White mud-mediated uiO-66-nh2-sodium alginate composite aerogel, preparation method and application thereof
The preparation method of UiO-66-NH2-sodium alginate composite aerogel mediated by white mud solves the problems of agglomeration and uneven cross-linking of UiO-66-NH2 powder, realizes efficient adsorption of Cd(II) and resource utilization of solid waste, improves adsorption performance and mechanical strength, and is easy to recycle and regenerate.
Patent Information
- Application Number
- CN202611587017.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, UiO-66-NH2 micro-nano powders tend to agglomerate in aqueous phases, resulting in a reduction of effective adsorption sites. The heterogeneous structure of the sodium alginate matrix formed by traditional cross-linking methods hinders the diffusion of heavy metal ions, and there is a lack of effective solutions for the resource utilization of solid waste.
A method mediated by white clay was adopted, in-situ growth of UiO-66-NH2 on the surface of white clay powder was achieved through solvothermal reaction. The calcium carbonate ions released from the white clay were cross-linked with sodium alginate to form a uniform composite aerogel structure. The white clay also served as an in-situ growth carrier and calcium source for MOF, realizing endogenous cross-linking.
It improves adsorption performance and mass transfer efficiency, enhances mechanical strength, achieves efficient adsorption of Cd(II), facilitates solid-liquid separation and recycling, and realizes the resource utilization of industrial solid waste.
Smart Images

Figure CN123059627A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of water treatment and environmental functional materials technology, specifically relating to a mud-mediated UiO-66-NH2-sodium alginate composite aerogel, its preparation method, and its application. Background Technology
[0002] Cadmium (Cd) is one of the most toxic heavy metal pollutants, exhibiting bioaccumulation and non-degradability. It can enter the human body through the food chain, and long-term exposure can damage the kidneys, bones, and respiratory system. With the rapid development of industries such as electroplating, metallurgy, batteries, and printing and dyeing, cadmium-containing wastewater has become a prominent environmental problem urgently needing treatment. Among existing water treatment technologies, adsorption is widely considered one of the most promising methods for engineering applications due to its simple operation, low energy consumption, wide applicable concentration range, and low likelihood of secondary pollution. The key lies in developing adsorption materials with high adsorption capacity, good stability, and easy regeneration.
[0003] Metal-organic frameworks (MOFs) have attracted widespread attention due to their ultra-high specific surface area, tunable pore size, and abundant functional sites. Among them, UiO-66-NH2 containing amino functional groups not only exhibits excellent water stability, but its amino groups can also selectively adsorb Cd(II) through coordination, chelation, and electrostatic interactions. However, UiO-66-NH2 usually exists in the form of micro- and nano-sized powders, which are prone to aggregation in aqueous phases, leading to a significant reduction in effective adsorption sites.
[0004] To improve the recyclability of powder materials, current technologies often involve loading MOFs onto natural polymer matrices such as sodium alginate (SA) to form gels or aerogels. Sodium alginate molecules contain abundant carboxyl groups, which can react with polyvalent metal ions (such as Ca²⁺, Ca²⁺, and Ca²⁺). 2+ Crosslinking forms a three-dimensional network structure, making it an ideal matrix material for immobilizing powder adsorbents. However, traditional crosslinking processes generally employ external diffusion crosslinking by dripping or injecting sodium alginate solution into a calcium salt solution. This crosslinking mechanism proceeds from the outside in, with calcium ions first coordinating with the carboxyl groups of sodium alginate on the gel surface to form a dense and hard outer shell. The internal crosslinking degree is low, resulting in a heterogeneous structure that is "tight on the outside and loose on the inside," significantly hindering the diffusion and mass transfer of heavy metal ions to the active sites within the material. To address this issue, Chinese patent CN109078588B discloses a composite aerogel that uses a calcium carbonate and D-gluconic acid-δ-lactone (GDL) sustained-release system to achieve endogenous in-situ crosslinking of sodium alginate. However, this scheme uses attapulgite as the main material, does not introduce active adsorbent components such as MOF, and does not address the dispersion and agglomeration inhibition of MOF powder, thus limiting its adsorption capacity. Furthermore, even if analytically pure calcium carbonate is directly used to replace the calcium carbonate component in the above system, its single composition makes it difficult to provide a synergistic enhancement effect on the matrix while simultaneously providing a calcium source.
[0005] On the other hand, the alkali recovery process in the paper industry generates a large amount of white mud solid waste every year, the main component of which is calcium carbonate (CaCO3), and it also contains oxides such as silicon, aluminum, and iron. Currently, most of the white mud is directly landfilled or used in low-end building materials, which not only occupies land resources, but its strong alkalinity may also pollute the soil and groundwater, and there is a lack of high-value-added resource utilization methods.
[0006] In summary, there is currently a lack of a composite aerogel preparation scheme that can effectively disperse and fix MOF active components, achieve uniform cross-linking of sodium alginate matrix, and simultaneously take into account the resource utilization of solid waste. Summary of the Invention
[0007] In view of the above, it is necessary to provide a white mud-mediated UiO-66-NH2-sodium alginate composite aerogel, its preparation method and application. The obtained aerogel has a uniform structure, excellent mass transfer performance and high mechanical strength. The adsorption capacity for Cd(II) reaches 415.6 mg / g, and adsorption equilibrium can be reached within 120 min. It is also easy to separate solid and liquid and recycle, realizing the synergy of industrial solid waste resource utilization and heavy metal pollution control.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a mud-mediated UiO-66-NH2-sodium alginate composite aerogel includes the following steps:
[0010] S1. The white mud produced in the papermaking alkali recovery process is washed, dried and ground to obtain white mud powder.
[0011] S2. The zirconium source and the amino-containing organic ligand are dissolved in an organic solvent, and the white mud powder is added. UiO-66-NH2 is grown in situ on the surface of the white mud powder through a solvothermal reaction. After solid-liquid separation, washing and drying, white mud@UiO-66-NH2 composite powder is obtained.
[0012] S3. The white mud@UiO-66-NH2 composite powder is dispersed in an aqueous solution of sodium alginate, and D-gluconic acid-δ-lactone is added. The mixture is allowed to stand and solidify. The hydrolysis of D-gluconic acid-δ-lactone causes the system to slowly acidify, which promotes the slow release of calcium ions from the calcium carbonate contained in the white mud powder. The calcium ions coordinate and crosslink with the carboxyl groups of sodium alginate to form a composite hydrogel. The calcium ions required to form the composite hydrogel come from the white mud powder itself, and no calcium salt is added during the crosslinking process.
[0013] S4. The composite hydrogel is pre-frozen and then freeze-dried to obtain the mud-mediated UiO-66-NH2-sodium alginate composite aerogel.
[0014] In this invention, further, in step S1, the white mud is washed with water until the supernatant is neutral, dried at 60–100°C for 12–36 hours, ground, and then passed through a 100–300 mesh sieve. (0 mesh sieve)
[0015] In this invention, further, in step S2, the zirconium source is zirconium tetrachloride, the amino-containing organic ligand is 2-aminoterephthalic acid, and the organic solvent is N,N-dimethylformamide; the mass ratio of the zirconium source to the amino-containing organic ligand is 1:(0.6-1.6); 0.5-3.0 g of the white mud powder is added to every 100 mL of the organic solvent; the temperature of the solvothermal reaction is 100-150 °C and the time is 12-36 h; after the reaction is completed, the mixture is washed sequentially with N,N-dimethylformamide and anhydrous ethanol, and then vacuum dried at 50-80 °C for 8-24 h.
[0016] In this invention, further, in step S3, the mass concentration of the sodium alginate aqueous solution is 1-4 wt%; the mass ratio of the white mud@UiO-66-NH2 composite powder to the sodium alginate is 1:(0.5-4); the amount of D-gluconic acid-δ-lactone added is 0.2%-1.0% of the mass of the sodium alginate aqueous solution; and the temperature for static curing is 15-40℃ and the time is 6-36h.
[0017] In this invention, further, in step S4, the pre-freezing temperature is -80 to -20°C and the time is 8 to 24 hours; the freeze-drying vacuum degree is not greater than 20 Pa and the time is 24 to 72 hours.
[0018] This invention also proposes a white mud-mediated MOF / sodium alginate composite aerogel, prepared by any of the above preparation methods; the composite aerogel includes a sodium alginate three-dimensional network framework and white mud@UiO-66-NH2 composite powder dispersed and anchored in the sodium alginate three-dimensional network framework, wherein UiO-66-NH2 in the composite powder is grown in situ on the surface of white mud particles; the white mud powder simultaneously serves as an in-situ growth carrier of UiO-66-NH2 and an endogenous calcium source, the sodium alginate three-dimensional network framework is formed by cross-linking of calcium ions released by the white mud powder itself, and the cross-linking density is uniformly distributed along the radial direction of the composite aerogel.
[0019] In this invention, the composite aerogel is a self-supporting monolithic block with a compressive stress of 0.15 to 0.22 MPa at 50% compressive strain and a maximum Langmuir adsorption capacity of not less than 400 mg / g for Cd(II).
[0020] The present invention also proposes the application of the composite aerogel prepared by the above-described preparation method, or the composite aerogel, in the adsorption and removal of Cd(II) from cadmium-containing wastewater.
[0021] In this invention, the pH of the cadmium-containing wastewater is 4-7, the initial concentration of Cd(II) is 25-500 mg / L, the dosage of the composite aerogel is 0.05-1.0 g / L, and the adsorption temperature is 15-40℃.
[0022] In this invention, the composite aerogel after adsorption saturation is further desorbed and regenerated using a 0.05-0.2 mol / L EDTA solution for a desorption time of 1-5 h; the composite aerogel is reused at least 5 times, and the Cd(II) removal rate in the 5th cycle is not less than 85%.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects.
[0024] 1. Significantly improved adsorption performance and mass transfer efficiency. This invention achieves uniform in-situ crosslinking of sodium alginate from the inside out through the endogenous slow-release of calcium ions from white mud, forming a three-dimensional macroporous / mesoporous network with a uniform radial distribution of crosslinking density. This overcomes the inherent defect of the traditional exogenous crosslinking method, which suffers from a "tight outside and loose inside" structure that limits mass transfer. Under the conditions of an initial Cd(II) concentration of 200 mg / L, a dosage of 0.2 g / L, pH 5.5, and 25℃, the composite aerogel of this invention reaches adsorption equilibrium in 120 min, with an equilibrium adsorption capacity of 415.6 mg / g; while the traditional exogenous CaCl2 crosslinked aerogel of Comparative Example 3 requires 240 min and has an equilibrium adsorption capacity of only 358.6 mg / g. Langmuir fitting results show that the maximum Langmuir adsorption capacity of the composite aerogel of this invention reaches 449.7 mg / g, which is also higher than the 362.8 mg / g of Comparative Example 3. The significant improvement in adsorption rate is due to the unobstructed mass transfer pathway provided by the uniform cross-linked structure, which enables Cd(II) to diffuse rapidly to the active sites inside the material, rather than relying solely on surface adsorption.
[0025] 2. The in-situ growth strategy produces a synergistic enhancement effect. This invention uses papermaking sludge as an in-situ growth carrier for UiO-66-NH2, enabling MOF crystals to grow in situ on the surface of sludge particles. This effectively inhibits the aggregation of MOF nanoparticles and better preserves their microporous structure and high specific surface area advantages. In Example 3, the BET specific surface area of the sludge@UiO-66-NH2 in-situ composite powder reached 763.5 m². 2 / g, significantly higher than that of physically mixed powders with the same MOF content (512.8m). 2 / g). Comparative Example 1 further confirms that the equilibrium adsorption capacity of Cd(II) in the physically mixed aerogel is only 287.6 mg / g, less than 70% of that in this invention (415.6 mg / g). It is understood that the calcium sites on the surface of the white mud particles can pre-coordinate with the carboxyl groups of the organic ligands, providing heterogeneous nucleation centers for UiO-66-NH2, allowing the crystals to grow in a dispersed rather than aggregated form, thereby exposing more amino active sites for Cd(II) coordination chelation.
[0026] 3. Excellent mechanical properties and structural stability. The associated inorganic components in the white mud (such as oxides of silicon, aluminum, and iron) interact with the three-dimensional network of sodium alginate, endowing the composite aerogel with excellent compressive strength and fracture resistance. In Example 5, the compressive stress of the composite aerogel of the present invention at 50% compressive strain reached 0.18 MPa, significantly higher than that of Comparative Example 2 (0.11 MPa) and Comparative Example 3 (0.075 MPa), and it did not break or shed powder under severe water disturbance. Comparative Example 2 further shows that the compressive stress decreased significantly after replacing the white mud with an equal amount of analytically pure calcium carbonate, indicating that the associated inorganic components in the white mud played an additional reinforcing role in the three-dimensional framework, rather than simply acting as a calcium source.
[0027] 4. Easy to engineer and recycle, combining environmental protection and economic benefits. Nano-sized UiO-66-NH2 is firmly anchored within a macroscopic aerogel framework. After adsorption, complete solid-liquid separation can be achieved using tweezers or a filter, overcoming the engineering bottlenecks of traditional MOF powder adsorbents, which are prone to loss, difficult to recycle, and easily cause secondary pollution. Example 6 shows that after 5 adsorption-desorption cycles, the Cd(II) removal rate remains at 87.5%, demonstrating good reusability. Simultaneously, this invention uses recycled white mud from papermaking alkali as both an in-situ growth carrier for MOFs and an endogenous calcium source, eliminating the need for external calcium salts or inert host materials such as attapulgite. This achieves high-value-added resource utilization of industrial solid waste, reduces material costs and the burden of solid waste disposal, and realizes a win-win situation for both environmental protection and economics through "waste-to-waste" treatment. Attached Figure Description
[0028] Figure 1 This is a schematic diagram illustrating the preparation process and endogenous in-situ crosslinking mechanism of the UiO-66-NH2-sodium alginate composite aerogel mediated by white mud in Examples 1 and 2 of the present invention.
[0029] Figure 2 The diagram shows the structural characterization of the white mud, UiO-66-NH2, and white mud@UiO-66-NH2 composite powder in Example 3 of this invention. Figure 2 (a) XRD patterns of white clay, UiO-66-NH2 and white clay@UiO-66-NH2 composite powders; Figure 2(b) shows the FTIR spectra of white mud, UiO-66-NH2 and white mud@UiO-66-NH2 composite powder.
[0030] Figure 3 The diagram shows the pore structure characterization of the white mud@UiO-66-NH2 composite powder in Example 3 of this invention and the physically mixed powder in Comparative Example 1. Figure 3 (a) is the N2 adsorption-desorption isotherm of white mud@UiO-66-NH2 composite powder and physical mixed powder of Comparative Example 1; Figure 3 (b) shows the BJH pore size distribution curves of the white mud@UiO-66-NH2 composite powder and the physically mixed powder of Comparative Example 1.
[0031] Figure 4 This is a schematic diagram comparing the cross-sectional structures of a traditional exogenous CaCl2 cross-linked aerogel and the endogenous in-situ cross-linked aerogel of the present invention in Example 3 of the present invention. Figure 4 (a) is a schematic diagram of the cross-sectional structure of a traditional exogenous CaCl2 cross-linked aerogel; Figure 4 (b) is a schematic diagram of the cross-sectional structure of the in-situ cross-linked aerogel of the white mud of the present invention.
[0032] Figure 5 The graphs show the adsorption kinetics of Cd(II) on different materials in Example 4 of this invention. Figure 5 (a) shows the adsorption kinetics curves of Cd(II) for different materials; Figure 5 (b) shows the pseudo-second-order kinetic linear fit of Cd(II) for different materials.
[0033] Figure 6 This is a comparison chart of Cd(II) adsorption isotherms and adsorption capacities in Example 4 of the present invention. Figure 6 (a) shows the adsorption isotherm of Cd(II) and the Langmuir fitting curve; Figure 6 (b) is a comparison of the maximum adsorption capacity of Langmuir for the four materials.
[0034] Figure 7 This is the curve showing the effect of the initial pH of the solution on the adsorption capacity of Cd(II) in Example 4 of the present invention.
[0035] Figure 8 This is a graph showing the effect of adsorbent dosage on Cd(II) removal rate and adsorption capacity in Example 4 of the present invention.
[0036] Figure 9 The figures show the compressive stress-strain curves of composite aerogels obtained by different crosslinking methods in Example 5 of the present invention.
[0037] Figure 10 This is a performance diagram of the composite aerogel in Example 6 of the present invention after five adsorption-desorption cycles, wherein, Figure 10 (a) is the Cd(II) removal rate of the composite aerogel after five adsorption-desorption cycles; Figure 10 (b) represents the desorption rate of the composite aerogel after five adsorption-desorption cycles.
[0038] Figure 11 This is a diagram showing the selective adsorption results of coexisting metal ions by the composite aerogel in Example 6 of the present invention.
[0039] Figure 12 This is the XPS spectrum of the composite aerogel after Cd(II) adsorption in Example 7 of the present invention, wherein, Figure 12 (a) is the Cd3d XPS spectrum of the composite aerogel after Cd(II) adsorption; Figure 12 (b) is the N1s XPS spectrum of the composite aerogel after Cd(II) adsorption. Detailed Implementation
[0040] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0041] The preparation process and endogenous in-situ crosslinking mechanism of the mud-mediated UiO-66-NH2-sodium alginate composite aerogel in Examples 1 and 2 of this invention are as follows: Figure 1 As shown, the preparation process includes: reacting papermaking sludge particles with MOF precursors via a solvothermal reaction in a high-pressure reactor to obtain MOF-loaded sludge composite particles; adding the obtained composite particles to a sodium alginate solution and adding GDL slow-release acidifier; under the action of GDL, the system is slowly acidified, causing calcium carbonate in the sludge to release Ca2+. 2+ Ca 2+ The aerogel undergoes endogenous in-situ uniform cross-linking with the carboxyl groups of sodium alginate to form an "egg-box" structure; finally, it is freeze-dried to obtain a cylindrical porous aerogel.
[0042] Example 1: White mud pretreatment and preparation of white mud@UiO-66-NH2 composite powder
[0043] (1) White mud pretreatment: Take 500g of dehydrated white mud produced in the papermaking alkali recovery process, wash it repeatedly with deionized water until the supernatant is neutral, dry it in an 80℃ oven for 24h, grind it and pass it through a 200-mesh sieve to obtain purified white mud powder, whose main component is CaCO3, and also contains oxide components such as silicon, aluminum, and iron.
[0044] (2) In-situ synthesis: Weigh 1.0 g of zirconium tetrachloride (ZrCl4) and 1.0 g of 2-aminoterephthalic acid, and dissolve them in 100 mL of N,N-dimethylformamide (DMF). Stir for 30 min until clear. Add 1.5 g of the above purified white mud powder and ultrasonically disperse for 1 h. Transfer the mixture to a 200 mL polytetrafluoroethylene-lined high-pressure reactor and react at 120 °C for 24 h using a solvothermal method. After the reaction is complete, allow it to cool naturally, collect the product by centrifugation, wash it three times each with DMF and anhydrous ethanol, and vacuum dry it at 60 °C for 12 h to obtain white mud@UiO-66-NH2 composite powder, labeled as WM@UiO-66.
[0045] Example 2: Preparation of white mud@UiO-66-NH2-sodium alginate composite aerogel
[0046] (1) Preparation of sodium alginate precursor solution: Dissolve 0.5g sodium alginate (SA) powder in 24.5g deionized water and stir continuously in a 60℃ water bath until completely dissolved to prepare a transparent SA solution with a mass concentration of 2.0 wt%.
[0047] (2) Blending and dispersion: 0.5g of WM@UiO-66 composite powder obtained in Example 1 was added to 25g of SA solution, stirred vigorously for 2h, and then subjected to ultrasonic treatment for 30min to obtain a uniform dispersion.
[0048] (3) In-situ curing: Add 0.1 g D-gluconic acid-δ-lactone (GDL) to the above dispersion, stir rapidly for 5 min, pour into a mold, and seal and let it stand for 24 h at 25℃ for curing. During the curing period, GDL slowly hydrolyzes, acidifying the system and promoting the slow release of Ca from the white mud from the inside out. 2+ Ca 2+ It forms an "egg-box structure" coordination crosslinking with the carboxyl groups of sodium alginate to form a composite hydrogel. No external calcium salt is added during the curing process; the calcium ions required for crosslinking come entirely from the white clay powder itself.
[0049] (4) Freeze-drying: Take out the solidified hydrogel, rinse the surface with deionized water, pre-freeze at -80℃ for 12h, and then transfer it into a freeze dryer and freeze-dry for 48h under a vacuum of less than 10Pa to obtain a self-supporting white mud@UiO-66-NH2-sodium alginate composite aerogel, labeled as WM@UiO-66 / SA.
[0050] Example 3: Characterization of Material Structure and Pore Properties
[0051] The material was characterized by X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FTIR), and N2 adsorption-desorption testing.
[0052] XRD analysis: Figure 2(a) XRD patterns of white clay, UiO-66-NH2, and white clay@UiO-66-NH2 composite powders. White clay exhibits typical calcite-type CaCO3 diffraction peaks (2θ = 23.1°, 29.4°, 36.0°, 39.4°, 43.2°, 47.5°, 48.5°). UiO-66-NH2 exhibits characteristic diffraction peaks at 7.4° and 8.1°. The white clay@UiO-66-NH2 composite powder retains both sets of characteristic peaks, proving that UiO-66-NH2 was successfully grown in situ on the surface of white clay.
[0053] FTIR analysis: Figure 2 (b) is the FTIR spectrum. 3450 cm⁻¹ -1 and 3355cm -1 The peak at 1568 cm⁻¹ represents the stretching vibration peak of amino(NH) groups. -1 and 1386cm -1 The peak at 1422 cm⁻¹ represents the asymmetric / symmetric stretching vibration of the carboxyl group. -1 874cm -1 and 712cm -1 The peak at this point is a characteristic peak of carbonate, further confirming that the composite powder contains both amino MOF and calcium carbonate components.
[0054] N2 adsorption-desorption analysis: Figure 3 (a) is the N2 adsorption-desorption isotherm. Figure 3 (b) shows the pore size distribution curve of BJH. The BET specific surface area of the WM@UiO-66 in-situ composite powder is 763.5 m². 2 / g, total pore volume is 0.49cm³ 3 / g; while the BET specific surface area of the physically mixed powder of white mud and UiO-66-NH2 with the same MOF content (Comparative Example 1) was only 512.8m². 2 / g, total pore volume is 0.31cm 3 / g. BJH pore size distribution showed that the mesopores of the in-situ composite powder were concentrated around 3.8 nm, with a narrow pore size distribution; the pore size distribution of the physically mixed powder was broadened and concentrated around 5.6 nm. These results indicate that white mud, as an in-situ growth carrier, effectively inhibited the aggregation of MOF nanoparticles, allowing more micro-mesoporous structures to be preserved.
[0055] Aerogel cross-sectional structure: The cross-sectional structure of the aerogel was observed, and the results are as follows. Figure 4 As shown: Traditional exogenous CaCl2 cross-linked aerogel ( Figure 4 (a) The surface forms a dense outer shell, while the interior is loosely cross-linked, exhibiting a heterogeneous structure of "tight on the outside and loose on the inside"; the composite aerogel of this invention ( Figure 4(b) The internal cross-linking is uniform, forming a through three-dimensional macroporous / mesoporous network. The cross-linking density is uniformly distributed radially, which is conducive to the rapid diffusion of Cd(II) into the internal active sites.
[0056] Example 4: Cd(II) Adsorption Performance Test
[0057] Cd(II) stock solution was prepared using Cd(NO3)2·4H2O, and the residual concentration was determined using inductively coupled plasma optical emission spectrometry (ICP-OES). The standard adsorption conditions were: initial Cd(II) concentration 200 mg / L, dosage 0.2 g / L, pH 5.5, temperature 25℃, and shaking speed 180 r / min. Each experiment was repeated three times, and the average value was taken.
[0058] (1) Adsorption kinetics: The adsorption amount was measured by sampling at different times, and the results are as follows. Figure 5 As shown in (a), the WM@UiO-66 / SA aerogel of this invention reached adsorption equilibrium in 120 min, with an equilibrium adsorption capacity of 415.6 mg / g; the physical mixed aerogel of Comparative Example 1 reached 287.6 mg / g in 180 min; the analytical grade CaCO3 endogenous cross-linked aerogel of Comparative Example 2 reached 367.9 mg / g in 150 min; and the exogenous CaCl2 cross-linked aerogel of Comparative Example 3 required 240 min to reach 358.6 mg / g. Figure 5 (b) shows that all systems conform to the pseudo-second-order kinetic model, with a correlation coefficient R. 2 The value >0.99 indicates that chemisorption is the rate-determining step, with amino coordination and ion exchange both participating in Cd(II) adsorption.
[0059] (2) Adsorption isotherms: Cd(II) solutions with initial concentrations of 25–500 mg / L were prepared, and the equilibrium adsorption capacity was measured. The results are as follows: Figure 6 As shown in (a). The adsorption data of the aerogel of this invention conforms to the Langmuir model, fitting the maximum Langmuir adsorption capacity q. max It is 449.7 mg / g, K L It is 0.082 L / mg, R 2 =0.998; the maximum adsorption capacities of Langmuir for Comparative Examples 1, 2, and 3 were 312.6, 389.4, and 362.8 mg / g, respectively. Figure 6 (b)).
[0060] (3) Effect of pH: When the initial pH increased from 2.0 to 6.0, the adsorption capacity increased from 86.5 mg / g to 423.8 mg / g; the adsorption capacity remained high in the pH range of 4 to 7, and decreased slightly when the pH was further increased to 8.0. Figure 7When the acidity is too strong, amino protonation inhibits coordination; when the alkalinity is too strong, Cd(II) hydrolysis leads to a decrease in the effective ion concentration. Therefore, a pH of 4–7 is preferred.
[0061] (4) Effect of dosage: When the dosage increased from 0.05 g / L to 1.0 g / L, the Cd(II) removal rate increased from 12.4% to 91.7%, and the adsorption capacity decreased from 496.0 mg / g to 183.4 mg / g. Figure 8 Among the results, the adsorbent was more fully dispersed in the solution at a dosage of 0.05 g / L, resulting in a relatively excessive amount of Cd(II) that could be contacted per unit mass of adsorbent, and a higher utilization rate of active sites, thus leading to a higher measured adsorption capacity per unit volume. The aforementioned maximum adsorption capacity of Langmuir, 449.7 mg / g, was obtained by fitting data under a dosage of 0.2 g / L, and the experimental conditions differ between the two methods. Considering both removal rate and adsorption capacity, 0.2–0.5 g / L is the optimal dosage range.
[0062] Example 5: Mechanical Property Testing
[0063] A cylindrical aerogel specimen (20 mm in diameter and 15 mm in height) was subjected to compression testing using a universal testing machine at a compression rate of 2 mm / min. The results are as follows: Figure 9 As shown, the WM@UiO-66 / SA aerogel of this invention exhibits a compressive stress of 0.18 MPa at 50% strain, significantly higher than that of the analytically pure CaCO3 endogenously crosslinked aerogel in Comparative Example 2 (0.11 MPa) and the exogenously crosslinked CaCl2 aerogel in Comparative Example 3 (0.075 MPa). After 10 cycles of 50% strain compression, the sample height recovery rate is approximately 93%, and it does not break or shed powder under vigorous stirring, demonstrating good engineering stability.
[0064] Example 6: Cyclic Regeneration and Selective Adsorption Test
[0065] Cyclic regeneration: Adsorption was carried out for 3 hours at an initial Cd(II) concentration of 50 mg / L, a dosage of 0.4 g / L, pH 5.5, and a temperature of 25 °C until equilibrium was reached. Subsequently, the saturated aerogel was placed in 0.1 mol / L EDTA solution for desorption for 3 hours, completing one adsorption-desorption cycle. Results are as follows: Figure 10 As shown: the removal rate of Cd(II) in the first cycle was 98.6%, and the removal rate remained at 87.5% after 5 cycles. Figure 10 (a)); the first cycle desorption rate was 91.8%, and the fifth cycle desorption rate was 85.6% ( Figure 10 (b) demonstrates that the material has excellent regeneration stability.
[0066] Selectivity: In a system containing Cd(II), Pb(II), Cu(II), Zn(II), Ni(II), Ca(II), and Na(I) (initial concentration of each ion 50 mg / L, dosage 0.4 g / L, pH 5.5, temperature 25℃), the removal rate of each ion was determined, and the results are as follows: Figure 11 As shown, the Cd(II) removal rate reached 94.6%, significantly higher than other coexisting ions, indicating that the amino group and the white mud component endowed the material with good selective adsorption capacity for Cd(II).
[0067] Example 7: Adsorption Mechanism Analysis
[0068] The composite aerogel after Cd(II) adsorption was characterized by XPS, and the results are as follows: Figure 12 As shown. Figure 12 In (a), Cd 3d appears at binding energies of 405.4 eV and 412.2 eV. 5 / 2 and Cd 3d 3 / 2 Characteristic peaks confirm that Cd(II) was successfully immobilized on the material surface. Figure 12 In (b), the N 1s spectrum shows a free amino-NH2 peak at 399.5 eV, a Cd-N peak at 400.8 eV (formed by coordination with Cd(II)), and a protonated amino-NH3 peak at 402.0 eV. + This indicates that amino groups synergistically adsorb Cd(II) through coordination chelation and electrostatic interaction; at the same time, calcium carbonate in the white mud can form a pH buffer microenvironment at the local micro-interface, which is conducive to the deprotonation of amino groups and promotes the coordination of Cd(II), thereby achieving physicochemical dual synergistic adsorption.
[0069] Comparative Example 1: White mud + UiO-66-NH2 physical mixed aerogel
[0070] UiO-66-NH2 powder was synthesized using the same formulation as in Example 1 without the addition of white clay. The MOF content of the WM@UiO-66 composite powder in Example 1 was determined by thermogravimetric analysis. UiO-66-NH2 powder and purified white clay powder were ground and mixed with the same MOF content as in Example 2, and the remaining operations were the same to obtain a physically mixed aerogel. The BET specific surface area of this physically mixed powder was 512.8 m². 2 / g, the equilibrium adsorption capacity of the corresponding aerogel for Cd(II) was 287.6 mg / g, the equilibrium time was 180 min, and the maximum adsorption capacity of Langmuir was 312.6 mg / g, all significantly lower than the product in the example. This comparative example demonstrates that mud as an in-situ growth carrier is not a simple physical superposition, but that in-situ composite significantly improves MOF dispersibility and active site utilization.
[0071] Comparative Example 2: Analysis of pure CaCO3 endogenous cross-linked aerogel
[0072] Using the WM@UiO-66 composite powder used in Example 2 as a reference (0.5g), the actual contents of calcium carbonate and UiO-66-NH2 were determined by thermogravimetric analysis. Then, based on the amount of calcium carbonate contained in 0.5g of the composite powder, an equivalent amount of analytical grade CaCO3 powder was weighed, and simultaneously, based on the amount of UiO-66-NH2 contained in the composite powder, an equivalent amount of UiO-66-NH2 powder was weighed. The weighed analytical grade CaCO3 powder and UiO-66-NH2 powder were ground and mixed evenly, and the remaining operations were the same as in Example 2, to obtain an analytical grade CaCO3 endogenous cross-linked aerogel. Its Cd(II) equilibrium adsorption capacity was 367.9 mg / g, the equilibrium time was 150 min, and the 50% strain compressive stress was 0.11 MPa. This comparative example demonstrates that white mud is not a simple replacement of analytical grade CaCO3; the crystal morphology, particle size distribution, and various impurity components in the white mud collectively produce a unique slow-release behavior and enhancing effect.
[0073] Comparative Example 3: Traditional exogenous CaCl2 cross-linked aerogel
[0074] The WM@UiO-66 composite powder obtained in Example 1 was formulated into an SA dispersion according to the method in Example 2. After being injected into a mold, it was immersed in a 2wt% CaCl2 solution for exogenous crosslinking for 4 hours. The remaining operations were the same as in Example 2, resulting in an exogenously crosslinked aerogel. Its Cd(II) equilibrium adsorption capacity was 358.6 mg / g, the equilibrium time was extended to 240 min, and the 50% strain compressive stress was only 0.075 MPa. This comparative example demonstrates that the traditional "tight outside, loose inside" crosslinking structure severely restricts mass transfer, and the endogenous in-situ crosslinking of this invention is the key to improving the adsorption rate and mechanical strength.
[0075] The above embodiments are only used to illustrate the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention.
Claims
1. A method for preparing a mud-mediated UiO-66-NH2-sodium alginate composite aerogel, characterized in that, Includes the following steps: S1. The white mud produced in the papermaking alkali recovery process is washed, dried and ground to obtain white mud powder; S2. Dissolve the zirconium source and the amino-containing organic ligand in an organic solvent, add the white mud powder, and allow UiO-66-NH2 to grow in situ on the surface of the white mud powder through a solvothermal reaction. Then, after solid-liquid separation, washing and drying, white mud@UiO-66-NH2 composite powder is obtained. S3. The white mud@UiO-66-NH2 composite powder is dispersed in an aqueous solution of sodium alginate, and D-gluconic acid-δ-lactone is added. The mixture is then allowed to stand and solidify. The hydrolysis of D-gluconic acid-δ-lactone causes the system to slowly acidify, which promotes the slow release of calcium ions from the calcium carbonate contained in the white mud powder. The calcium ions coordinate and crosslink with the carboxyl groups of sodium alginate to form a composite hydrogel. The calcium ions required to form the composite hydrogel come from the white mud powder itself, and no calcium salt is added during the crosslinking process. S4. The composite hydrogel is pre-frozen and then freeze-dried to obtain the mud-mediated UiO-66-NH2-sodium alginate composite aerogel.
2. The preparation method according to claim 1, characterized in that, In step S1, the white mud is washed with water until the supernatant is neutral, dried at 60-100℃ for 12-36 hours, ground, and then passed through a 100-300 mesh sieve.
3. The preparation method according to claim 1, characterized in that, In step S2, the zirconium source is zirconium tetrachloride, the amino-containing organic ligand is 2-aminoterephthalic acid, and the organic solvent is N,N-dimethylformamide; the mass ratio of the zirconium source to the amino-containing organic ligand is 1:0.6-1.6; 0.5-3.0 g of the white mud powder is added to every 100 mL of the organic solvent; the temperature of the solvothermal reaction is 100-150 °C and the time is 12-36 h; after the reaction is completed, the mixture is washed successively with N,N-dimethylformamide and anhydrous ethanol, and then vacuum dried at 50-80 °C for 8-24 h.
4. The preparation method according to claim 1, characterized in that, In step S3, the mass concentration of the sodium alginate aqueous solution is 1-4 wt%; the mass ratio of the white mud@UiO-66-NH2 composite powder to the sodium alginate is 1:0.5-4; the amount of D-gluconic acid-δ-lactone added is 0.2%-1.0% of the mass of the sodium alginate aqueous solution; and the static curing temperature is 15-40℃ and the time is 6-36h.
5. The preparation method according to claim 1, characterized in that, In step S4, the pre-freezing temperature is -80 to -20°C and the time is 8 to 24 hours; the freeze-drying vacuum degree is no greater than 20 Pa and the time is 24 to 72 hours.
6. A clay-mediated UiO-66-NH2-sodium alginate composite aerogel, characterized in that, The composite aerogel is prepared by the preparation method according to any one of claims 1 to 5; the composite aerogel includes a sodium alginate three-dimensional network framework and white mud@UiO-66-NH2 composite powder dispersed and anchored in the sodium alginate three-dimensional network framework, wherein UiO-66-NH2 is in situ grown on the surface of white mud particles in the composite powder; the white mud powder also serves as an in situ growth carrier of UiO-66-NH2 and an endogenous calcium source, the sodium alginate three-dimensional network framework is formed by cross-linking of calcium ions released by the white mud powder itself, and the cross-linking density is uniformly distributed along the radial direction of the composite aerogel.
7. The composite aerogel according to claim 6, characterized in that, The composite aerogel is a self-supporting monolithic block with a compressive stress of 0.15–0.22 MPa at 50% compressive strain and a maximum Langmuir adsorption capacity of not less than 400 mg / g for Cd(II).
8. The composite aerogel prepared by the preparation method according to any one of claims 1 to 5, or the composite aerogel according to claim 6 or 7, is used for the adsorption and removal of Cd(II) from cadmium-containing wastewater.
9. The application according to claim 8, characterized in that, The cadmium-containing wastewater has a pH of 4–7, an initial Cd(II) concentration of 25–500 mg / L, a dosage of the composite aerogel of 0.05–1.0 g / L, and an adsorption temperature of 15–40 °C.
10. The application according to claim 9, characterized in that, After adsorption saturation, the composite aerogel is desorbed and regenerated using a 0.05–0.2 mol / L EDTA solution for 1–5 h. The composite aerogel is reused at least 5 times, and the Cd(II) removal rate in the 5th cycle is not less than 85%.
Citation Information
Patent Citations
Ultra-low density sodium alginate-attapulgite composite aerogel and its preparation method