A perovskite catalyst containing cation-anion vacancy pairs, its preparation method and application
By constructing perovskite catalysts with cation-anion vacancy pairs, the problems of low specific surface area and slow oxygen species migration in the catalytic oxidation of VOCs by perovskite materials were solved, thereby improving catalytic activity and stability and reducing costs.
Patent Information
- Application Number
- CN202510591296.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-10
AI Technical Summary
Perovskite materials suffer from problems such as low specific surface area, surface inert segregation, and slow oxygen species migration during the catalytic oxidation of VOCs, which limits their application in heterogeneous catalysis. Furthermore, oxygen vacancies are easily deactivated under high temperature conditions.
Perovskite catalysts containing cation vacancies were synthesized using a non-stoichiometric method, and anionic vacancies were formed around the cation vacancies using surface engineering to construct cation-anion vacancy pairs, thereby enhancing oxygen migration capacity and catalytic activity.
This improved the oxygen cycling performance and stability of the catalyst, reduced the synthesis cost, and achieved a highly efficient catalytic effect in the catalytic oxidation of VOCs.
Smart Images

Figure CN123059638A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalysts and air pollution control, specifically relating to a perovskite catalyst containing cation-anion vacancy pairs, its preparation method, and its application in the catalytic oxidation of VOCs. Background Technology
[0002] Commonly used technologies for gas purification include filtration, adsorption, catalytic oxidation, and plasma. Among these, catalytic oxidation technology has received widespread attention due to its advantages such as high efficiency, energy saving, and no secondary pollution. VOCs catalytic oxidation technology utilizes catalysts to oxidize VOCs into CO2; therefore, the main task is to develop high-efficiency catalysts with low-temperature activity.
[0003] Perovskite materials have become promising catalysts due to their low cost, excellent thermal stability, and tunable structure. However, their inherent defects, such as low specific surface area, surface inert segregation, and slow oxygen species migration, limit their widespread application in heterogeneous catalysis. To address these issues, researchers have focused on improving catalytic performance through precise design of surface active sites, with oxygen vacancy modulation technology receiving particular attention. Electrons near oxygen vacancies delocalize from the O 2p orbitals before lattice oxygen is extracted. This optimization of the electronic structure accelerates the transfer of electrons to the antibonding orbitals of chemisorbed oxygen molecules, promoting oxygen molecule activation and improving lattice oxygen supply efficiency. However, the steady-state concentration of oxygen vacancies is controlled by both the formation and annihilation rates. Under high-temperature conditions, oxygen vacancies are easily refilled by active oxygen species to form stable lattice oxygen; therefore, suppressing oxygen vacancy deactivation has become a research focus. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a perovskite catalyst containing cation-anion vacancy pairs for the catalytic oxidation of VOCs, its preparation method, and its applications. This catalyst first utilizes a non-stoichiometric synthesis method to synthesize a perovskite catalyst with cation vacancies, saving on rare earth metal inputs and reducing synthesis costs. Then, surface engineering is used to etch the surface, dissolving the active lattice oxygen surrounding the cation vacancies, thereby forming cation-anion vacancy pairs. Compared to single oxygen vacancies, constructing cation-anion vacancy pairs is beneficial for both activating surrounding lattice oxygen and regenerating oxygen vacancies, thus improving oxygen cycle performance, enhancing oxygen migration capacity, and improving catalytic activity and stability. This catalyst exhibits good catalytic performance in the catalytic oxidation of VOCs.
[0005] Based on this, the technical solution of the present invention is as follows:
[0006] A perovskite catalyst, the catalyst having the chemical formula A y BO xFurthermore, the catalyst surface contains anionic vacancies and cation vacancies, i.e., anionic-cation vacancy pairs;
[0007] Where A is a rare earth element; B is Mn; x is a number greater than 0 and less than or equal to 4; and y is a number between 0.7 and 1.0.
[0008] In this invention, anion vacancies are formed around cation vacancies, thereby forming anion-cation vacancy pairs.
[0009] According to an embodiment of the present invention, the anion vacancy is asymmetric.
[0010] According to an embodiment of the present invention, the cation vacancy is an A ion vacancy and the anion vacancy is an oxygen vacancy.
[0011] According to an embodiment of the present invention, A is selected from at least one of lanthanum, praseodymium, and samarium.
[0012] According to an embodiment of the present invention, x is 1, 2, 3, 3.15 or 4.
[0013] According to an embodiment of the present invention, y is 0.7, 0.8, 0.9 or 1.0.
[0014] The present invention also provides a method for preparing the above-mentioned perovskite catalyst, comprising:
[0015] (1) Mix soluble rare earth salts, soluble manganese salts, citric acid, urea and water to obtain a mixed solution;
[0016] (2) Remove the water from the mixture to obtain the perovskite precursor;
[0017] (3) The precursor is calcined to obtain a lanthanum manganese perovskite material containing cation vacancies;
[0018] (4) The lanthanum manganese perovskite material containing cation vacancies is surface-treated in an acidic solution to obtain the perovskite catalyst.
[0019] According to an embodiment of the present invention, in step (1), the soluble rare earth salt may be selected from, but is not limited to, rare earth nitrates or rare earth halides; specifically, it may be selected from, but is not limited to, lanthanum nitrate, lanthanum chloride, praseodymium nitrate, praseodymium chloride, samarium nitrate or samarium chloride.
[0020] According to an embodiment of the present invention, in step (1), the soluble manganese salt may be selected from, but is not limited to, manganese nitrates or halides; specifically, it may be selected from, but is not limited to, manganese nitrate or manganese chloride.
[0021] According to an embodiment of the present invention, in step (1), the soluble rare earth salt and the soluble manganese salt are fed in a non-stoichiometric ratio; specifically, the molar ratio of the soluble rare earth salt and the soluble manganese salt is 0.7 to 1.0:1.0, for example, 0.7:1.0, 0.8:1.0, 0.9:1.0 or 1.0:1.0.
[0022] According to an embodiment of the present invention, in step (1), the molar ratio of the sum of the molar amounts of the soluble rare earth salt and the soluble manganese salt to that of citric acid is 1.0:(1.0 to 1.4).
[0023] According to an embodiment of the present invention, in step (1), the molar ratio of the soluble manganese salt to urea is 1.0:(2.5 to 3.5).
[0024] In step (1) of this invention, the water content is not particularly limited, as long as the raw materials are dissolved.
[0025] According to an embodiment of the present invention, in step (2), the water in the mixture is removed so that the mixture is a yellow viscous gel. Further, the yellow viscous gel is dried, for example, at a temperature of 100–140°C for 10–14 hours.
[0026] According to an embodiment of the present invention, in step (3), the atmosphere of the calcination treatment is air, the heating rate of the calcination treatment is 1 to 3 °C / min, the temperature of the calcination treatment is 700 to 800 °C, and the holding time of the calcination treatment is 2 to 6 hours.
[0027] According to an embodiment of the present invention, in step (4), the acidic solution is nitric acid or hydrochloric acid.
[0028] According to an embodiment of the present invention, in step (4), the concentration of the acidic solution is 0.5 to 1.5 mol / L.
[0029] According to an embodiment of the present invention, in step (4), the surface treatment time is 20 to 40 minutes.
[0030] According to an embodiment of the present invention, in step (4), after surface treatment, the product can also be centrifuged, washed and dried, for example, washed with deionized water and anhydrous ethanol until the washing liquid is neutral; or dried at 60-100°C.
[0031] As an exemplary embodiment of the present invention, the method for preparing the perovskite catalyst specifically includes:
[0032] (1) Mix soluble lanthanum salt, soluble manganese salt, citric acid, urea and water to obtain a transparent mixture;
[0033] (2) The excess water in the obtained mixture is evaporated by a rotary evaporator until a yellow viscous gel is formed. After drying, the perovskite precursor is obtained.
[0034] (3) The perovskite precursor was calcined to obtain lanthanum manganese perovskite material containing cation vacancies.
[0035] (4) The lanthanum manganese perovskite material containing cation vacancies is surface-treated in an acidic solution, and then centrifuged, washed and dried to obtain the perovskite catalyst.
[0036] The present invention also provides a perovskite catalyst prepared by the above method.
[0037] The present invention also provides the application of the above-mentioned perovskite catalyst in the catalytic oxidation of VOCs.
[0038] Specifically, in the catalytic oxidation, the gas hourly space velocity (GHSV) is 80,000-160,000 mL / (g·h), the catalyst dosage is 50-150 mg, the VOCs concentration is 50-150 ppm, the carrier gas is air, the reaction temperature is 50-200 °C, and the pressure is atmospheric pressure.
[0039] The beneficial effects of this invention are:
[0040] (1) The present invention uses non-stoichiometric feeding to introduce abundant cation vacancies into the prepared perovskite precursor, thereby activating the surrounding lattice oxygen, and with the help of surface treatment with acidic solution, oxygen vacancies are generated around the cation vacancies and anion-cation vacancy pairs are formed.
[0041] (2) This invention utilizes the regulatory effect of cation vacancies to construct asymmetric oxygen vacancies, thereby avoiding catalyst deactivation caused by oxygen vacancy annihilation during the catalytic reaction.
[0042] (3) The perovskite catalyst containing anion and cation vacancy pairs prepared in this invention has a dual function of anion and cation vacancy pairs during the catalytic process. It activates the surrounding lattice oxygen and promotes the regeneration of oxygen vacancies, thereby enhancing the cycling ability of oxygen species and improving catalytic performance.
[0043] (4) The raw materials of this invention are low in cost, easy to obtain, and the preparation method is simple, making it easy to conduct experiments and promote industrially. Attached Figure Description
[0044] Figure 1 The X-ray powder diffraction (XRD) patterns of the samples obtained in Example 1 and Comparative Examples 1-2 are shown.
[0045] Figure 2 The image shown is an electron microscope image of the catalyst obtained in Comparative Example 1.
[0046] Figure 3 The image shows an electron microscope image of the catalyst obtained in Comparative Example 2.
[0047] Figure 4 The image shows an electron microscope image of the catalyst obtained in Example 1.
[0048] Figure 5 The graph shows the activity test results of the products in Example 1 and Comparative Examples 1-2. Detailed Implementation
[0049] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0050] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0051] Comparative Example 1
[0052] The present invention provides a method for preparing a stoichiometric lanthanum manganese perovskite (LMO) catalyst, specifically including the following steps:
[0053] Step 1: Disperse 4.330g (0.01mol) lanthanum nitrate hexahydrate, 3.580g (0.01mol) manganese nitrate solution (50wt%) and 4.611g (0.024mol) citric acid in 30mL of deionized water and stir magnetically until the solid is completely dissolved to obtain a transparent mixed stock solution.
[0054] Step 2: Transfer the obtained stock solution to a flask and use a rotary evaporator to evaporate excess water at a speed of 150 rad in an 80°C water bath until a yellow viscous gel is formed. Dry it at 120°C with forced air for 12 hours to obtain the perovskite precursor.
[0055] Step 3: The perovskite precursor is heated to 750°C in an air atmosphere at a heating rate of 2°C / min and held at that temperature for 4 hours, then allowed to cool naturally to obtain a stoichiometric lanthanum manganese perovskite precursor catalyst.
[0056] Comparative Example 2
[0057] Embodiments of the present invention provide a lanthanum manganese perovskite (L...) containing cation vacancies. 0.8 The method for preparing MO catalysts specifically includes the following steps:
[0058] Step 1: Disperse 3.464g (0.008mol) lanthanum nitrate hexahydrate, 3.580g (0.01mol) manganese nitrate solution (50wt%), 4.149g citric acid and 1.802g urea in 30mL of deionized water and stir magnetically until the solid is completely dissolved to obtain a transparent mixed stock solution.
[0059] Step 2: Transfer the obtained stock solution to a flask and use a rotary evaporator to evaporate excess water at a speed of 150 rad in an 80°C water bath until a yellow viscous gel is formed. Dry it at 120°C for 12 hours to obtain the perovskite precursor.
[0060] Step 3: The perovskite precursor is heated to 750°C in an air atmosphere at a heating rate of 2°C / min and held at that temperature for 4 hours, then allowed to cool naturally to obtain a lanthanum manganese perovskite catalyst containing cation vacancies.
[0061] Example 1
[0062] This invention provides lanthanum manganese perovskite (HL) rich in anion and cation vacancies. 0.8 The method for preparing MO catalysts specifically includes the following steps:
[0063] Step 1: Disperse 3.464g (0.008mol) lanthanum nitrate hexahydrate, 3.580g (0.01mol) manganese nitrate solution (50wt%), 4.149g citric acid and 1.802g urea in 30mL of deionized water and stir magnetically until the solid is completely dissolved to obtain a transparent mixed stock solution.
[0064] Step 2: Transfer the obtained stock solution to a flask and use a rotary evaporator to evaporate excess water at a speed of 150 rad in an 80°C water bath until a yellow viscous gel is formed. Dry it at 120°C for 12 hours to obtain the perovskite precursor.
[0065] Step 3: The perovskite precursor is heated to 750°C in an air atmosphere at a heating rate of 2°C / min and held for 4 hours, then cooled naturally to obtain lanthanum manganese perovskite material containing anion and cation vacancies.
[0066] Step 4: The lanthanum manganese perovskite material containing cation vacancies was surface-treated in 1 mol / L dilute nitric acid solution for 30 min, and the solid was separated by centrifugation. It was washed three times with deionized water and anhydrous ethanol until the washing solution was neutral. After drying at 80℃ for 12 h, a lanthanum manganese perovskite catalyst rich in anion and cation vacancy pairs was obtained.
[0067] Figure 1The X-ray powder diffraction (XRD) patterns of the samples obtained in Example 1 and Comparative Examples 1-2 are shown in the figures. As can be seen from the figures, all three catalysts exhibit LaMnO4. 3.15 Diffraction peaks of (JCPDS card NO.50-0298).
[0068] Figure 2 The images show electron microscopy (EM) images of the catalyst obtained in Comparative Example 1. Image a represents a high-angle annular dark-field scanning transmission electron microscope (HAADF-STEM), image b represents an integrated differential phase contrast scanning transmission electron microscope (iDPC-STEM) image, and image c represents an atomic intensity map. In image c, 1, 2, and 3 represent the atomic intensity information of regions 1, 2, and 3 in image b, respectively. As can be seen from the images, the stoichiometric perovskite catalyst contains no vacancies.
[0069] Figure 3 The images show electron microscopy (EM) images of the catalyst obtained in Comparative Example 2. Image a represents a high-angle annular dark-field scanning transmission electron microscope (HAADF-STEM), image b represents an integrated differential phase contrast scanning transmission electron microscope (iDPC-STEM) image, and image c represents an atomic intensity map. In image c, 1, 2, and 3 represent the atomic intensity information of regions 1, 2, and 3 in image b, respectively. The images show that the non-stoichiometric perovskite catalyst contains lanthanum vacancies.
[0070] Figure 4 The images show electron microscopy (EM) images of the catalyst obtained in Example 1. As can be seen from the figures, the perovskite catalyst contains lanthanum-oxygen vacancy pairs. Image a represents a high-angle annular dark-field scanning transmission electron microscope (HAADF-STEM) image, image b represents an integrated differential phase contrast scanning transmission electron microscope (iDPC-STEM) image, and image c represents an atomic intensity map. In image c, 1, 2, 3, and 4 represent the atomic intensity information of regions 1, 2, 3, and 4 in image b, respectively.
[0071] Catalyst activity test:
[0072] The reaction was carried out in a quartz tube reactor with an inner diameter of 4 mm and a length of 400 mm. The catalyst content was 50 mg, the temperature gradient was 5 °C, the temperature was 150 °C, and maintained for half an hour. The gas hourly space velocity (GHSV) was 120,000 mL / gh, the VOCs concentration was 100 ppm, and air was used as the balance gas.
[0073] Activity test results as follows Figure 5 As shown, the lanthanum manganese perovskite catalyst rich in cation-anion vacancy pairs exhibits good catalytic activity in the VOCs oxidation reaction, indicating that the catalyst in this invention has excellent catalytic performance for the elimination of VOCs pollutants.
[0074] The embodiments of the present invention have been described above by way of example. However, the scope of protection of the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made by those skilled in the art within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A perovskite catalyst, characterized in that, The chemical formula of the catalyst is A y BO x Furthermore, the catalyst surface contains anionic vacancies and cation vacancies, i.e., anionic-cation vacancy pairs; Where A is a rare earth element; B is Mn; x is a number greater than 0 and less than or equal to 4; and y is a number between 0.7 and 1.
0.
2. The catalyst according to claim 1, characterized in that, The cation vacancy pair is an A ion vacancy, and the anion vacancy is an oxygen vacancy.
3. The catalyst according to claim 1, characterized in that, A is selected from at least one of lanthanum, praseodymium, and samarium.
4. The method for preparing the catalyst according to any one of claims 1-3, characterized in that, It includes: (1) Mix soluble rare earth salts, soluble manganese salts, citric acid, urea and water to obtain a mixed solution; (2) Remove the water from the mixture to obtain the perovskite precursor; (3) The precursor is calcined to obtain a lanthanum manganese perovskite material containing cation vacancies; (4) The lanthanum manganese perovskite material containing cation vacancies is surface-treated in an acidic solution to obtain the perovskite catalyst.
5. The method according to claim 4, characterized in that, In step (1), the soluble rare earth salt is selected from rare earth nitrates or rare earth halides; for example, it is selected from at least one of lanthanum nitrate, lanthanum chloride, praseodymium nitrate, praseodymium chloride, samarium nitrate, or samarium chloride. The soluble manganese salt is selected from manganese nitrates or halides, for example, it is selected from at least one of manganese nitrate or manganese chloride.
6. The method according to claim 4, characterized in that, In step (1), the molar ratio of the soluble rare earth salt and the soluble manganese salt is 0.7 to 1.0:1.
0. Preferably, in step (1), the molar ratio of the sum of the molar amounts of the soluble rare earth salt and the soluble manganese salt to that of citric acid is 1.0:1.0 to 1.
4. Preferably, in step (1), the molar ratio of the soluble manganese salt to urea is 1.0:2.5 to 3.
5.
7. The method according to claim 4, characterized in that, In step (3), the atmosphere for the calcination treatment is air, the heating rate for the calcination treatment is 1-3℃ / min, the temperature for the calcination treatment is 700-800℃, and the holding time for the calcination treatment is 2-6 hours.
8. The method according to claim 4, characterized in that, In step (4), the acidic solution is nitric acid or hydrochloric acid. Preferably, in step (4), the concentration of the acidic solution is 0.5 to 1.5 mol / L.
9. The method according to claim 4, characterized in that, In step (4), the surface treatment time is 20 to 40 minutes.
10. The use of the catalyst according to any one of claims 1-3 in the catalytic oxidation of VOCs.