A bimetallic core-shell dehydrogenation catalyst, a preparation method and applications thereof
By preparing a bimetallic core-shell dehydrogenation catalyst, utilizing the core-shell structure of TiCeAlOx or TiLaAlOx support and TiCeOx or TiLaOx shell, the problems of high precious metal usage and easy catalyst deactivation were solved, achieving efficient and economical dehydrogenation.
Patent Information
- Application Number
- CN202510587799.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-10
Smart Images

Figure CN123059660A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organic liquid hydrogen storage technology, and relates to a bimetallic core-shell dehydrogenation catalyst, its preparation method and its application. Background Technology
[0002] Hydrogen energy is attracting widespread attention due to its clean, efficient, and sustainable characteristics. However, the unique physicochemical properties of hydrogen determine that hydrogen storage technology is a key technological challenge limiting the large-scale application of hydrogen energy. Finding safe, efficient, and high-capacity hydrogen storage technologies has become a research hotspot in the hydrogen energy field. Organic liquid hydrogen storage technology, with its advantages of high hydrogen storage density, liquid storage and transportation, and high safety, is considered a hydrogen energy storage and transportation technology with great application potential.
[0003] Organic liquid hydrogen storage technology involves the hydrogenation and dehydrogenation processes of hydrogen storage carriers. While the hydrogenation process is relatively mature, the dehydrogenation process, due to reaction kinetics, typically requires overcoming high activation energies, making it difficult to proceed at low temperatures. However, high temperatures easily trigger side reactions. Under high-temperature conditions, hydrogen storage carriers (such as methylcyclohexane and perhydrodibenzyltoluene) are prone to thermal cracking or polycondensation reactions on the catalyst surface during dehydrogenation. The alkanes produced by cracking significantly affect the purity of the hydrogen product from the dehydrogenation process, and the dehydrogenation-polymerization reaction on the catalyst surface easily forms carbon deposits, reducing catalyst lifetime and activity. The efficiency, selectivity, and reaction conditions of the dehydrogenation process directly affect the overall performance of the organic hydrogen storage system. Besides the stability of dehydrogenation catalysts, the high cost of dehydrogenation catalysts is also a major obstacle to the large-scale application of organic liquid hydrogen storage technology. Patent CN115709078B discloses a dehydrogenation catalyst for organic hydrogen storage technology that uses a palladium (Pd)-molybdenum (Mo) bimetallic active component to achieve efficient dehydrogenation at low temperatures, with the amount of precious metal Pd exceeding 0.5 wt%. CN115869969B discloses an organic liquid hydrogen storage dehydrogenation catalyst using alumina as a support, which promotes the dispersion of the active component through strong interaction between the catalyst support, improving the selectivity of the hydrogen storage compound dehydrogenation process and enhancing the catalyst's stability. However, its precious metal content is 0.1-1.8 wt%, still presenting the problem of high precious metal content and high catalyst cost. Efficient and economical dehydrogenation technology can enable organic hydrogen storage carriers to release hydrogen rapidly and selectively under suitable conditions, while more economically meeting future energy supply needs. The construction of efficient and low-cost dehydrogenation catalyst systems is the core to achieving this goal. Summary of the Invention
[0004] This invention provides a bimetallic core-shell dehydrogenation catalyst, its preparation method, and its application, which addresses the problems of high precious metal content, high hydrogen impurity content, and easy deactivation of dehydrogenation catalysts in existing organic liquid hydrogen storage technologies.
[0005] The first aspect of the present invention provides a bimetallic core-shell dehydrogenation catalyst, the bimetallic core-shell dehydrogenation catalyst comprising a support and an active component, the support being TiCeAlOx or TiLaAlOx, the active component comprising a core and a shell covering the core, the shell being a TiCeOx or TiLaOx oxide layer, the core comprising a transition metal and a noble metal, wherein x∈(1,2).
[0006] In some embodiments of the present invention, the mass ratio of the carrier to the active component is (0.01-0.1):1.
[0007] In some embodiments of the present invention, the molar ratio of Ti, Al and Ce elements in the TiCeAlOx support is (2-20):(20-100):1; the molar ratio of Ti, Al and La elements in the TiLaAlOx support is (2-20):(20-100):1.
[0008] In some embodiments of the present invention, the mass ratio of the shell to the core is (2-20):1.
[0009] In some embodiments of the present invention, the molar ratio of the noble metal to the transition metal is (0.05-0.25):1.
[0010] In some embodiments of the present invention, the noble metal is selected from one or more of Pt, Ru, Pd, Ir, and Rh.
[0011] In some embodiments of the present invention, the transition metal is selected from one or more of Ni, Sn, Zn, Cu, Mn, and Co.
[0012] A second aspect of this invention provides a method for preparing a bimetallic core-shell dehydrogenation catalyst, comprising the following steps:
[0013] 1) Dissolve Ti precursor, Al precursor and Ce precursor or Ti precursor, Al precursor and La precursor in deionized water to obtain a mixed solution;
[0014] 2) Dissolve the precipitant in deionized water to obtain a precipitant solution;
[0015] 3) Add the mixed solution obtained in step 1) and the precipitant solution obtained in step 2) to an ethanol solution containing a cationic surfactant to carry out a coprecipitation reaction. After the reaction is completed, age, wash, dry and calcine to obtain TiCeAlOx or TiLaAlOx; where x∈(1,2);
[0016] 4) Mix the noble metal precursor, transition metal precursor, TiCeAlOx or TiLaAlOx obtained in step 3), deionized water, and urea. After stirring and impregnation, perform hydrothermal aging, drying, calcination, and reduction at higher temperatures to obtain the bimetallic core-shell dehydrogenation catalyst.
[0017] In some embodiments of the present invention, in step 1), the Ti precursor, Al precursor, Ce precursor, and La precursor are respectively nitrates or chlorides of Ti, Al, Ce, and La.
[0018] In some embodiments of the present invention, in step 1), the concentration of the Ti precursor solution is 0.01-0.05 mol / L; the concentration of the Al precursor solution is 0.1-0.5 mol / L; the concentration of the Ce precursor solution is 0.005-0.01 mol / L; and the concentration of the La metal precursor solution is 0.005-0.01 mol / L.
[0019] In some embodiments of the present invention, in step 1), the molar ratio of Ti, Al and Ce elements in the mixed solution is (2-20):(20-100):1; the molar ratio of Ti, Al and La elements is (2-20):(20-100):1.
[0020] In some embodiments of the present invention, in step 2), the precipitant is selected from one or more of sodium hydroxide, ammonia, ammonium carbonate, and sodium carbonate.
[0021] In some embodiments of the present invention, in step 2), the molar concentration of the precipitant in the precipitant solution is 0.1-0.5 mol / L.
[0022] In some embodiments of the present invention, in step 3), the flow rate ratio of the mixed solution to the precipitant solution is (1.25-2):1.
[0023] In some embodiments of the present invention, in step 3), the cationic surfactant is octadecyltrimethylammonium chloride and / or octadecyltrimethylammonium bromide.
[0024] In some embodiments of the present invention, in step 3), the concentration of ethanol in the ethanol solution is 0.001-0.01 mol / L.
[0025] In some embodiments of the present invention, in step 3), the mass-to-volume ratio of the cationic surfactant to the ethanol solution is (0.07-0.08 g / mL): 1.
[0026] In some embodiments of the present invention, in step 3), the pH of the system during the coprecipitation reaction is 7.3-10.2.
[0027] In some embodiments of the present invention, in step 3), the temperature of the coprecipitation reaction is 60-81°C; and the time of the coprecipitation reaction is 1-4 hours.
[0028] In some embodiments of the present invention, in step 3), the aging time is 18-36 hours.
[0029] In some embodiments of the present invention, in step 3), the drying temperature is 60-81°C and the drying time is 4-16 hours.
[0030] In some embodiments of the present invention, in step 3), the calcination temperature is 400-700°C and the calcination time is 3-10 hours.
[0031] In some embodiments of the present invention, in step 4), the noble metal precursor is selected from one or more of the nitrates or chlorides of Ru, Pt, Pd, Ir, and Rh.
[0032] In some embodiments of the present invention, in step 4), the concentration of the noble metal in the noble metal precursor is 0.0001-0.001 mol / L.
[0033] In some embodiments of the present invention, in step 4), the transition metal precursor is selected from one or more nitrates or chlorides of Ni, Co, Fe, Mn, Cu, and Zn.
[0034] In some embodiments of the present invention, in step 4), the concentration of the transition metal in the transition metal precursor is 0.002-0.05 mol / L.
[0035] In some embodiments of the present invention, in step 4), the temperature of the system during the stirring and impregnation process is 15-60°C; and the pH is 6.5-9.0.
[0036] In some embodiments of the present invention, in step 4), the molar ratio of the noble metal ions in the noble metal precursor, the transition metal particles in the transition metal precursor, the titanium ions in the TiCeAlOx or TiLaAlOx and urea is (0.0001-0.001):(0.002-0.05):1:0.1.
[0037] In some embodiments of the present invention, in step 4), the temperature of the hydrothermal aging is 120-200°C; and the time of the hydrothermal aging is 100-220 hours.
[0038] In some embodiments of the present invention, in step 4), a hydrogen-argon mixture is introduced during the heating and reduction process, wherein the volume of hydrogen in the hydrogen-argon mixture accounts for 5-50% of the total gas volume.
[0039] In some embodiments of the present invention, in step 4), the heating reduction temperature is 250-500°C, and the heating reduction time is 2-10h.
[0040] The third aspect of the present invention provides the application of the bimetallic core-shell dehydrogenation catalyst as described above and the bimetallic core-shell dehydrogenation catalyst obtained by the preparation method described above in the dehydrogenation reaction of organic hydrogen storage materials.
[0041] Compared with the prior art, the present invention has the following advantages:
[0042] (1) This invention utilizes the strong interaction between the metal and the oxide support to obtain a core-shell structure of a noble metal-transition metal alloy core coated with TiCeOx or TiLaOx oxide, which changes the nucleation and growth process of the noble metal-transition metal alloy, so that the alloy particles maintain a specific structure and form smaller particles, suppressing the situation where the sintering size of the alloy particles increases, improving the atomic utilization rate of the catalyst, and effectively reducing the cost of the catalyst.
[0043] (2) The unique interfacial charge transfer effect of the core-shell structure of the bimetallic core-shell dehydrogenation catalyst prepared by the present invention enhances the interaction between metals, promotes the activation of CH bonds and the desorption of H2, and effectively inhibits the breaking of CC bonds and the generation of carbon deposits in the dehydrogenation process, thus achieving higher dehydrogenation efficiency and catalyst stability.
[0044] (3) The bimetallic core-shell dehydrogenation catalyst prepared by the present invention introduces rare earth elements with abundant defect sites, which effectively prevents the agglomeration of active metal elements, reduces the particle size of active metal, improves the dispersibility of active metal elements, and improves the atomic utilization rate. It can reduce the amount of precious metals while ensuring catalytic activity, and effectively reduce the cost of catalyst.
[0045] (4) The synthesis process of the bimetallic core-shell dehydrogenation catalyst prepared by this invention is simple and easy to produce on a large scale. Attached Figure Description
[0046] Figure 1 The image shows the XRD characterization of the TiLaAlOx support in Example 1 of this invention.
[0047] Figure 2 The image shows the XRD characterization of the Pt-Ni bimetallic core-shell catalyst in Example 1 of this invention. Detailed Implementation
[0048] The following details the specific implementation of a bimetallic core-shell dehydrogenation catalyst, its preparation method, and its applications.
[0049] This invention utilizes the strong interaction between the metal and the oxide support to prepare a core-shell structure of a noble metal-transition metal alloy core coated with TiCeOx or TiLaOx oxides. This alters the nucleation and growth process of the noble metal-transition metal alloy, allowing the alloy particles to maintain a specific structure and form smaller particles. This suppresses the increase in particle size during sintering, improves the atom utilization rate of the catalyst, and effectively reduces the catalyst cost. Simultaneously, the interfacial charge transfer effect of the core-shell structure enhances the interaction between the metals, promoting the activation of CH bonds and the desorption of H2, while effectively suppressing the breaking of C-C bonds and the formation of carbon deposits during dehydrogenation, resulting in higher dehydrogenation efficiency and catalyst stability. Based on these findings, this invention was completed.
[0050] The first aspect of this invention provides a bimetallic core-shell dehydrogenation catalyst, comprising a support and an active component. The support is TiCeAlOx or TiLaAlOx, and the active component comprises a shell and a core encapsulated within the shell. The shell is a TiCeOx or TiLaOx oxide layer, and the core comprises a transition metal and a noble metal, where x ∈ (1, 2). Here, x is not a stoichiometric unit, but represents that the stoichiometric ratio of oxygen can vary, typically between 1 and 2. This variable stoichiometric ratio means that the material may have different structural forms; for example, titanium oxide-cerium (TiCeOx) or titanium oxide-lanthanum (TiLaOx) may form different oxygen vacancy concentrations, thereby affecting its catalytic activity, electronic structure, or material properties.
[0051] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the mass ratio of the support to the active component is (0.01-0.1):1, optionally (0.01-0.05):1 or (0.05-0.1):1. Controlling the mass ratio of the support to the active component within an appropriate range can significantly improve metal dispersion, reduce agglomeration, and thus enhance catalytic activity. Simultaneously, it helps to uniformly distribute active centers, optimize surface and interface effects, and increase the reaction rate. Furthermore, the oxygen defect structure of the TiCeOx or TiLaOx oxide layer endows the support with the ability to regulate the electronic environment, affecting the electronic structure of the metal and its catalytic properties, allowing for precise adjustment of the selectivity of the dehydrogenation reaction and achieving superior catalytic performance.
[0052] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the molar ratio of Ti, Al, and Ce elements in the TiCeAlOx support is (2-20):(20-100):1, which can be selected as (2-5):(20-100):1, (5-10):(20-100):1, (10-15):(20-100):1, (15-20):(20-100):1, (2-20):(20-50):1, (2-20) The molar ratio of Ti, Al and La elements in the TiLaAlOx support is (2-20):(20-100):1, which can be selected as (2-3):(20-50):1, (3-5):(20-50):1, (2-5):(20-30):1, 1, (2-5):(30-40):1 or (2-5):(40-50):1, etc.
[0053] In the bimetallic core-shell dehydrogenation catalyst provided by the present invention, the molar ratio of Ti to Ce in the TiCeOx oxide layer is (2-5):1, which can be (2-3):1, (3-4):1 or (4-5):1; the molar ratio of Ti to La in the TiLaOx oxide layer is (2-5):1, which can be (2-3):1, (3-4):1 or (4-5):1.
[0054] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the mass ratio of the shell to the core is (2-20):1, which can be selected as (2-8):1, (8-12):1, (12-16):1, (16-20):1, (5-10):1, or (10-20):1, etc. Controlling this mass ratio helps to optimize the metal distribution and electronic structure regulation. A higher shell ratio can enhance the stability of the oxide layer, improve the metal-support interface effect, and improve the anti-sintering ability of the active metal, thereby ensuring the long-term stability of the catalyst in the dehydrogenation reaction.
[0055] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the molar ratio of noble metal to transition metal is (0.05-0.25):1, which can be selected as (0.05-0.1):1, (0.1-0.15):1, (0.15-0.2):1, or (0.2-0.25):1, etc. In the bimetallic core-shell dehydrogenation catalyst system, controlling the molar ratio of noble metal to transition metal within the range of (0.05-0.25):1 can effectively regulate the electronic structure of the catalyst and the interaction between metals. Noble metal, as the main active center, can endow the catalyst with excellent dehydrogenation activity, while transition metal enhances the catalytic function of noble metal through electron transfer and redox regulation, while also improving the metal-support interface effect. Lower noble metal content can improve metal utilization and reduce catalyst cost, while appropriate transition metal can promote electron supply, optimize the distribution of active sites, and enhance the adsorption and activation capacity of reactants, thereby improving the selectivity and kinetic performance of the dehydrogenation reaction.
[0056] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the noble metal is selected from one or more of Pt, Ru, Pd, Ir, and Rh.
[0057] In the bimetallic core-shell dehydrogenation catalyst provided by this invention, the transition metal is selected from one or more of Ni, Sn, Zn, Cu, Mn, and Co.
[0058] A second aspect of this invention provides a method for preparing a bimetallic core-shell dehydrogenation catalyst, comprising the following steps:
[0059] 1) Dissolve Ti precursor, Al precursor and Ce precursor or Ti precursor, Al precursor and La precursor in deionized water to obtain a mixed solution.
[0060] 2) Dissolve the precipitant in deionized water to obtain a precipitant solution;
[0061] 3) Add the mixed solution obtained in step 1) and the precipitant solution obtained in step 2) to an ethanol solution containing a cationic surfactant to carry out a coprecipitation reaction. After the reaction is completed, age, wash, dry and calcine to obtain TiCeAlOx or TiLaAlOx; where x∈(1,2);
[0062] 4) Mix the noble metal precursor, transition metal precursor, TiCeAlOx or TiLaAlOx obtained in step 3), deionized water, and urea. After stirring and impregnation, perform hydrothermal aging, drying, calcination, and reduction at higher temperatures to obtain the bimetallic core-shell dehydrogenation catalyst.
[0063] In the preparation method of the bimetallic core-shell dehydrogenation catalyst provided by the present invention, step 1) is to dissolve Ti precursor, Al precursor and Ce precursor or Ti precursor, Al precursor and La precursor in deionized water to obtain a mixed solution.
[0064] In step 1) of this invention, the Ti precursor, Al precursor, Ce precursor, and La precursor are nitrates or chlorides of Ti, Al, Ce, and La, respectively.
[0065] In step 1) of this invention, the concentration of the Ti precursor solution is 0.01-0.05 mol / L, optionally 0.01-0.03 mol / L or 0.03-0.05 mol / L; the concentration of the Al precursor solution is 0.1-0.5 mol / L, optionally 0.1-0.3 mol / L or 0.3-0.5 mol / L; the concentration of the Ce precursor solution is 0.005-0.01 mol / L, optionally 0.005-0.008 mol / L or 0.008-0.01 mol / L; and the concentration of the La metal precursor solution is 0.005-0.01 mol / L, optionally 0.005-0.008 mol / L or 0.008-0.01 mol / L.
[0066] In step 1) of this invention, the molar ratio of Ti, Al, and Ce in the mixed solution is (2-20):(20-100):1, which can be (2-3):(20-50):1, (3-5):(20-50):1, (2-5):(20-30):1, (2-5):(30-40):1, or (2-5):(40-50):1, etc. The molar ratio of Ti, Al, and La is (2-20):(20-100):1, which can be (2-3):(20-50):1, (3-5):(20-50):1, (2-5):(20-30):1, (2-5):(30-40):1, or (2-5):(40-50):1, etc.
[0067] In the preparation method of the bimetallic core-shell dehydrogenation catalyst provided by the present invention, step 2) is to dissolve the precipitant in deionized water to obtain a precipitant solution.
[0068] In step 2) of this invention, the precipitant is selected from one or more of sodium hydroxide, ammonia, ammonium carbonate, and sodium carbonate.
[0069] In step 2) of this invention, the molar concentration of the precipitant in the precipitant solution is 0.1-0.5 mol / L, which can be selected as 0.1-0.3 mol / L or 0.3-0.5 mol / L.
[0070] In the preparation method of the bimetallic core-shell dehydrogenation catalyst provided by this invention, step 3) involves adding the mixed solution obtained in step 1) and the precipitant solution obtained in step 2) to an ethanol solution containing a cationic surfactant for co-precipitation. After the reaction is completed, the catalyst is aged, washed, dried, and calcined to obtain TiCeAlOx or TiLaAlOx. Specifically: the mixed solution obtained in step 1) and the precipitant solution obtained in step 2) are added dropwise to a four-necked flask containing a cationic surfactant and an ethanol solution at a certain flow rate ratio. The co-precipitation reaction is carried out under normal pressure, a certain temperature, and a certain pH. After co-precipitation, the catalyst is aged. After aging, the catalyst is filtered and washed with deionized water until neutral. Then, it is transferred to an oven for drying, calcined in a muffle furnace, and ground to obtain the catalyst support TiCeAlOx or TiLaAlOx.
[0071] In step 3) of this invention, the flow rate ratio of the mixed solution to the precipitant solution is (1.25-2):1, which can be (1.25-1.5):1 or (1.5-2):1. If the dripping rate of the mixed solution is lower than this range, the nucleation rate of the functional groups is too fast, which will eventually lead to an increase in the size of the catalyst particles and affect the dispersion of the active components; if it is higher than this range, the functional groups will not easily nucleate, affecting the stability of the synthesis process.
[0072] In step 3) of this invention, the cationic surfactant is octadecyltrimethylammonium chloride and / or octadecyltrimethylammonium bromide.
[0073] In step 3) of the present invention, the concentration of ethanol in the ethanol solution is 0.001-0.01 mol / L, which can be selected as 0.01-0.0015 mol / L or 0.0015-0.01 mol / L.
[0074] In step 3) of this invention, the mass-to-volume ratio of the cationic surfactant to the ethanol solution is (0.07-0.08 g / mL):1, which can be (0.07-0.073 g / mL):1, (0.073-0.075 g / mL):1, (0.075-0.078 g / mL):1, or (0.078-0.08 g / mL):1.
[0075] In step 3) of this invention, the pH of the system during the coprecipitation reaction is 7.3-10.2, which can be selected as 7.3-7.5, 7.5-8, 8-10, or 10-10.2.
[0076] In step 3) of this invention, the temperature of the coprecipitation reaction is 60-81℃, which can be 60-70℃ or 70-81℃; the time of the coprecipitation reaction is 1-4h, which can be 1-2h or 2-4h.
[0077] In step 3) of this invention, aging is carried out at 60-81℃, or optionally 60-70℃ or 70-81℃, and the aging time is 18-36h, or optionally 18-24h or 24-36h.
[0078] In step 3) of the present invention, the drying temperature is 60-81℃, which can be 60-70℃ or 70-81℃, and the drying time is 4-16h, which can be 4-10h or 10-16h.
[0079] In step 3) of this invention, the calcination temperature is 400-700℃, 400-500, 500-600 or 600-700℃, and the calcination time is 3-10h, which can be 3-5h, 5-7h, 7-8h or 8-10h.
[0080] In the preparation method of the bimetallic core-shell dehydrogenation catalyst provided by this invention, step 4) involves mixing a noble metal precursor, a transition metal precursor, TiCeAlOx or TiLaAlOx obtained in step 3), deionized water, and urea. After stirring and impregnation, the mixture undergoes hydrothermal aging, drying, calcination, and reduction at higher temperatures to obtain the bimetallic core-shell dehydrogenation catalyst. Specifically: the noble metal precursor, transition metal precursor, TiCeAlOx or TiLaAlOx catalyst support, deionized water, and urea are mixed in proportion and mixed evenly at room temperature. The mixture is then stirred and impregnated for a certain time at a certain temperature and pH. Afterward, the mixture is transferred to a hydrothermal reactor for hydrothermal aging. After aging, the mixture is filtered, dried, and then transferred to a muffle furnace for high-temperature calcination. After cooling, the sample is removed and placed in a tube furnace, where a hydrogen-argon mixture is introduced for programmed temperature reduction. After cooling and grinding, the bimetallic core-shell dehydrogenation catalyst is obtained.
[0081] In step 4) of this invention, the noble metal precursor is selected from one or more of the nitrates or chlorides of Ru, Pt, Pd, Ir, and Rh.
[0082] In step 4) of this invention, the concentration of the noble metal in the noble metal precursor is 0.0001-0.001 mol / L, which can be selected as 0.0001-0.00015 mol / L or 0.00015-0.001 mol / L.
[0083] In step 4) of this invention, the transition metal precursor is one or more of the nitrates or chlorides of Ni, Co, Fe, Mn, Cu, and Zn.
[0084] In step 4) of the present invention, the concentration of the transition metal in the transition metal precursor is 0.002-0.05 mol / L, which can be selected as 0.002-0.01 mol / L, 0.01-0.02 mol / L, 0.02-0.03 mol / L, 0.03-0.04 mol / L or 0.04-0.05 mol / L.
[0085] In step 4) of this invention, the stirring and soaking time is 18-30 hours, which can be 18-24 hours or 24-30 hours.
[0086] In step 4) of the present invention, the temperature of the system during the stirring and impregnation process is 15-60℃, which can be selected as 15-30℃, 30-45℃ or 45-60℃; the pH is 6.5-9.0, which can be selected as 6.5-7, 7-8 or 8-9.
[0087] In step 4) of this invention, the drying time is 24-48h, which can be 24-30h, 30-40h or 40-48h.
[0088] In step 4) of the present invention, the calcination temperature is 400-800℃, which can be selected as 400-500℃, 500-600℃, 600-700℃ or 700-800℃, and the calcination time is 4-16h, which can be selected as 4-8h, 8-12h or 12-16h.
[0089] In step 4) of this invention, the molar ratio of noble metal ions in the noble metal precursor, transition metal ions in the transition metal precursor, titanium ions in TiCeAlOx or TiLaAlOx, and urea is (0.0001-0.001):(0.002-0.05):1:0.1, and can be optionally (0.0001-0.00015):(0.002-0.05):1:0. 1. The urea feed ratios are (0.00015-0.001):(0.002-0.05):1:0.1, (0.0001-0.001):(0.002-0.01):1:0.1, (0.0001-0.001):(0.01-0.03):1:0.1, or (0.0001-0.001):(0.03-0.05):1:0.1, etc. If the urea feed ratio is too high, it is easy to cause the precious metal precursor and transition metal precursor to hydrolyze too quickly, which will increase the particle size of the precious metal and transition metal elements under hydrothermal conditions, thus affecting the dispersion of the precious metal and transition metal elements. Conversely, if the urea feed ratio is lower than this, it is easy to cause the precious metal precursor and transition metal precursor to not be completely hydrolyzed, ultimately affecting the loading rate of the precious metal and transition metal elements. Appropriate urea dosage is beneficial to improving the dispersion of precious metals and transition metals.
[0090] In step 4) of this invention, the hydrothermal aging temperature is 120-200℃, which can be selected as 120-140℃, 140-160℃, 160-180℃ or 180-200℃; the hydrothermal aging time is 100-220h, which can be selected as 100-120h, 120-150h, 150-180h, 180-200h or 200-220h.
[0091] In step 4) of this invention, a hydrogen-argon mixture is introduced during the heating and reduction process. The volume ratio of hydrogen in the hydrogen-argon mixture is 5-50% of the total gas volume, which can be selected as 5-20%, 20-35%, or 30-50%. The flow rate of the hydrogen-argon mixture is 90-110 mL / min, which can be selected as 90-100 mL / min or 100-110 mL / min.
[0092] In step 4) of this invention, the heating reduction temperature is 250-500℃, which can be selected as 250-300℃, 300-400℃ or 400-500℃, and the heating reduction time is 2-10h, which can be selected as 2-5h or 5-10h.
[0093] The third aspect of the present invention provides the application of the above-described bimetallic core-shell dehydrogenation catalyst and the bimetallic core-shell dehydrogenation catalyst prepared by the above-described method in the dehydrogenation reaction of organic hydrogen storage materials.
[0094] In this invention, the dehydrogenation reaction of organic hydrogen storage materials is a process in which hydrogen is released from hydrogen storage molecules by a catalyst under appropriate temperature and pressure. First, the hydrogen storage material (such as formic acid, liquid organic hydrogen storage compounds, etc.) comes into contact with the catalyst. The catalyst lowers the reaction energy barrier by activating CH bonds, allowing hydrogen atoms to detach from the organic molecules and form hydrogen gas (H2). During this reaction, the generated hydrogen can be directly used for fuel cell power supply or industrial applications, while the dehydrogenated organic molecules can be recycled, achieving efficient and safe hydrogen energy storage and release.
[0095] In this invention, the organic hydrogen storage material is selected from one or more of benzene, toluene, naphthalene, quinoline, carbazole, benzyltoluene, dibenzyltoluene, and N-ethylcarbazole, or a fully hydrogenated mixture thereof. The mass ratio of the organic hydrogen storage support material to the catalyst is (10-100):1, optionally (10-30):1, (30-50):1, (50-70):1, (70-90):1, or (90-100):1. The dehydrogenation reaction conditions are: reaction temperature 150-280℃, optionally 150-200℃, 200-270℃, or 270-280℃; reaction time 1-4h, optionally 1-2h, 2-3h, or 3-4h; and reaction pressure at atmospheric pressure.
[0096] The bimetallic core-shell dehydrogenation catalyst of this invention enhances the intermetallic interaction through the interfacial charge transfer effect on the surface of the unique core-shell structure, significantly promoting CH bond activation and improving hydrogen desorption efficiency, while effectively suppressing side reactions (such as carbon deposition and CC bond breaking). Furthermore, the introduction of rare earth elements (cerium (Ce) and lanthanum (La)) enhances the catalyst's dispersibility and stability, prevents the agglomeration of active metal elements, and ensures that the catalyst maintains high efficiency during long-term operation.
[0097] To make the technical means, creative features, objectives and effects of this invention easy to understand, the invention will be specifically described below in conjunction with embodiments and accompanying drawings.
[0098] In the following examples, unless otherwise stated, all reactants are commercially available products.
[0099] Unless otherwise specified, the purity of each product in each embodiment of the present invention exceeds 98%.
[0100] Example 1
[0101] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.2892 g of cerium nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of octadecyltrimethylammonium bromide (CTAB) and 250 mL of anhydrous ethanol. The pH of the flask was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C was continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the mixture was ground to obtain the catalyst support. The XRD characterization of the prepared catalyst support is shown in the appendix. Figure 1 From the appendix Figure 1 It can be seen that the overall crystallinity of the catalyst support is low, and there are amorphous TiOx and CeOx substances with oxygen vacancies on the surface of the support.
[0102] 0.0016 g of platinum tetrachloride, 0.0653 g of nickel nitrate hexahydrate, and 0.7325 g of urea were weighed and dissolved in 50 mL of deionized water. 1 g of carrier was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. After the sample was completely dry, it was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The tube furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst. The XRD characterization of the core-shell bimetallic dehydrogenation catalyst is shown in the appendix. Figure 2 From the appendix Figure 2 It can be seen that the catalyst surface after reduction by a mixture of hydrogen and argon gas does not have characteristic peaks of metals Pt and Ni, indicating that Pt and Ni elements have low particle size and good dispersion on the catalyst surface.
[0103] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270℃, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 97.12%, the selectivity of the dehydrogenation product was 99.15%, and the total hydrocarbon content of the tail gas was 48.2 ppm.
[0104] Example 2
[0105] 2.4816 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.2892 g of cerium nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0106] 0.0016 g of platinum tetrachloride, 0.0653 g of nickel nitrate hexahydrate, and 0.7325 g of urea were weighed and dissolved in 50 mL of deionized water. 1 g of carrier was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0107] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction was completed, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 95.59%, the selectivity of the dehydrogenation product was 97.78%, and the total hydrocarbon content of the tail gas was 65.1 ppm.
[0108] Example 3
[0109] 2.4816 g of titanium tetrachloride and 21.2996 g of aluminum nitrate nonahydrate were dissolved in 200 mL of deionized water with 0.2892 g of cerium nitrate hexahydrate to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the solution was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the solution was ground to obtain the catalyst support.
[0110] 0.0032 g of platinum tetrachloride, 0.0653 g of nickel nitrate hexahydrate, and 0.7325 g of urea were weighed and dissolved in 50 mL of deionized water. 1 g of support was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0111] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction was completed, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 95.19%, the selectivity of the dehydrogenation product was 99.75%, and the total hydrocarbon content of the tail gas was 40.7 ppm.
[0112] Example 4
[0113] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.5663 g of lanthanum nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0114] 0.0016 g of platinum tetrachloride, 0.0739 g of cobalt nitrate hexahydrate, and 0.7325 g of urea were weighed and dissolved in 50 mL of deionized water. 1 g of support was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0115] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction was completed, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 96.30%, the selectivity of the dehydrogenation product was 98.72%, and the total hydrocarbon content of the tail gas was 48.6 ppm.
[0116] Example 5
[0117] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.5663 g of lanthanum nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0118] 0.0028 g of neodymium nitrate, 0.0653 g of nickel nitrate hexahydrate, and 0.7325 g of urea were weighed and dissolved in 50 mL of deionized water. 1 g of support was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0119] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction was completed, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 95.45%, the selectivity of the dehydrogenation product was 99.05%, and the total hydrocarbon content of the tail gas was 43.3 ppm.
[0120] Example 6
[0121] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.5663 g of lanthanum nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0122] 0.0016 g of platinum tetrachloride, 0.0653 g of nickel nitrate hexahydrate, and 0.7325 g of urea hexahydrate were weighed and dissolved in 50 mL of deionized water. 1 g of support was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally crystallized at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0123] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. After the catalyst was reused 5 times, the dehydrogenation efficiency was 90.25%, the selectivity of the dehydrogenation product was 99.37%, and the total hydrocarbon content of the tail gas was 48.2 ppm.
[0124] Example 7
[0125] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 1.1326 g of lanthanum nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0126] Weigh 0.0025 g iridium chloride, 0.0536 g zinc nitrate hexahydrate, and 0.7325 g urea hexahydrate and dissolve them in 50 mL of deionized water. Add 1 g of carrier and stir at room temperature for 1 h. Transfer the sample to a hydrothermal reactor and age it at 180 °C for 120 h. After aging, filter and dry the filter cake at 80 °C. After the sample is completely dry, transfer it to a muffle furnace and calcine it at 550 °C for 6 h. After cooling, remove the sample and place it in a tube furnace. Purge with a hydrogen-argon mixture (10% hydrogen + 90% argon) at a flow rate of 100 mL / min. Heat the tube furnace to 300 °C at a rate of 5 °C / min and maintain the temperature for 5 h. After cooling, grind to obtain a core-shell bimetallic dehydrogenation catalyst.
[0127] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction was completed, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 94.33%, the selectivity of the dehydrogenation product was 95.65%, and the total hydrocarbon content of the tail gas was 50.3 ppm.
[0128] Comparative Example 1
[0129] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.2892 g of cerium nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of octadecyltrimethylammonium bromide and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C was continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. Finally, it was calcined in a muffle furnace at 600 °C for 5 h and ground to obtain the catalyst support.
[0130] 0.0653 g of nickel nitrate hexahydrate and 0.7325 g of urea were dissolved in 50 mL of deionized water. 1 g of support was added, and the mixture was stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After crystallization, the sample was filtered and the filter cake was dried at 80 °C. After complete drying, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The tube furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell monometallic dehydrogenation catalyst.
[0131] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270℃, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 29.55%, the selectivity of the dehydrogenation product was 87.03%, and the total hydrocarbon content of the tail gas was 354.5 ppm.
[0132] Comparative Example 2
[0133] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.2892 g of cerium nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. Finally, it was calcined in a muffle furnace at 600 °C for 5 h and ground to obtain the catalyst support.
[0134] 0.0016 g of platinum tetrachloride and 0.7325 g of urea were dissolved in 50 mL of deionized water. 1 g of carrier was added and stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The tube furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell bimetallic dehydrogenation catalyst.
[0135] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270℃, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 77.35%, the selectivity of the dehydrogenation product was 97.33%, and the total hydrocarbon content of the tail gas was 55.3 ppm.
[0136] As can be seen from the comparison of Example 1, Comparative Example 1, and Comparative Example 2, the bimetallic core-shell dehydrogenation catalyst (Example 1) has higher reactivity and dehydrogenation selectivity compared with the single metal core-shell catalyst (Comparative Example 1 and Comparative Example 2).
[0137] Comparative Example 3
[0138] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate and 0.2892 g of cerium nitrate hexahydrate were dissolved in 200 mL of deionized water to prepare a metal salt solution. 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 18.0322 g of CTAB and 250 mL of anhydrous ethanol. The pH of the flask was maintained at 7.5, and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. After calcination in a muffle furnace at 600 °C for 5 h, the catalyst support was obtained by grinding.
[0139] 0.0096 g of platinum tetrachloride and 0.7325 g of urea were dissolved in 50 mL of deionized water. 1 g of carrier was added and stirred at room temperature for 1 h. The sample was then transferred to a hydrothermal reactor and hydrothermally aged at 180 °C for 120 h. After aging, the sample was filtered and the filter cake was dried at 80 °C. Once completely dry, the sample was transferred to a muffle furnace and calcined at 550 °C for 6 h. After cooling, the sample was placed in a tube furnace, and a hydrogen-argon mixture (10% hydrogen + 90% argon) was introduced at a flow rate of 100 mL / min. The furnace was heated to 300 °C at a rate of 5 °C / min and held for 5 h. After cooling, the sample was ground to obtain a core-shell monometallic dehydrogenation catalyst.
[0140] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270 °C, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 97.35%, the selectivity of the dehydrogenation product was 99.11%, and the total hydrocarbon content of the tail gas was 44.0 ppm.
[0141] Comparative Example 4
[0142] 1.2408 g of titanium tetrachloride, 21.2996 g of aluminum nitrate nonahydrate, and 0.2892 g of cerium nitrate hexahydrate were weighed and dissolved in 200 mL of deionized water to prepare a metal salt solution. Then, 33.3624 g of sodium hydroxide was dissolved in 150 mL of deionized water to prepare a precipitate. The prepared metal salt solution and precipitate were added dropwise to a four-necked flask at a volumetric flow rate of 4:3. The flask was pre-filled with 250 mL of anhydrous ethanol, and the pH was maintained at 7.5 and the temperature at 70 °C. After vigorous stirring and co-precipitation, dynamic aging at 70 °C was continued for 24 h. After aging, the mixture was filtered and washed with deionized water until neutral. It was then transferred to an oven and dried at 80 °C for 12 h. Finally, it was calcined in a muffle furnace at 600 °C for 5 h and ground to obtain the catalyst support.
[0143] Weigh 0.0016 g platinum tetrachloride, 0.0653 g nickel nitrate hexahydrate, and 50 mL deionized water. Add 1 g of support and stir at room temperature for 1 h. Transfer the sample to an oven and dry at 80 °C for 24 h. After drying, transfer the sample to a muffle furnace and calcine at 550 °C for 6 h. After cooling, remove the sample and place it in a tube furnace. Purge with a hydrogen-argon mixture (10% hydrogen + 90% argon) at a flow rate of 100 mL / min. Heat the tube furnace to 300 °C at a rate of 5 °C / min and maintain for 5 h. After cooling, grind to obtain a simple impregnated supported bimetallic dehydrogenation catalyst.
[0144] The catalyst was applied to the dehydrogenation reaction of perhydrodibenzyltoluene. 0.5 g of catalyst and 5 g of perhydrodibenzyltoluene were weighed and placed in a reaction vessel. The reaction temperature was raised to 270℃, and the dehydrogenation reaction was carried out for 1 h. After the reaction, the composition of the residual liquid phase and the generated gas was qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The analytical results showed that the dehydrogenation efficiency was 97.12%, the selectivity of the dehydrogenation product was 87.95%, and the total hydrocarbon content of the tail gas was 73.25 ppm.
[0145] A comparison of Example 1 and Comparative Example 3 shows that the bimetallic core-shell dehydrogenation catalyst with low noble metal loading (Example 1) has similar catalytic effects to the monometallic core-shell catalyst with high noble metal loading (Comparative Example 3). A comparison of Example 1 and Comparative Example 4 shows that the bimetallic core-shell dehydrogenation catalyst (Example 1) with the same active component loading has a significantly better catalytic effect than the simply impregnated supported bimetallic dehydrogenation catalyst (Comparative Example 4). These two sets of experimental comparisons demonstrate that the existence of the bimetallic core-shell structure effectively improves the atom utilization rate of noble metals.
[0146] The above embodiments are preferred examples of the present invention and are not intended to limit the scope of protection of the present invention. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the scope of protection of the present invention.
[0147] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
Claims
1. A bimetallic core-shell dehydrogenation catalyst, characterized in that, The bimetallic core-shell dehydrogenation catalyst includes a support and an active component. The support is TiCeAlOx or TiLaAlOx, and the active component includes a core and a shell covering the core. The shell is a TiCeOx or TiLaOx oxide layer, and the core includes a transition metal and a noble metal, where x∈(1,2).
2. The bimetallic core-shell dehydrogenation catalyst according to claim 1, characterized in that, The mass ratio of the carrier to the active component is (0.01-0.1):
1.
3. The bimetallic core-shell dehydrogenation catalyst according to claim 1, characterized in that, The molar ratio of Ti, Al and Ce in the TiCeAlOx support is (2-20):(20-100):1; the molar ratio of Ti, Al and La in the TiLaAlOx support is (2-20):(20-100):
1.
4. The bimetallic core-shell dehydrogenation catalyst according to claim 1, characterized in that, The mass ratio of the shell to the core is (2-20):
1.
5. The bimetallic core-shell dehydrogenation catalyst according to claim 1, characterized in that, The molar ratio of the noble metal to the transition metal is (0.05-0.25):
1.
6. The bimetallic core-shell dehydrogenation catalyst according to claim 1, characterized in that, It also includes one or more of the following features: A1) The precious metal is selected from one or more of Pt, Ru, Pd, Ir, and Rh; A2) The transition metal is selected from one or more of Ni, Sn, Zn, Cu, Mn, and Co.
7. A method for preparing a bimetallic core-shell dehydrogenation catalyst, characterized in that, Includes the following steps: 1) Dissolve Ti precursor, Al precursor and Ce precursor or Ti precursor, Al precursor and La precursor in deionized water to obtain a mixed solution; 2) Dissolve the precipitant in deionized water to obtain a precipitant solution; 3) Add the mixed solution obtained in step 1) and the precipitant solution obtained in step 2) to an ethanol solution containing a cationic surfactant to carry out a coprecipitation reaction. After the reaction is completed, age, wash, dry and calcine to obtain TiCeAlOx or TiLaAlOx; where x∈(1,2); 4) Mix the noble metal precursor, transition metal precursor, TiCeAlOx or TiLaAlOx obtained in step 3), deionized water, and urea. After stirring and impregnation, perform hydrothermal aging, drying, calcination, and reduction at higher temperatures to obtain the bimetallic core-shell dehydrogenation catalyst.
8. The method for preparing the bimetallic core-shell dehydrogenation catalyst according to claim 7 further comprises any one or more of the following features: In step 1) of B1), the Ti precursor, Al precursor, Ce precursor, and La precursor are nitrates or chlorides of Ti, Al, Ce, and La, respectively. B2) In step 1), the concentration of the Ti precursor solution is 0.01-0.05 mol / L; the concentration of the Al precursor solution is 0.1-0.5 mol / L; the concentration of the Ce precursor solution is 0.005-0.01 mol / L; and the concentration of the La metal precursor solution is 0.005-0.01 mol / L. In step 1) of B3), the molar ratio of Ti, Al and Ce in the mixed solution is (2-20):(20-100):1; the molar ratio of Ti, Al and La is (2-20):(20-100):
1. In step 2) of B4), the precipitant is selected from one or more of sodium hydroxide, ammonia, ammonium carbonate, and sodium carbonate; In step 2) of B5), the molar concentration of the precipitant in the precipitant solution is 0.1-0.5 mol / L; In step 3) of B6), the flow rate ratio of the mixed solution to the precipitant solution is (1.25-2):1; In step 3) of B7), the cationic surfactant is octadecyltrimethylammonium chloride and / or octadecyltrimethylammonium bromide; In step 3) of B8, the concentration of ethanol in the ethanol solution is 0.001-0.01 mol / L; In step 3) of B9), the mass-to-volume ratio of the cationic surfactant to the ethanol solution is (0.07-0.08 g / mL): 1; In step 3) of B10, the pH of the system during the coprecipitation reaction is 7.3-10.2; In step 3) of B11), the temperature of the coprecipitation reaction is 60-81℃; the time of the coprecipitation reaction is 1-4h. In step 3) of B12), the aging time is 18-36 hours; In step 3) of B13), the drying temperature is 60-81℃ and the drying time is 4-16h; In step 3) of B14, the calcination temperature is 400-700℃ and the calcination time is 3-10h.
9. The method for preparing the bimetallic core-shell dehydrogenation catalyst according to claim 7 further comprises any one or more of the following features: In step 4) of C1), the noble metal precursor is selected from one or more of the nitrates or chlorides of Ru, Pt, Pd, Ir, and Rh; In step 4) of C2), the concentration of the noble metal in the noble metal precursor is 0.0001-0.001 mol / L; In step 4), the transition metal precursor is one or more of the nitrates or chlorides of Ni, Co, Fe, Mn, Cu, and Zn; In step 4) of C3), the concentration of the transition metal in the transition metal precursor is 0.002-0.05 mol / L; In step 4) of C4), the stirring and impregnation time is 18-30 hours; In step 4) of C5), the temperature of the system during the stirring and impregnation process is 15-60℃; the pH is 6.5-9.
0. In step 4) of C6), the drying time is 24-48 hours; In step 4) of C7), the calcination temperature is 400-800℃ and the calcination time is 4-16h; In step 4) of C8, the molar ratio of noble metal ions in the noble metal precursor, transition metal particles in the transition metal precursor, titanium ions in TiCeAlOx or TiLaAlOx, and urea is (0.0001-0.001):(0.002-0.05):1:0.1; In step 4) of C9), the temperature of the hydrothermal aging is 120-200℃; the time of the hydrothermal aging is 100-220h. In step 4) of C10, a hydrogen-argon mixture is introduced during the heating and reduction process, wherein the volume of hydrogen in the hydrogen-argon mixture accounts for 5-50% of the total gas volume; In step 4) of C11), the heating reduction temperature is 250-500℃, and the heating reduction time is 2-10h.
10. The application of the bimetallic core-shell dehydrogenation catalyst according to any one of claims 1-6 and / or the bimetallic core-shell dehydrogenation catalyst prepared by any one of claims 7-9 in the dehydrogenation reaction of organic hydrogen storage materials.
Citation Information
Patent Citations
A dehydrogenation catalyst, preparation method thereof and dehydrogenation method
CN115869969B