A high-strength alloy wire and its preparation method

By combining semi-solid shear stirring, pulsed current and PLD technology, the contradiction between the strength and conductivity of alloy wires has been resolved, and high-strength, high-conductivity alloy wires have been prepared to meet the needs of large-capacity power systems.

CN122889520BActive Publication Date: 2026-11-17江苏华旺新材料有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611364885.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17
Estimated Expiration
2046-09-04

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve a balance between strength and conductivity when preparing alloy conductors. Traditional conductor materials have limitations in strength, conductivity, and heat resistance, making it difficult to meet the demands of high-capacity, long-distance, and high-reliability power systems.

Method used

High-strength alloy wires are prepared by combining semi-solid shear stirring, pulsed current, high-current pulsed low-energy electron beam and physical vapor deposition (PLD) technologies. The process includes aluminum liquid refining, homogenization treatment, rolling, drawing and surface composite conductive layer deposition, which improves the strength and conductivity of the alloy wires.

Benefits of technology

It achieves a balance between high strength and high conductivity, reduces the number of transmission lines and construction costs, and enhances the economic value of the power system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a high-strength alloy wire and its preparation method, relating to the field of wire technology. The invention first reduces the segregation of aluminum components in the molten aluminum by bottom-blowing refining combined with magnetic coupling stirring, initially improving the alloy's conductivity. Subsequently, during the solidification process of the molten aluminum, semi-solid shear stirring is combined to achieve a grain refinement strengthening effect. During the warm rolling of the formed billet, pulsed current is applied to achieve a dislocation strengthening effect, thus doubly improving the wire's strength. Then, the alloy surface is irradiated with a high-current pulsed low-energy electron beam, which facilitates the formation of a nanoscale grain layer and nano-pits on the surface, improving the adhesion to the subsequent copper layer. Finally, a composite conductive layer is deposited on the alloy surface using a PLD method. This composite conductive layer possesses excellent conductivity while also acting as a physical barrier to effectively protect the internal alloy. The high-strength alloy wire prepared by this invention exhibits both high strength and high conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of conductor technology, specifically to a high-strength alloy conductor and its preparation method. Background Technology

[0002] As power systems develop towards larger capacity, longer distances, and higher reliability, the limitations of traditional conductor materials are becoming increasingly apparent. They struggle to balance strength, conductivity, and heat resistance. For example, ordinary aluminum conductors have low strength, while copper conductors are expensive and scarce. To overcome this bottleneck, materials scientists have developed high-strength aluminum alloy and copper alloy conductors through alloying and process optimization. Through alloying design, base metals such as aluminum and copper are combined with alloying elements such as magnesium, silicon, zirconium, and scandium. Combined with advanced manufacturing processes such as heat treatment, rapid solidification, and hot deformation, the performance of alloy conductors has been further optimized, giving them broad application prospects in ultra-high voltage power transmission, electrified railways, aerospace, and other fields.

[0003] In the fabrication of alloy conductors, increasing strength often comes at the cost of decreasing conductivity, making it difficult to achieve a balance between the two. Therefore, fabricating conductors that combine both strength and conductivity is crucial. This paper addresses the contradiction between conductor strength and conductivity by coating the internal alloy material with a high-hardness composite conductive layer. A robust physical barrier is formed on the outside of the alloy material through a rational deposition process. Furthermore, reducing component segregation during alloy fabrication combined with grain strengthening techniques enhances the strength of the alloy material, solving the problems inherent in traditional conductive materials. This reduces the number of transmission lines and construction costs, bringing greater economic value to power companies and society. Summary of the Invention

[0004] The purpose of this invention is to provide a high-strength alloy wire and its preparation method to solve the problems existing in the prior art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a high-strength alloy wire, comprising the following preparation steps: (1) Add aluminum ingots to a medium-frequency induction furnace and melt them at 700-710℃ for 15-25 minutes. Add aluminum-manganese alloy ingots, aluminum-copper alloy ingots, magnesium ingots, and aluminum-zinc alloy ingots. Raise the temperature to 735-745℃. Purge the aluminum alloy melt with refining gas from the bottom of the furnace and turn on the magnetic coupling stirring device to stir at a frequency of 6Hz for 15-20 minutes. Then remove the slag to obtain aluminum liquid. (2) Transfer the aluminum liquid into a mixing agitator and use orthogonal blades for semi-solid shearing and stirring for 30-40 minutes. Then transfer it into a preheated mold and homogenize it in a box-type resistance furnace at 410-430℃ for 4-6 hours. Then send it into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, apply a vertical pulse current and simultaneously turn on the warm roll device to heat the roll. When the temperature reaches 230-250℃, start rolling. The rolling deformation is 70-80% of the total processing rate. Roll in 5 passes on average and then naturally age to obtain aluminum alloy bars. (3) Fix the aluminum alloy rod on the cold drawing machine and draw it 9-11 times at a speed of 20m / min. After taking it out, perform artificial aging. After completion, an aluminum alloy wire with a diameter of 2.8-3mm is obtained. Irradiate the aluminum alloy wire with a high current pulsed low energy electron beam. Pulse 10-20 times at a target distance of 8cm. Then deposit a 20-30μm copper layer through PLD, followed by a 30-40μm titanium nitride layer. After deposition, an alloy wire with a diameter of 2.9-3.1mm is obtained.

[0006] Furthermore, the aluminum liquid in step (1) contains the following elements by weight percentage: Mn: 0.94-1.19%, Cu: 0.48-0.62%, Mg: 1.26-1.46%, Zn: 0.63-0.75%, with the balance being Al.

[0007] Furthermore, the specific operation of purging and refining in step (1) is as follows: argon gas is introduced from the bottom of the furnace at a flow rate of 4-8 L / min.

[0008] Furthermore, in step (2), the preheated mold is heated to 500°C, has a diameter of 30mm, and a height of 100mm.

[0009] Furthermore, the pulse parameters of the pulse current in step (2) are: current 150A, frequency 50Hz.

[0010] Furthermore, the specific operation of natural aging in step (2) is to keep it at room temperature for 48 hours.

[0011] Furthermore, the diameter of the aluminum alloy rod in step (2) is 1.3-1.6 cm.

[0012] Furthermore, the specific operation of artificial aging in step (3) is to maintain it at 180℃ for 9 hours.

[0013] Furthermore, in step (3), the energy of the high-current pulsed low-energy electron beam is 20keV and the pulse width is 3μs.

[0014] Furthermore, the specific operational steps for PLD deposition in step (3) are as follows: A molecular pump is used to evacuate the vacuum to 4 × 10⁻⁶.- 4 Pa, using a high-purity copper target as the copper source, with a wavelength of 308 nm, a pulse width of 20 ns, and an energy of 2 J / cm. 2 Laser deposition was performed; then, using a high-purity titanium nitride target as the titanium nitride source, a laser deposition was performed with a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 Laser deposition.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: This invention utilizes semi-solid shear stirring and pulsed current to improve the strength of aluminum alloys, and uses high-current pulsed low-energy electron beam combined with PLD deposition of composite conductive layer to improve the conductivity of wires. The prepared wires have the effect of high strength and high conductivity.

[0016] First, argon gas is introduced into the melt for refining. Impurities in the melt are removed by bottom blowing refining combined with magnetic coupling stirring, and a flow field effect is generated in the melt. The diffusion of gas promotes full mixing of the melt, reduces component segregation, and initially improves the conductivity of the alloy. Subsequently, semi-solid shear stirring is combined during the solidification of aluminum liquid. The shearing action can further inhibit grain growth and achieve a fine grain strengthening effect. When the formed billet is warm rolled, pulsed current is applied to reduce micropores and crack defects during the warm rolling process and achieve a dislocation strengthening effect, thus improving the strength of the conductor in two dimensions.

[0017] Finally, the alloy surface is irradiated with a high-current pulsed low-energy electron beam. On the one hand, the energy of the electron beam can instantly melt the alloy surface and then rapidly cool it under the action of the cold substrate, which is conducive to the formation of a nanoscale grain layer, thereby improving the surface strength of the alloy. On the other hand, the bombardment of the electron beam will form nano-pits on the surface, which will enhance the bonding force with the subsequent copper layer. A copper layer is first deposited on the alloy surface by PLD and then a titanium nitride layer is deposited. The copper can produce a mechanical interlocking effect with the alloy surface, tightly bonded to the substrate and alleviate the phenomenon of large difference in thermal expansion coefficient between the substrate and titanium nitride. Titanium nitride has excellent conductivity and can also act as a physical barrier to effectively protect the internal alloy, further enhancing the conductivity and strength of the wire. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] To more clearly illustrate the method provided by the present invention, the following embodiments are provided for detailed explanation. The testing methods for various properties of a high-strength alloy wire produced in the following embodiments are as follows: Tensile strength: Refer to GB / T228.1-2010 "Metallic materials, tensile testing - Part 1: Test at room temperature", cut an alloy wire with a length of 25cm, use the universal testing machine clamp to hold both ends of the specimen, stretch it at a tensile rate of 10mm / min until the specimen breaks, and calculate its tensile strength based on the maximum load and cross-sectional area. Elongation at break: Refer to GB / T228.1-2010 "Metallic materials, tensile testing - Part 1: Test at room temperature", cut an alloy wire with a length of 25cm, use the universal testing machine clamp to hold both ends of the specimen, stretch at a tensile rate of 10mm / min until the specimen breaks, and calculate the total elongation at break. Electrical conductivity: Referring to the standard GB / T3048.2-2007 "Test methods for electrical properties of wires and cables - Part 2: Test for resistivity of metallic materials", the sample was placed in a constant temperature room at 20℃ for 4 hours, and the resistance value of the wire was measured using a QJ36S-2 DC low resistance tester. The conductivity was calculated using international annealed copper as the standard.

[0020] Example 1; (1) Add aluminum ingots to a medium-frequency induction furnace and melt at 700°C for 15 min. Add aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence. Heat to 735°C and purge and refine the melt by introducing argon gas from the bottom of the furnace at a rate of 4 L / min. At the same time, turn on the magnetic coupling stirring device and stir at a frequency of 6 Hz for 15 min. After standing for 10 min, use a vacuum slag removal device to remove the surface slag and obtain aluminum liquid. The aluminum liquid contains the following elements by weight percentage: Mn: 0.94%, Cu: 0.48%, Mg: 1.26%, Zn: 0.63%, with the balance being Al. (2) The aluminum liquid is transferred into a mixing mixer and stirred for 30 minutes at a speed of 800 rpm and a stirring temperature of 590°C using orthogonal blades. Then it is transferred into a mold preheated to 500°C with a diameter of 30 mm and a height of 100 mm. It is homogenized in a box-type resistance furnace at 410°C for 4 hours. Then it is sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current of 150 A and a frequency of 50 Hz is applied. At the same time, the warm roll device is turned on to heat the roll. When the temperature reaches 230°C, rolling begins. The rolling deformation is 75% of the total processing rate. It is rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm is obtained. (3) The mechanically polished aluminum alloy rod was fixed on a cold drawing machine and drawn at a speed of 20 m / min. It was drawn 10 times with a compression of 15%. After each 2-drawing, it was annealed at 350℃ for 2 hours. After the drawing was completed, it was artificially aged at 180℃ for 9 hours to obtain an aluminum alloy wire with a diameter of 2.9 mm. The aluminum alloy wire was irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The pulses were applied 10 times at a target distance of 8 cm. The wire was then placed on a PLD deposition stage and the cavity was evacuated to 4 × 10⁻⁶ m / min using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm.

[0021] Example 2; (1) Add aluminum ingots to a medium-frequency induction furnace and melt at 700°C for 20 min. Add aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence. Heat to 735°C and purge and refine the melt by introducing argon gas from the bottom of the furnace at a rate of 5 L / min. At the same time, turn on the magnetic coupling stirring device and stir at a frequency of 6 Hz for 18 min. After standing for 10 min, use a vacuum slag removal device to remove the surface slag and obtain aluminum liquid. The aluminum liquid contains the following elements by weight percentage: Mn: 1%, Cu: 0.52%, Mg: 1.31%, Zn: 0.66%, with the balance being Al. (2) The aluminum liquid was transferred into a mixing mixer and stirred for 35 minutes at a speed of 800 rpm and a stirring temperature of 600℃ using orthogonal blades. Then it was transferred into a mold preheated to 500℃ with a diameter of 30 mm and a height of 100 mm. It was homogenized in a box-type resistance furnace at 415℃ for 4.5 hours. Then it was sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current of 150A and a frequency of 50Hz was applied. At the same time, the warm roll device was turned on to heat the roll. When the temperature reached 235℃, rolling began. The rolling deformation was 75% of the total processing rate. It was rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm was obtained. (3) The mechanically polished aluminum alloy rod was fixed on a cold drawing machine and drawn at a speed of 20 m / min. It was drawn 10 times with a compression of 15%. After each two-time drawing, it was annealed at 350℃ for 2 hours. After the drawing was completed, it was artificially aged at 180℃ for 9 hours to obtain an aluminum alloy wire with a diameter of 2.9 mm. The aluminum alloy wire was irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The beam was pulsed 12 times at a target distance of 8 cm. Then it was placed on a PLD deposition stage and the cavity was evacuated to 4 × 10⁻⁶ m / min using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm.

[0022] Example 3; (1) Add aluminum ingots to a medium-frequency induction furnace and melt at 705°C for 20 min. Add aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence. Heat to 740°C and purge and refine the melt by introducing argon gas from the bottom of the furnace at a rate of 6 L / min. At the same time, turn on the magnetic coupling stirring device and stir at a frequency of 6 Hz for 18 min. After standing for 10 min, use a vacuum slag removal device to remove the surface slag and obtain aluminum liquid. The aluminum liquid contains the following elements by weight percentage: Mn: 1.06%, Cu: 0.55%, Mg: 1.36%, Zn: 0.7%, with the balance being Al. (2) The aluminum liquid is transferred into a mixing mixer and stirred for 35 minutes at a speed of 800 rpm and a stirring temperature of 605℃ using orthogonal blades. Then it is transferred into a mold preheated to 500℃ with a diameter of 30 mm and a height of 100 mm. It is homogenized in a box-type resistance furnace at 420℃ for 5 hours. Then it is sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current of 150A and a frequency of 50Hz is applied. At the same time, the warm roll device is turned on to heat the roll. When the temperature reaches 240℃, rolling begins. The rolling deformation is 75% of the total processing rate. It is rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm is obtained. (3) The mechanically polished aluminum alloy rod was fixed on a cold drawing machine and drawn at a speed of 20 m / min. It was drawn 10 times with a compression of 15%. After each 2-drawing, it was annealed at 350℃ for 2 hours. After the drawing was completed, it was artificially aged at 180℃ for 9 hours to obtain an aluminum alloy wire with a diameter of 2.9 mm. The aluminum alloy wire was irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The beam was pulsed 15 times at a target distance of 8 cm. Then it was placed on a PLD deposition stage and the cavity was evacuated to 4 × 10⁻⁶ m / min using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm.

[0023] Example 4; (1) Add aluminum ingots to a medium-frequency induction furnace and melt at 705°C for 25 min. Add aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence. Heat to 740°C and purge and refine the melt by introducing argon gas from the bottom of the furnace at a rate of 7 L / min. At the same time, turn on the magnetic coupling stirring device and stir at a frequency of 6 Hz for 18 min. After standing for 10 min, use a vacuum slag removal device to remove the surface slag and obtain aluminum liquid. The aluminum liquid contains the following elements by weight percentage: Mn: 1.013%, Cu: 0.58%, Mg: 1.41%, Zn: 0.73%, with the balance being Al. (2) The aluminum liquid was transferred into a mixing mixer and stirred for 35 minutes at a speed of 800 rpm and a stirring temperature of 615℃ using orthogonal blades. Then it was transferred into a mold preheated to 500℃ with a diameter of 30 mm and a height of 100 mm. It was homogenized in a box-type resistance furnace at 425℃ for 5.5 hours. Then it was sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current of 150A and a frequency of 50Hz was applied. At the same time, the warm roll device was turned on to heat the roll. When the temperature reached 245℃, rolling began. The rolling deformation was 75% of the total processing rate. It was rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm was obtained. (3) The mechanically polished aluminum alloy rod was fixed on a cold drawing machine and drawn at a speed of 20 m / min. It was drawn 10 times with a compression of 15%. After each 2-drawing, it was annealed at 350℃ for 2 hours. After the drawing was completed, it was artificially aged at 180℃ for 9 hours to obtain an aluminum alloy wire with a diameter of 2.9 mm. The aluminum alloy wire was irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The beam was pulsed 18 times at a target distance of 8 cm. Then it was placed on a PLD deposition stage and the cavity was evacuated to 4 × 10⁻⁶ m / min using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm.

[0024] Example 5; (1) Add aluminum ingots to a medium-frequency induction furnace and melt at 710°C for 25 min. Add aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence. Heat to 745°C and purge and refine the melt by introducing argon gas from the bottom of the furnace at a rate of 8 L / min. At the same time, turn on the magnetic coupling stirring device and stir at a frequency of 6 Hz for 20 min. After standing for 10 min, use a vacuum slag removal device to remove the surface slag and obtain aluminum liquid. The aluminum liquid contains the following elements by weight percentage: Mn: 1.19%, Cu: 0.62%, Mg: 1.46%, Zn: 0.75%, with the balance being Al. (2) The aluminum liquid is transferred into a mixing mixer and stirred for 40 minutes at a speed of 800 rpm and a stirring temperature of 620°C using orthogonal blades. Then it is transferred into a mold preheated to 500°C with a diameter of 30 mm and a height of 100 mm. It is homogenized in a box-type resistance furnace at 430°C for 6 hours. Then it is sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current of 150 A and a frequency of 50 Hz is applied. At the same time, the warm roll device is turned on to heat the roll. When the temperature reaches 250°C, rolling begins. The rolling deformation is 75% of the total processing rate. It is rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm is obtained. (3) The mechanically polished aluminum alloy rod was fixed on a cold drawing machine and drawn at a speed of 20 m / min. It was drawn 10 times with a compression of 15%. After each two-time drawing, it was annealed at 350℃ for 2 hours. After the drawing was completed, it was artificially aged at 180℃ for 9 hours to obtain an aluminum alloy wire with a diameter of 2.9 mm. The aluminum alloy wire was irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The pulses were applied 20 times at a target distance of 8 cm. The wire was then placed on a PLD deposition stage and the cavity was evacuated to 4 × 10⁻⁶ m / min using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm.

[0025] Comparative Example 1; The difference between Comparative Example 1 and Example 3 is that step (1) is different. Step (1) is changed to: adding aluminum ingots into a medium frequency induction furnace and melting at 705°C for 20 min, then adding aluminum manganese alloy ingots, aluminum copper alloy ingots, magnesium ingots, and aluminum zinc alloy ingots in sequence, heating to 740°C and reacting for 20 min to obtain aluminum liquid; the aluminum liquid contains the following elements by weight percentage: Mn: 1.06%, Cu: 0.55%, Mg: 1.36%, Zn: 1.36%, with the balance being Al; the remaining steps are the same as in Example 2.

[0026] Comparative Example 2; The difference between Comparative Example 2 and Example 3 is that step (2) is different. Step (2) is changed to: the aluminum liquid is transferred into a mold with a diameter of 30 mm and a height of 100 mm that is preheated to 500°C, and homogenized in a box-type resistance furnace at 420°C for 5 hours. Then it is sent into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, a vertical pulse current with a current of 150 A and a frequency of 50 Hz is applied. At the same time, the warm roll device is turned on to heat the roll. When the temperature reaches 240°C, rolling begins. The rolling deformation is 75% of the total processing rate. It is rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm is obtained. The remaining steps are the same as in Example 2.

[0027] Comparative Example 3; The difference between Comparative Example 3 and Example 3 is that step (2) is different. Step (2) is changed to: the aluminum liquid is transferred into a mixing stirrer and stirred for 35 minutes at a speed of 800 rpm and a stirring temperature of 605°C using orthogonal blades. Then it is transferred into a mold preheated to 500°C with a diameter of 30 mm and a height of 100 mm. It is homogenized in a box-type resistance furnace at 420°C for 5 hours. Then it is sent into a rolling forming device. The warm roll device is turned on to heat the roll. When the temperature reaches 240°C, rolling begins. The rolling deformation is 75% of the total processing rate. It is rolled in 5 passes on average. After natural aging at room temperature for 48 hours, an aluminum alloy bar with a diameter of 1.5 cm is obtained. The remaining steps are the same as in Example 2.

[0028] Comparative Example 4; The difference between Comparative Example 4 and Example 3 is that step (3) is different. Step (3) is changed to: fixing the mechanically polished aluminum alloy rod on a cold drawing machine, drawing it at a speed of 20 m / min, drawing it 10 times with a compression of 15%, and performing intermediate annealing at 350°C for 2 hours after each 2-drawing. After drawing, artificially aging it at 180°C for 9 hours, and then obtaining an aluminum alloy wire with a diameter of 2.9 mm; ultrasonically cleaning the aluminum alloy wire at a frequency of 30 Hz for 10 minutes, purging the surface with nitrogen for 5 minutes, and then placing it on a deposition stage. The cavity is evacuated to 4 × 10 using a molecular pump. -4 Pa, using a wavelength of 308nm, a pulse width of 20ns, and an energy of 2J / cm. 2 After 5 minutes of laser pre-sputtering, a 25 μm copper layer was deposited. The target was then replaced with a high-purity titanium nitride target, using a wavelength of 248 nm, a pulse width of 30 ns, and an energy of 280 mJ / cm². 2 After laser pre-sputtering for 5 minutes, deposition was performed to obtain an alloy wire with a diameter of 3 mm; the remaining steps were the same as in Example 2.

[0029] Comparative Example 5; The difference between Comparative Example 5 and Example 3 is that step (3) is different. Step (3) is changed to: fixing the mechanically polished aluminum alloy rod on a cold drawing machine and drawing it at a speed of 20 m / min. It is drawn 10 times with a compression of 15%. After each 2-time drawing, it is annealed at 350°C for 2 hours. After the drawing is completed, it is artificially aged at 180°C for 9 hours. It is then irradiated with a high-current pulsed low-energy electron beam with an energy of 20 keV and a pulse width of 3 μs. The beam is pulsed 15 times at a target distance of 8 cm. Then, an aluminum alloy wire with a diameter of 2.9 mm is obtained. The remaining steps are the same as in Example 2.

[0030] Example of effect Table 1 below shows the performance analysis results of a high-strength alloy wire using Examples 1 to 5 and Comparative Examples 1 to 5 of the present invention.

[0031]

[0032] A comparison of the tensile strength experimental data from the examples and comparative examples reveals that the present invention, by combining semi-solid shear stirring during the gradual solidification of molten aluminum, can mechanically break up the solidified or partially solidified grains, making them finer and achieving a fine-grain strengthening effect, thus initially improving the strength of the alloy. Subsequently, when the formed billet is warm-rolled, pulsed current is applied. When the pulsed current passes through the material, it can reduce the dislocation density, drive dislocation slip and rearrangement, promote the regular ordering of dislocations, and hinder subsequent dislocation movement, thus achieving a dislocation strengthening effect. This dual-dimensionally improves the strength of the aluminum alloy. The surface of the alloy is irradiated with a high-current pulsed low-energy electron beam. The energy of the electron beam can instantly melt the alloy surface, which is then rapidly cooled under the action of a cold substrate, which is conducive to the formation of nanoparticles on the surface. The invention improves the surface strength of the alloy by creating a fine grain layer. A comparison of the experimental data on elongation at break between the examples and comparative examples reveals that the present invention enhances the elongation at break of the alloy wire through the combined strengthening effects of fine grain reinforcement and dislocation reinforcement. A comparison of the experimental data on conductivity between the examples and comparative examples reveals that the present invention utilizes bottom-blowing refining combined with magnetic coupling stirring to remove impurities from the aluminum alloy melt and generate a flow field effect in the melt. Gas diffusion promotes thorough mixing of the melt, reduces component segregation, and initially improves the alloy conductivity. Irradiation of the alloy surface with a high-current pulsed low-energy electron beam reduces the resistivity of the contact surface. Then, a composite conductive layer is deposited using PLD. The presence of the copper layer and the titanium nitride layer synergistically improves the conductivity of the wire.

[0033] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.

Claims

1. A high-strength alloy wire, characterized in that, The preparation steps include the following: (1) Add aluminum ingots to a medium-frequency induction furnace and melt them at 700-710℃ for 15-25 minutes. Add aluminum-manganese alloy ingots, aluminum-copper alloy ingots, magnesium ingots, and aluminum-zinc alloy ingots. Raise the temperature to 735-745℃. Purge the aluminum alloy melt with refining gas from the bottom of the furnace and turn on the magnetic coupling stirring device to stir at a frequency of 6Hz for 15-20 minutes. Then remove the slag to obtain aluminum liquid. (2) Transfer the aluminum liquid into a mixing agitator and use orthogonal blades for semi-solid shearing and stirring for 30-40 minutes. Then transfer it into a preheated mold and homogenize it in a box-type resistance furnace at 410-430℃ for 4-6 hours. Then send it into a semi-enclosed protective cover equipped with a pulse current assisted rolling forming device. Under nitrogen protection, apply a vertical pulse current and simultaneously turn on the warm roll device to heat the roll. When the temperature reaches 230-250℃, start rolling. The rolling deformation is 70-80% of the total processing rate. Roll in 5 passes on average and then naturally age to obtain aluminum alloy bars. (3) Fix the aluminum alloy rod on the cold drawing machine and draw it 9-11 times at a speed of 20m / min. After taking it out, perform artificial aging. After completion, an aluminum alloy wire with a diameter of 2.8-3mm is obtained. Irradiate the aluminum alloy wire with a high current pulsed low energy electron beam. Pulse 10-20 times at a target distance of 8cm. Then deposit a 20-30μm copper layer through PLD, followed by a 30-40μm titanium nitride layer. After deposition, an alloy wire with a diameter of 2.9-3.1mm is obtained.

2. The high-strength alloy wire according to claim 1, characterized in that, The aluminum liquid in step (1) contains the following elements by weight percentage: Mn: 0.94-1.19%, Cu: 0.48-0.62%, Mg: 1.26-1.46%, Zn: 0.63-0.75%, with the balance being Al.

3. The high-strength alloy wire according to claim 1, characterized in that, The specific operation of purging and refining in step (1) is as follows: Argon gas is introduced from the bottom of the furnace at a flow rate of 4-8 L / min.

4. The high-strength alloy wire according to claim 1, characterized in that, The temperature of the preheated mold in step (2) is 500℃, the diameter is 30mm and the height is 100mm.

5. A high-strength alloy conductor according to claim 1, characterized in that, The pulse parameters of the pulse current in step (2) are: current 150A, frequency 50Hz.

6. The high-strength alloy conductor according to claim 1, characterized in that, The specific operation of natural aging in step (2) is to keep it at room temperature for 48 hours.

7. A high-strength alloy wire according to claim 1, characterized in that, The diameter of the aluminum alloy rod in step (2) is 1.3-1.6cm.

8. A high-strength alloy wire according to claim 1, characterized in that, The specific operation of artificial aging in step (3) is to maintain it at 180℃ for 9 hours.

9. A high-strength alloy wire according to claim 1, characterized in that, In step (3), the energy of the high-current pulsed low-energy electron beam is 20keV and the pulse width is 3μs.

10. A high-strength alloy wire according to claim 1, characterized in that, The specific operation steps of the PLD deposition in the step (3) are as follows: using a molecular pump to vacuumize to 4×10 -4 Pa, taking high-purity copper target as copper source, using laser deposition with a wavelength of 308nm, a pulse width of 20ns and an energy of 2J / cm 2 ; then taking high-purity titanium nitride target as titanium nitride source, using laser deposition with a wavelength of 248nm, a pulse width of 30ns and an energy of 280mJ / cm 2 .

Citation Information

Patent Citations

  • Continuous semisolid extrusion forming method for preparing high-strength aluminum alloy lead

    CN102856009A

  • High-strength and high-conductivity aluminum alloy electrical conductor material and preparation method thereof

    CN121344432A