundamental reason for this difference is: On the one hand, traditional processes use a large amount of anhydrous hydrogen fluoride (molar ratio 1:60) as a solvent, and the amount of sodium hexafluorophosphate precipitated in dilute solutions is very limited; On the other hand, although the temperature is lower when the temperature is lowered to -30℃, as can be seen from the solubility data in Table 1, the range below 20℃ is a region with a low solubility slope. The amount of sodium hexafluorophosphate that can be precipitated by continuing to cool is limited, and a large amount of cooling energy is required, resulting in an energy consumption of up to 5.2 kWh / kg.

[0094] Furthermore, the traditional process has a D90 of 210 μm and uneven particle size distribution, indicating a lack of effective nucleation control methods.

[0095] This invention significantly improves synthesis efficiency and reduces HF usage through supercritical homogeneous reaction, and precisely matches the high solubility slope region for gradient crystallization, achieving comprehensive optimization in all dimensions of yield, purity, energy consumption, and crystal form.

[0096] A horizontal comparison between Examples 1 to 3 shows that: As the reaction temperature and pressure increased and the amount of catalyst increased, the conversion rate of phosphorus pentafluoride gradually improved, and the product purity also gradually improved. The yield of primary crystallization increased from 11.7% to 12.3%.

[0097] Example 2 achieves the best balance between overall production capacity, energy consumption, and product quality: purity 99.97%, D90 98μm, and energy consumption 4.2kWh / kg. Although Example 3 has the highest purity, its D90 is only 56μm, resulting in a finer powder that may lead to poor flowability in actual use. Example 1 has the lowest energy consumption, but its D90 is 142μm, indicating slightly coarser grains.

[0098] Comparing Comparative Example 2 with Example 2, it can be seen that without the addition of silane catalysts, the product purity decreased from 99.97% to 99.62%, and the primary crystallization yield decreased from 12.2% to 10.5%. The main reason is that the reaction time of the raw materials in the pipeline reactor is only 20 seconds, which is insufficient to achieve complete conversion of phosphorus pentafluoride without the assistance of catalysts. The residual unreacted sodium fluoride and / or phosphorus pentafluoride are encapsulated inside the crystals after entering the crystallization process, becoming impurities and resulting in a decrease in purity.

[0099] Comparing Comparative Example 3 with Example 2, it can be seen that although rapid cooling to 0°C resulted in a single crystallization yield of 14.8%, the purity was only 99.55%, the D90 was as low as 22 μm, and the energy consumption was as high as 5.8 kWh / kg. The main reason is that the operating pressure is lower than the saturated vapor pressure of anhydrous hydrogen fluoride at 20°C, which leads to solvent flash evaporation, bubble disturbance of the crystal surface, rough crystal surface, and increased impurity inclusion rate; at the same time, excessive supersaturation causes explosive nucleation, producing a large amount of ultrafine powder with extremely poor flowability.

[0100] Comparing Example 4 with Example 2, it can be seen that after replacing the Oslo crystallizer with a conventional stirred crystallizer, the primary crystallization yield and purity are similar to those of Example 2, but D90 increases from 98 μm to 235 μm, and fine crystal entrainment is observed. The main reason is that the conventional stirred crystallizer lacks a fluidization mechanism for particle size classification, resulting in the mixed growth of large and fine crystals. Fine crystals adhere to the surface of large crystals to form aggregates, leading to a wider particle size distribution.

[0101] Comparing Comparative Example 5 with Example 2, it can be seen that omitting the reaction stabilization step reduced the primary crystallization yield from 12.2% to 11.5%, and the purity from 99.97% to 99.70%, with a batch-to-batch D90 standard deviation of ±35 μm. The unavoidable feed fluctuations during pipeline reactor operation, without buffering and homogenization in the stirred tank, are directly transmitted to the crystallization process, causing periodic disturbances in crystallization conditions and leading to a decrease in product quality consistency. Therefore, the reaction stabilization step is a necessary step to ensure batch-to-batch product quality stability.

[0102] The embodiments described in this specific implementation are preferred embodiments of this application and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made to the structure, shape, and principle of this application should be covered within the scope of protection of this application.

Claims

1. A method for preparing sodium hexafluorophosphate, characterized in that, Includes the following steps: S1. Phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride are mixed, and a silane catalyst is added under supercritical anhydrous hydrogen fluoride conditions to carry out a homogeneous synthesis reaction to obtain a primary reaction solution containing sodium hexafluorophosphate; wherein, the silane catalyst is trimethylfluorosilane and / or triethylfluorosilane. S2. The primary reaction solution is subjected to a reaction stabilization treatment to obtain a stable reaction solution; S3. After precooling the stable reaction liquid, a two-stage gradient cooling crystallization is performed, and a gradient depressurization is performed simultaneously to obtain a crystallization slurry containing sodium hexafluorophosphate crystals; wherein, the two-stage gradient cooling crystallization includes a first-stage cooling crystallization and a second-stage cooling crystallization; the temperature of the first-stage cooling crystallization is 50-52℃, and the pressure is reduced to 0.72-0.75MPa; the temperature of the second-stage cooling crystallization is 20-22℃, and the pressure is reduced to 0.11-0.20MPa. S4. The crystallization slurry is subjected to solid-liquid separation. The sodium hexafluorophosphate crystals obtained by separation are washed and dried to obtain sodium hexafluorophosphate product. The mother liquor obtained by separation is recycled to step S1. The molar ratio of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride is 1.05-1.1:1:22-24; The reaction temperature for the homogeneous synthesis reaction was set to 190–220 °C, and the reaction pressure was set to 7.0–9.0 MPa.

2. The preparation method according to claim 1, characterized in that, In step S3, before the stable reaction solution undergoes two-stage gradient cooling crystallization, the stable reaction solution is pre-cooled to 60-65°C.

3. The preparation method according to claim 2, characterized in that, In step S3, the stable reaction solution is pre-cooled to 60-65°C, including the following steps: The stable reaction liquid is heated by exchanging heat with phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride, so that the stable reaction liquid is cooled to 70-80°C, and phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride are preheated to 120-150°C. The stable reaction liquid is cooled by exchanging heat with cooling water, so that the stable reaction liquid is cooled to 60-65℃.

4. The preparation method according to claim 1, characterized in that, In step S1, the reaction time of the homogeneous synthesis reaction is set to 15–30 s.

5. The preparation method according to claim 1, characterized in that, In step S1, the amount of the silane catalyst added is 0.1% to 0.5% of the total mass of phosphorus pentafluoride, sodium fluoride and anhydrous hydrogen fluoride.

6. The preparation method according to claim 1, characterized in that, In step S2, the phase stabilization treatment of the reaction includes: The primary reaction solution is stirred at a speed of 150–300 r / min for 5–15 min.

7. The preparation method according to claim 1, characterized in that, In step S4, the sodium hexafluorophosphate crystals are washed with anhydrous hydrogen fluoride 2 to 3 times; and / or In step S4, the drying temperature is 100-110℃, the drying time is 8-10h, and the vacuum degree is -0.09--0.1MPa.

Citation Information

Patent Citations

  • Synthetic method of hexafluorophosphate

    CN114132912A

  • Preparation method of high-purity sodium hexafluorophosphate

    CN119100421A